A preparation method and application of fast ion conductor based on in-situ curing
Through the copolymerization of highly sterically hindered monomers and cross-linking agents, a three-dimensional network structure is constructed, which solves the problems of ionic conductivity, mechanical strength and interface stability of in-situ solid polymer electrolytes, and improves the performance and life of lithium secondary batteries.
Patent Information
- Application Number
- CN202211159701.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-22
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-09-22
AI Technical Summary
It is difficult for in-situ solid polymer electrolytes to balance high ionic conductivity, mechanical strength and electrode-electrolyte interface stability, resulting in low cycle Coulombic efficiency and short cycle life of solid-state batteries.
Highly sterically hindered monomers and highly active cross-linking agents are copolymerized to broaden the ion migration channels through the sterically hindered volume effect, build a three-dimensional network structure, and improve mechanical strength and interface stability.
It significantly improves the ionic conductivity of the in-situ solid polymer electrolyte, enhances the energy density, Coulombic efficiency and cycle stability of lithium secondary batteries, and broadens the application fields of lithium secondary batteries.
Smart Images

Figure CN115513520B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solid electrolyte preparation, and in particular to a preparation method and application of a fast ion conductor based on in-situ solidification. Background Art
[0002] As primary energy sources are gradually facing depletion and the environmental crisis is becoming increasingly serious, it is particularly necessary to develop renewable clean energy such as solar energy, wind energy, and tidal energy. However, most of the above energy sources are intermittent energy sources, and new energy storage systems with high energy density and low loss are required for energy scheduling. Lithium secondary batteries are widely used due to their abundant lithium mineral resources and efficient energy storage and release capabilities, but the lithium-ion liquid batteries that have been successfully commercialized have serious safety problems such as leakage and explosion, and are also insufficient to meet the current product demand for energy storage systems. Therefore, the development of high energy density, high safety and high efficiency solid electrolyte batteries has become the future development direction of lithium secondary batteries.
[0003] Solid electrolyte batteries are divided into inorganic solid batteries and polymer solid batteries. Although inorganic solid electrolytes have high ionic conductivity and excellent lithium dendrite suppression ability, their large-scale commercial application is restricted by their brittleness, difficulty in large-scale production, poor interface compatibility and other issues. Polymer solid electrolytes are further divided into in-situ and ex-situ. Among them, in-situ solid polymer electrolytes (ISPE) have better application prospects than ex-situ solid polymer electrolytes (ESPE) due to their simple production process, environmentally friendly preparation process, ultra-low interface impedance, excellent interface compatibility and long cycle capacity.
[0004] Although the in-situ solid polymer electrolyte technology has been developed to a certain level, it is still difficult to balance high ionic conductivity, mechanical strength and electrode-electrolyte interface performance. Solid polymer electrolytes transport ions through the movement of polymer chain segments. Highly flexible solid polymer electrolytes have low glass transition temperatures and high ionic conductivity, but low mechanical strength and insufficient rigidity. At the same time, the electrode-electrolyte interface is unstable, resulting in low coulombic efficiency and short cycle life of solid-state batteries. Solid polymer electrolytes with a high degree of crystallinity have a high degree of polymer regularity, thus high mechanical strength and stable interface properties, but their polymer chain segments move weakly, and the ion migration channels are narrow, resulting in a very low ionic conductivity (10 -5 ~10 -7 S / cm), making it difficult to achieve commercial application. Therefore, achieving high ionic conductivity, high mechanical strength and stable interface properties is a major challenge for in-situ solid polymer electrolytes. Summary of the invention
[0005] The purpose of the present invention is to propose a preparation method and application of a fast ion conductor based on in-situ curing, in view of the problem that the current in-situ solid polymer electrolytes in the background art have difficulty in taking into account the ionic conductivity, mechanical strength and interface stability.
