Manufacturing process of shaft seal outer ring of nuclear power plant main pump
Through the five-axis machining center and thermal spraying process, the electroplating technology bottleneck in the manufacturing of the shaft seal outer ring of the nuclear main pump shaft seal of the nuclear power plant has been solved, localized manufacturing has been achieved, the cost and cycle have been reduced, the sealing effect and service life have been improved, and ensured It improves the quality and safety of the coating and solves the problems of peeling and peeling of the coating.
Patent Information
- Application Number
- CN202211189274.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-28
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-09-28
AI Technical Summary
It is difficult to efficiently manufacture the outer ring of the main pump shaft seal of a nuclear power plant in China with the existing technology. The electroplating technology has high cost, long cycle and great uncertainty, which leads to domestic manufacturing bottlenecks, and it is not easy to control the grinding parameters after electroplating. The coating peels and falls off, affecting the sealing effect and operational safety.
A five-axis machining center is used to process the outer ring of the shaft seal. Combined with the thermal spray process, the geometric tolerance and coating quality are ensured through surface grinding and non-destructive testing. A thermal spray coating of 75% Cr3C2 and 25% NiCr powder is used for display. Micro-hardness and bonding strength testing ensure the thickness, dimensional accuracy and geometric tolerance of the coating to avoid peeling and peeling of the coating.
It has realized the domestic manufacturing of the outer ring of the shaft seal of the nuclear power plant, reduced the cost and cycle, improved the sealing effect and service life, ensured the quality and safety of the coating, and avoided the shedding of the coating during disassembly and extreme circumstances. , which meets the operational requirements of nuclear power plants.
Smart Images

Figure CN115519439B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a manufacturing process for a shaft seal outer ring of a shaft seal core main pump of a nuclear power station. Background Art
[0002] The outer ring of the shaft seal of the nuclear power plant's main pump is a key component of the shaft seal main pump. The manufacturing accuracy of the outer ring of the shaft seal of the nuclear power plant's main pump directly affects the operation of the tertiary seal. If the shape and position tolerances of the outer ring cannot meet the accuracy requirements, it will affect the sealing effect of the mechanical seal and the safe operation of the nuclear power plant.
[0003] The surface treatment process for the outer ring and other components used to be electroplating, but the electroplating technology that meets the technical requirements of the nuclear main pump has not yet been mastered in China. Electroplating abroad not only increases costs but also has a long cycle, and due to the influence of various factors, there will be great uncertainty, and it may happen that the electroplating cannot be completed abroad. In the past, the grinding after electroplating was also completed by foreign countries. Once the grinding parameters are not well controlled, the coating will peel and fall off, and the thickness will be uneven. Therefore, the grinding parameters after electroplating are not controlled. These have restricted the domestic manufacturing of the shaft seal nuclear main pump shaft seal outer ring and other components. Summary of the invention
[0004] The purpose of the present invention is to disclose a manufacturing process for a shaft seal outer ring of a nuclear main pump of a nuclear power plant with high reliability, high precision and high efficiency. The technical solution of the present invention is: a manufacturing process for a shaft seal outer ring of a nuclear main pump of a nuclear power plant, comprising the following steps:
[0005] 1) Complete the machining of the outer ring (1) on the forging blank according to the drawing requirements, including rough turning, semi-finishing turning, and finishing turning, and leave a grinding allowance of 0.2 mm at the spraying position (2);
[0006] 2) The outer ring (1) is drilled, tapped and milled on the machining center equipment;
[0007] 3) Manually clean the metal burrs generated during the processing of the outer ring (1);
[0008] 4) According to the drawing requirements, use a grinder to complete the surface grinding of the outer ring (1) at the spraying position (2) before spraying, and the surface roughness reaches Ra0.8μm;
[0009] 5) Nondestructive penetrant testing of the outer ring (1) surface: first use a dye penetrant cleaning agent to remove the surface grease, apply a dye penetrant penetrant to the outer ring (1) surface, and the penetration time shall not be less than 20 minutes. The inspected area of the outer ring (1) surface shall remain moist during the penetration waiting time. Remove excess dye penetrant penetrant. After removing excess dye penetrant penetrant, dry the outer ring surface by normal evaporation. Apply a dye penetrant developer to the outer ring (1) surface. There shall be no hairline, cracks, cuts or other defects on the outer ring surface. The following are unqualified: a. Linear defect display; b. Circular defect display greater than 3 mm; c. Three or more defects arranged in a straight line with the spacing between each defect less than 3 mm;
[0010] 6) Perform surface thermal spraying on the spraying position (2), with the spraying thickness not less than 0.2 mm;
[0011] 7) Use a grinder to complete the surface grinding of the spraying position (2) after spraying according to the drawing requirements. The surface roughness of the spraying position (2) is Ra0.8μm;
[0012] 8) Repeat step 5) to perform non-destructive testing of the spraying position (2) to complete the entire process.