[0006] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0007] A method for preparing a fast ion conductor based on in-situ curing comprises the following steps:
[0008] Step 1. 15 to 30 parts (by mass) of a high steric hindrance monomer and 5 to 10 parts (by mass) of a cross-linking agent are mixed, and after removing water through a molecular sieve, 5 to 10 parts (by mass) of a lithium salt are added thereto, and the mixture is mixed evenly, and the obtained mixed solution A is stored at 2 to 8°C;
[0009] Step 2. 0.04-0.12 parts (by mass) of the initiator and 49.96-79.88 parts (by mass) of the plasticizer are mixed, and stirred for 30-120 minutes to mix evenly to obtain a mixed solution B;
[0010] Step 3. Mix the mixed solution A of step 1 and the mixed solution B of step 2, stir evenly, and obtain a curing precursor solution;
[0011] Step 4. Inject the solidification precursor solution prepared in step 3 into the battery cell with porous skeleton membrane, 2 Add 10 to 35 μL and in-situ cure at 30 to 80° C. for 0.5 to 48 hours to obtain a solid polymer fast ion conductor.
[0012] Furthermore, the high steric hindrance monomer is one or more of the following structural formulas:
[0013]
[0014] Among them, R 1 H or -CH 3 , R 2 It is a carbon chain with less than 4 carbon atoms, and X is F, Cl, Br or I.
[0015] Preferably, the high steric hindrance monomer is one or more of maleic anhydride, vinylene carbonate, dichlorovinyl carbonate, 4,5-dimethyl-1,3-dioxol-2-one, 4-chloromethyl-5-methyl-1,3-dioxol-2-one, 4-formyl-5-methyl-1,3-dioxol-2-one, olmesartan medoxomil impurity 83, 4-bromomethane-1,3-dioxolane-2-one, and 4-tert-butyl-5-methyl-1,3-dioxolane-2-one.
[0016] Furthermore, the crosslinking agent is an acrylic or methacrylic crosslinking agent, preferably one or more of 2-methyl-acrylic acid-2-ethylene oxide-ethyl ester, poly(ethylene glycol) diacrylate, poly(ethylene glycol) dimethacrylate, bisphenol A ethoxylate dimethacrylate, 2-methyl-acrylic acid-2-ethylene oxide-ethyl, trimethylolpropane triacrylate, pentaerythritol tetraacrylate, and phosphorus fluoride-based crosslinking agents.
[0017] Furthermore, the lithium salt is one or more of lithium hexafluorophosphate, lithium bis(trifluoromethylsulfonyl)imide, lithium perchlorate, lithium bis(fluorosulfonyl)imide, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium tetrafluoroborate, and lithium polyborate.
[0018] Further, the initiator is azobisisobutyronitrile, azobisisovaleronitrile, azobisisoheptanenitrile, benzoyl peroxide, Al(OTf) 3 , lithium iodide, lithium hexafluorophosphate, or more.
[0019] Furthermore, the plasticizer is a 0.8-2 mol / L lithium salt solution, the solute of the lithium salt solution is one or more of lithium hexafluorophosphate, lithium bis(trifluoromethylsulfonyl)imide, lithium perchlorate, lithium bis(fluorosulfonyl)imide, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium tetrafluoroborate, and lithium polyborate, and the solvent is one or more of ethylene carbonate (EC), propylene carbonate (PC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), and 1,3-dioxolane (DOL).
[0020] Furthermore, the battery cell with a porous skeleton membrane in step 4 is obtained by stacking a positive electrode sheet, a porous skeleton membrane and a negative electrode sheet in sequence, and then encapsulating them with an aluminum-plastic film. The active material of the positive electrode sheet is one of lithium iron phosphate, lithium nickel oxide, lithium cobalt oxide, lithium iron manganese phosphate, lithium manganese oxide, lithium nickel manganese oxide, nickel cobalt manganese ternary positive electrode, and sulfur positive electrode; the active material of the negative electrode sheet is one of a metal lithium sheet, a metal lithium alloy, graphite, hard carbon, molybdenum disulfide, lithium titanate, graphene, and a silicon-carbon negative electrode; and the porous skeleton membrane is one of a polyethylene film, a polypropylene film, a wood cellulose film, a glass fiber film, a polyimide electrospun membrane, a polyvinylidene fluoride electrospun membrane, and a polyacrylonitrile electrospun membrane.
[0021] The present invention provides a method for preparing a fast ion conductor based on in-situ curing. The structural characteristics and lithium ion transport mechanism of the obtained solid polymer fast ion conductor are as follows:
[0022]
[0023] Lithium ions in COO - and X - Hopping transfer on the group site, continuous COO- and X - The group sites make the lithium ion path coherent.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] The present invention provides a method for preparing a fast ion conductor based on in-situ curing. The method comprises the following steps: copolymerizing a high steric hindrance monomer with a high-activity cross-linking agent, and utilizing the steric hindrance volume effect to broaden the ion migration channel, thereby shortening the ion transport path of the in-situ solid polymer electrolyte and greatly improving the ion conductivity. At the same time, the three-dimensional network structure synergistically constructed by the high steric hindrance monomer and the high-activity cross-linking agent has high mechanical strength and stable electrode electrolyte interface properties, effectively solving the problem that the current in-situ solid polymer electrolyte is difficult to balance ionic conductivity, mechanical strength and interface stability. The prepared fast ion conductor is applied to lithium secondary batteries, which can effectively improve the energy density, coulomb efficiency and cycle stability of lithium secondary batteries, and broaden the application field of lithium secondary batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The AC impedance curves of the solid polymer fast ion conductors obtained in Example 1 and Comparative Example 1;
[0027] Figure 2 The linear sweep voltammetric curves of the solid polymer fast ion conductors obtained in Example 2 and Comparative Example 2;
[0028] Figure 3 The rate performance test results of the lithium secondary battery assembled with the solid polymer fast ion conductor obtained in Example 2;
[0029] Figure 4 The test results of the cycle performance of the lithium secondary battery assembled with the solid polymer fast ion conductor obtained in Example 2 are shown. DETAILED DESCRIPTION
[0030] The present invention is further described below in conjunction with some comparative examples and embodiments. It is worth noting that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0031] A method for preparing a lithium secondary battery based on an in-situ solidified fast ion conductor comprises the following steps:
[0032] Step 1: Preparation of positive electrode:
[0033] 1.1 Dissolve 5 wt.% of polyvinylidene fluoride (PVDF) relative to the mass of the positive electrode material in 32 wt.% of nitrogen methyl pyrrolidone (NMP) relative to the mass of the total slurry, stir for 1 h to obtain a PVDF solution, and the stirring rate is 2000 r / min;
[0034] 1.2 Add 5wt.% of conductive carbon black to the PVDF solution obtained in step 1.1, and continue stirring at a speed of 2000r / min for 1h; then, add 90wt.% of positive electrode active material to the obtained mixed solution, and continue stirring at a speed of 2000r / min for 2h to obtain a slurry;
[0035] 1.3 The slurry obtained in step 1.2 is vacuumed, defoamed, filtered, coated on aluminum foil, dried at 120°C, rolled, and then stored in a vacuum oven at 80°C. When used, it is cut into pieces to obtain a positive electrode;
[0036] Step 2: Preparation of negative electrode:
[0037] 2.1 Mix the negative electrode active material, binder, conductive carbon black and deionized water in a mass ratio of 1:1:1:1, vacuum the obtained slurry to remove bubbles, filter it, apply it on copper foil, dry it at 120°C, roll it, and then store it in a vacuum oven at 80°C. When using it, cut it into pieces to obtain a negative electrode; wherein the binder is one of sodium carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR), polyacrylic acid (PAA), and LA132 / LA133, and the capacity of the negative electrode material is 1.01 to 1.05 times that of the positive electrode material;
[0038] Step 3, preparing a solidification precursor solution of a solid polymer fast ion conductor;
[0039] Step 4: stack the negative electrode, porous skeleton membrane, and positive electrode in the order of stacking and encapsulating with aluminum-plastic film to obtain a cell with a porous skeleton membrane; inject the solidification precursor solution prepared in step 3 into the cell with a porous skeleton membrane, and add 10% solidification liquid per 1 cm 2 10 to 35 μL is added, in-situ cured at 30 to 80° C. for 0.5 to 48 hours, and allowed to stand at room temperature for 12 hours to obtain a lithium secondary battery.
[0040] The obtained lithium secondary battery was tested using a LAND battery charge and discharge tester.