[0013] Step 4) The grinding parameters used are: grinding wheel speed 22~25m / s, workpiece speed: 10~12m / min, grinding wheel axial movement 380~420mm / min, grinding wheel radial feed 0.001~0.003mm.
[0014] In step 6), at least 5 points are selected to measure the microhardness of the coating, and the average hardness value is required to be between 700HV and 900HV. In step 6), at least 5 points are selected to test the bonding strength of the coating, and the average bonding strength value is required to be not less than 70MPa.
[0015] Step 6) Use the drop hammer method to test the bonding strength on the sample. Place a semicircular hammer with a diameter of 10 mm on the coating surface and use another hammer to hammer the coating to obtain a small pit of about 0.2 mm. Cracks are allowed at the edge of the small pit, but the coating on the surface of the pit is considered qualified if there is no peeling or shedding.
[0016] Step 6) The specific test steps of the thermal vibration test used are as follows: heat the coated sample to 350°C, keep it warm for 10 minutes, then quickly immerse it in room temperature water to cool it for 5 seconds to 10 seconds, which is recorded as one cycle. After 10 cycles, visually inspect the coating surface to ensure that there is no peeling or shedding of the coating.
[0017] The thermal spraying powder used in step 6) is 75% by mass of Cr3C2 and 25% by mass of NiCr.
[0018] The above process steps are also applicable to other outer rings and shaft seal guide rings of the shaft seal main pump of the nuclear power plant, and the main pump shutdown seal moving ring.
[0019] Technical effects of the present invention:
[0020] The present invention adopts a five-axis machining center to process all holes and slots of various angles. The advantage of this method is that the processing of all holes and slots of various angles can be completed in one clamping. The angle conversion of the workpiece can be completed by rotating the worktable of the five-axis machining center, thereby ensuring the form and position tolerances of holes and slots of various angles and the corresponding position accuracy requirements.
[0021] The present invention creatively selects spraying as a surface treatment process and applies it to the manufacture of the shaft seal outer ring of the shaft seal main pump, replacing the existing electroplating process, so that the main pump shaft seal outer ring component does not need to be shipped abroad for electroplating, which solves the manufacturing bottleneck of the localization of the main pump, completes the localization of key processes, greatly reduces costs, shortens cycles, and greatly improves the service life of the nuclear main pump shaft seal of the nuclear power plant and increases strength. Before and after surface spraying, the spraying position must be non-destructively tested to ensure the quality of thermal spraying of the workpiece.
[0022] In the technical solution of the present invention, the grinding wheel speed is 22-25 m / s, the workpiece speed is 10-12 m / min, the grinding wheel axial movement is 380-420 mm / min, and the grinding wheel radial feed is 0.001-0.003 mm. Through research and experiments, the grinder selects appropriate grinding parameters to grind the sprayed surface, thereby ensuring the thickness of the sprayed layer and the dimensional accuracy and form and position tolerance accuracy of the sprayed layer. More importantly, the coating will not peel or fall off, and the thickness will not be uneven due to the selection of inappropriate parameters during grinding. There is no need to grind abroad, which reduces the manufacturing cost and greatly shortens the manufacturing cycle.