[0041] The preparation and application of the solid polymer fast ion conductor solidification precursor solution in step 3 are as follows:
[0042] Example 1
[0043] In a dry glove box filled with argon (O 2 <0.1ppm, H 2O<0.1ppm), 20 parts by weight of a high steric hindrance monomer maleic anhydride and 5 parts by weight of a high activity crosslinking agent polyethylene glycol dimethacrylate (PEGDMA) are stirred and mixed, and after removing water through a molecular sieve, 5 parts by weight of lithium bis(fluorosulfonyl)imide are added and stirred for 30 minutes to completely dissolve the lithium salt, and the obtained mixed solution A is stored at 2 to 8°C; 0.04 parts by weight of azobisisobutyronitrile AIBN initiator and 69.96 parts by weight of a plasticizer (1 mol / L lithium salt solution, the solute is lithium bis(fluorosulfonyl)imide, and the solvent is a mixed solvent of 1,3-dioxolane (DOL) and dimethyl carbonate (DMC) in a volume ratio of 1:1) are mixed, stirred for 40 minutes to mix evenly, and a mixed solution B is obtained; the mixed solution A and the mixed solution B are mixed and stirred evenly to obtain a curing precursor solution.
[0044] The dried lithium cobalt oxide positive electrode and graphite negative electrode were cut and stacked in the order of negative electrode, porous skeleton membrane, and positive electrode, and then packaged with aluminum plastic film to obtain a battery with a porous skeleton membrane. The porous skeleton membrane was a 100um thick wood cellulose membrane. Then, the solidified precursor liquid was injected into the battery with the porous skeleton membrane. 2 35 μL was added to the solution, in-situ cured at 60° C. for 1 h, and allowed to stand at room temperature for 12 h to obtain a lithium secondary battery.
[0045] The first discharge specific capacity (1C) of the lithium secondary battery obtained in Example 1 is 125 mAh / g, and the effective cycle number is 265.
[0046] Example 2
[0047] In a dry glove box filled with argon (O 2 <0.1ppm, H 2 O<0.1ppm), 20 parts by weight of high steric hindrance monomer vinylene carbonate and 5 parts by weight of high activity crosslinking agent pentaerythritol tetraacrylate are stirred and mixed, and after removing water through a molecular sieve, 5 parts by weight of lithium bis(trifluoromethylsulfonyl)imide (LITFSI) are added and stirred for 30 minutes to completely dissolve the lithium salt, and the obtained mixed solution A is stored at 2-8°C; 0.04 parts by weight of azobis(isobutyronitrile) AIBN initiator and 69.96 parts by weight of a plasticizer (1 mol / L lithium salt solution, the solute is bis(trifluoromethylsulfonyl)imide, and the solvent is a mixed solvent of 1,3-dioxolane (DOL) and dimethyl carbonate (DMC) in a volume ratio of 1:1) are mixed, stirred for 40 minutes to mix evenly, and a mixed solution B is obtained; the mixed solution A and the mixed solution B are mixed and stirred evenly to obtain a curing precursor solution.
[0048] The dried lithium iron phosphate positive electrode and lithium foil negative electrode were cut and stacked in the order of negative electrode, porous skeleton membrane, and positive electrode, and then packaged with aluminum plastic film to obtain a battery cell with a porous skeleton membrane. The porous skeleton membrane was a 22um thick polyimide electrospun membrane. Then, the solidified precursor solution was injected into the battery cell with the porous skeleton membrane. 2 35 μL was added to the solution, in-situ cured at 70° C. for 0.5 h, and allowed to stand at room temperature for 12 h to obtain a lithium secondary battery.
[0049] The first discharge specific capacity (1C) of the lithium secondary battery obtained in Example 2 is 150 mAh / g, and the effective cycle number is 320.
[0050] Example 3
[0051] In a dry glove box filled with argon (O 2 <0.1ppm, H 2 O<0.1ppm), 15 parts by weight of the high steric hindrance monomer Olmesartan medoxomil impurity 83 and 5 parts by weight of the high activity cross-linking agent phosphorus fluoride-based cross-linking agent (FTGA) were stirred and mixed, and after removing water through a molecular sieve, 5 parts by weight of lithium hexafluorophosphate (LiPF 6 ) and stirred for 30 minutes to completely dissolve the lithium salt, and the obtained mixed solution A was stored at 2-8°C; 0.1 parts by mass of azobisisobutyronitrile AIBN initiator and 74.9 parts by mass of plasticizer (1 mol / L lithium salt solution, the solute is lithium hexafluorophosphate, and the solvent is a mixed solvent of ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of 1:1) were mixed, and stirred for 40 minutes to mix evenly to obtain a mixed solution B; the mixed solution A and the mixed solution B were mixed and stirred evenly to obtain a curing precursor solution.
[0052] The dried ternary positive electrode NCM811 and the graphite negative electrode were stacked in the order of negative electrode, porous skeleton membrane, and positive electrode, and then packaged with aluminum-plastic film to obtain a battery with a porous skeleton membrane. The porous skeleton membrane was a 180um thick glass fiber membrane. Then, the solidified precursor liquid was injected into the battery with the porous skeleton membrane. 2 35 μL was added to the solution, in-situ cured at 70° C. for 2 h, and allowed to stand at room temperature for 12 h to obtain a lithium secondary battery.
[0053] The first discharge specific capacity (1C) of the lithium secondary battery obtained in Example 3 is 165 mAh / g, and the effective cycle number is 180.
[0054] Example 4
[0055] In a dry glove box filled with argon (O 2 <0.1ppm, H 2O<0.1ppm), 25 parts by weight of a high steric hindrance monomer 4-bromomethane-1,3-dioxolane-2-one and 5 parts by weight of a high-activity crosslinking agent trimethylolpropane triacrylate are stirred and mixed, and after removing water through a molecular sieve, 5 parts by weight of lithium difluorooxalate borate (LIDFOB) are added and stirred for 30 minutes to completely dissolve the lithium salt, and the obtained mixed solution A is stored at 2-8°C; 0.09 parts by weight of a benzoyl peroxide initiator and 64.91 parts by weight of a plasticizer (1 mol / L lithium salt solution, the solute is lithium difluorooxalate borate, and the solvent is a mixed solvent of propylene carbonate (PC), ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of 1:1:1) are mixed, stirred for 40 minutes to mix evenly, and a mixed solution B is obtained; the mixed solution A and the mixed solution B are mixed and stirred evenly to obtain a curing precursor solution.
[0056] The dried sulfur positive electrode and lithium foil negative electrode were cut and stacked in the order of negative electrode, porous skeleton membrane, and positive electrode, and then packaged with aluminum plastic film to obtain a battery cell with a porous skeleton membrane. The porous skeleton membrane was a 20um thick porous polypropylene membrane. Then, the solidified precursor solution was injected into the battery cell with the porous skeleton membrane. 2 35 μL was added to the solution, in-situ cured at 80° C. for 1 h, and allowed to stand at room temperature for 12 h to obtain a lithium secondary battery.
[0057] The first discharge specific capacity (1C) of the lithium secondary battery obtained in Example 4 is 850 mAh / g, and the effective cycle number is 150.
[0058] Comparative Example 1
[0059] In a dry glove box filled with argon (O 2 <0.1ppm, H 2 O<0.1ppm), 25 parts by mass of high-activity oligomer polyethylene glycol dimethacrylate (PEGDMA) and 5 parts by mass of lithium bis(fluorosulfonyl)imide were stirred for 30 minutes to completely dissolve the lithium salt, and the obtained mixed solution A was stored at 2-8°C; 0.04 parts by mass of azobisisobutyronitrile AIBN initiator and 69.96 parts by mass of plasticizer (1 mol / L lithium salt solution, the solute is lithium bis(fluorosulfonyl)imide, and the solvent is a mixed solvent of 1,3-dioxolane (DOL) and dimethyl carbonate (DMC) in a volume ratio of 1:1) were mixed, stirred for 40 minutes to mix evenly, and a mixed solution B was obtained; the mixed solution A and the mixed solution B were mixed and stirred evenly to obtain a curing precursor solution.
[0060] The dried lithium cobalt oxide positive electrode and graphite negative electrode were cut and stacked in the order of negative electrode, porous skeleton membrane, and positive electrode, and then packaged with aluminum plastic film to obtain a battery with a porous skeleton membrane. The porous skeleton membrane was a 100um thick wood cellulose membrane. Then, the solidified precursor liquid was injected into the battery with the porous skeleton membrane. 2 35 μL was added to the solution, in-situ cured at 60° C. for 1 h, and allowed to stand at room temperature for 12 h to obtain a lithium secondary battery.
[0061] The first discharge specific capacity (1C) of the lithium secondary battery obtained in Comparative Example 1 is 92 mAh / g, and the effective cycle number is 143.
[0062] Comparative Example 2
[0063] In a dry glove box filled with argon (O 2 <0.1ppm, H 2 O<0.1ppm), 25 parts by mass of pentaerythritol tetraacrylate and 5 parts by mass of lithium bis(trifluoromethylsulfonyl)imide (LITFSI) were stirred for 30 minutes to completely dissolve the lithium salt, and the obtained mixed solution A was stored at 2-8°C; 0.04 parts by mass of azobisisobutyronitrile AIBN initiator and 69.96 parts by mass of plasticizer (1 mol / L lithium salt solution, the solute is lithium bis(fluorosulfonyl)imide, and the solvent is a mixed solvent of 1,3-dioxolane (DOL) and dimethyl carbonate (DMC) in a volume ratio of 1:1) were mixed, stirred for 40 minutes to mix evenly, and a mixed solution B was obtained; the mixed solution A and the mixed solution B were mixed and stirred evenly to obtain a curing precursor solution.
[0064] The dried lithium iron phosphate positive electrode and lithium foil negative electrode were cut and stacked in the order of negative electrode, porous skeleton membrane, and positive electrode, and then packaged with aluminum plastic film to obtain a battery cell with a porous skeleton membrane. The porous skeleton membrane was a 22um thick polyimide electrospun membrane. Then, the solidified precursor solution was injected into the battery cell with the porous skeleton membrane. 2 35 μL was added to the solution, in-situ cured at 70° C. for 0.5 h, and allowed to stand at room temperature for 12 h to obtain a lithium secondary battery.
[0065] The first discharge specific capacity (1C) of the lithium secondary battery obtained in Comparative Example 2 is 120 mAh / g, and the effective cycle number is 146.
[0066] Figure 1 The AC impedance curves of the solid polymer fast ion conductors obtained in Example 1 and Comparative Example 1; Figure 1 It can be seen that the solid-state fast ion conductor of the embodiment has an exponential improvement in ion conductivity, indicating that the solid-state fast ion conductor proposed by the present invention is effective. Figure 2The linear sweep voltammetric curves of the solid polymer fast ion conductor obtained in Example 2 and Comparative Example 2 are: Figure 2 It can be seen that compared with the comparative example, the electrochemical stability window of the solid-state fast ion conductor in the embodiment is broadened, indicating that the high steric hindrance monomer of the present invention makes the in-situ solid-state fast ion conductor system more stable. Figure 3 and Figure 4 It shows that the lithium secondary battery obtained in the embodiment of the present invention has more excellent rate performance and long cycle capacity.
[0067] The above-described embodiments and comparative examples are merely descriptions of preferred embodiments of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, improvements and optimizations may be made within the scope of the present invention, and such improvements and optimizations shall also be deemed as the protection scope of the present invention.
Claims
1. A method for preparing a fast ion conductor based on in-situ curing, characterized in that: The following steps are involved: Step 1. 15 to 30 parts by weight of a high steric hindrance monomer and 5 to 10 parts by weight of a cross-linking agent are mixed, and after removing water through a molecular sieve, 5 to 10 parts by weight of a lithium salt are added and mixed evenly, and the obtained mixed solution A is stored at 2 to 8°C; Step 2. 0.04-0.12 parts by mass of the initiator and 49.96-79.88 parts by mass of the plasticizer are mixed, and stirred for 30-120 minutes to mix evenly to obtain a mixed solution B; Step 3. Mix the mixed solution A of step 1 and the mixed solution B of step 2, stir evenly, and obtain a curing precursor solution; Step 4. Inject the solidification precursor solution prepared in step 3 into the battery cell with porous skeleton membrane, 2 Add 10 to 35 μL, and in-situ cure at 30 to 80° C. for 0.5 to 48 hours to obtain a solid polymer fast ion conductor; Wherein, the high steric hindrance monomer is one or more of the following structural formulas: R1 is H or -CH3, R2 is a carbon chain with less than 4 carbon atoms, and X is F, Cl, Br or I; The crosslinking agent is an acrylic acid or methacrylic acid crosslinking agent.
2. The method for preparing a fast ion conductor based on in-situ curing according to claim 1, characterized in that: The high steric hindrance monomer is one or more of maleic anhydride, vinylene carbonate, dichlorovinyl carbonate, 4,5-dimethyl-1,3-dioxol-2-one, 4-chloromethyl-5-methyl-1,3-dioxol-2-one, 4-formyl-5-methyl-1,3-dioxol-2-one, olmesartan medoxomil impurity 83, 4-bromomethane-1,3-dioxolane-2-one, and 4-tert-butyl-5-methyl-1,3-dioxolane-2-one.
3. The method for preparing a fast ion conductor based on in-situ curing according to claim 1, characterized in that: The lithium salt is one or more of lithium hexafluorophosphate, lithium bis(trifluoromethylsulfonyl)imide, lithium perchlorate, lithium bis(fluorosulfonyl)imide, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium tetrafluoroborate, and lithium polyborate.
4. The method for preparing a fast ion conductor based on in-situ curing according to claim 1, characterized in that: The initiator is one or more of azobisisobutyronitrile, azobisisovaleronitrile, azobisisoheptanenitrile, benzoyl peroxide, Al(OTf)3, lithium iodide, and lithium hexafluorophosphate.
5. The method for preparing a fast ion conductor based on in-situ curing according to claim 1, characterized in that: The plasticizer is a 0.8-2 mol / L lithium salt solution, the solute of the lithium salt solution is one or more of lithium hexafluorophosphate, lithium bis(trifluoromethylsulfonyl)imide, lithium perchlorate, lithium bis(fluorosulfonyl)imide, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium tetrafluoroborate, and lithium polyborate, and the solvent is one or more of ethylene carbonate, propylene carbonate, dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, and 1,3-dioxolane.
6. The method for preparing a fast ion conductor based on in-situ curing according to claim 1, characterized in that: The battery cell with the porous skeleton membrane in step 4 is obtained by stacking the positive electrode sheet, the porous skeleton membrane and the negative electrode sheet in sequence and then encapsulating them with an aluminum-plastic film.
7. The method for preparing a fast ion conductor based on in-situ curing according to claim 6, characterized in that: The active material of the positive electrode plate is one of lithium iron phosphate, lithium nickel oxide, lithium cobalt oxide, lithium iron manganese phosphate, lithium manganese oxide, lithium nickel manganese oxide, nickel cobalt manganese ternary positive electrode, and sulfur positive electrode; the active material of the negative electrode plate is one of metal lithium sheet, metal lithium alloy, graphite, hard carbon, molybdenum disulfide, lithium titanate, graphene, and silicon carbon negative electrode; the porous skeleton membrane is one of polyethylene film, polypropylene film, wood cellulose film, glass fiber film, polyimide electrospun membrane, polyvinylidene fluoride electrospun membrane, and polyacrylonitrile electrospun membrane.
8. Use of the fast ion conductor obtained by the method of any one of claims 1 to 7 in a lithium secondary battery.
Citation Information
Patent Citations
Polymer electrolyte based on vinylene carbonate and polyethylene (methyl) acrylate and preparation method of polymer electrolyte
CN107492680A
In-situ flame-retardant solid electrolyte and preparation method thereof
CN107645015A
Composite electrolyte structure and lithium metal battery including the same
CN108232289A
Solid polymer electrolyte and solid lithium ion battery
CN110518282A
Polymerized in-situ hybrid solid ion-conductive compositions
CN110914940A