[0023] In the technical solution of the present invention, at least 5 points are selected for microhardness, and the average hardness value is required to be between 700HV and 900HV, which can ensure that the thermal spray coating surface of the shaft seal outer ring of the main pump is not scratched during disassembly and assembly, thereby ensuring the normal disassembly and assembly of the outer ring. In particular, when the main pump shaft seal is overhauled, the outer ring is located outside the shaft seal, and rubs against the seal body during disassembly and assembly, and the entire shaft seal sleeve is radiated. If it is scratched, it will be difficult to remove, increasing the risk of maintenance personnel being exposed to radiation. This method can effectively detect the hardness quality of the spray layer, avoid scratches, and ensure the smooth disassembly and assembly of the shaft seal. The coating bonding strength test used in the technical solution of the present invention selects at least 5 points, and the average bonding strength value is required to be not less than 70MPa. The bonding force between the coating and the substrate can be detected to ensure that the coating will not fall off from the surface of the substrate, thereby ensuring that the main pump will not be affected by the shedding of the coating and the normal assembly. Moreover, if the coating falls off into the coolant, it may cause an accident. This method is used to detect whether the coating bonding strength is qualified.
[0024] In the technical solution of the present invention, the coated sample is heated to 350°C, kept warm for 10 minutes, and then quickly immersed in water at room temperature for cooling for 5 to 10 seconds, which is recorded as one cycle. After 10 cycles, the coating surface is visually inspected, and it is required that the coating has no peeling or shedding. This method can ensure that in the event of a sudden loss of cooling water in a nuclear power plant, simulating the use of seawater as a coolant, whether the thermal spray coating has shedding phenomenon, and can detect the quality of the coating under such extreme conditions.
[0025] The powder used for thermal spraying in the technical solution of the present invention is composed of 75% by mass of Cr3C2 and 25% by mass of NiCr. It can improve the toughness and bonding strength of the coating while ensuring the hardness, and can meet the main pump operating conditions and various extreme conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 Schematic diagram of the outer ring and spraying position DETAILED DESCRIPTION
[0027] A manufacturing process for a shaft seal outer ring of a nuclear power plant shaft seal core main pump, comprising the following steps:
[0028] 1) Complete the machining sequence of outer ring 1 on the forging blank according to the drawing requirements, including rough turning, semi-finishing turning, and finishing turning, and leave a 0.2mm grinding allowance at the spraying position 2;
[0029] 2) If Figure 1 As shown, the outer ring 1 is drilled, tapped and milled on the machining center equipment;
[0030] 3) Manually clean the metal burrs generated during the processing of the outer ring 1;
[0031] 4) According to the requirements of the drawing, the surface of the outer ring 1 spraying position 2 is ground by a grinder before spraying, and the surface roughness reaches Ra0.8μm;
[0032] 5) Nondestructive penetrant testing of the outer ring 1 surface: first use a dye penetrant cleaning agent to remove the surface grease covering, apply a dye penetrant penetrant to the outer ring 1 surface, the penetration time is not less than 20 minutes, the outer ring 1 surface area to be inspected should be kept moist during the penetration waiting time, remove excess dye penetrant penetrant, remove excess dye penetrant penetrant and use normal evaporation to dry the outer ring surface, apply a dye penetrant developer to the outer ring 1 surface, the outer ring surface should not have hairline, cracks, cuts and other defects, the following are unqualified: a, linear defect display; b, circular defect display greater than 3 mm; c, three or more displays arranged in a straight line and the distance between each defect is less than 3 mm;
[0033] 6) If Figure 1 As shown, the surface of the spraying position 2 is thermally sprayed, and the spraying thickness is not less than 0.2mm;
[0034] 7) Use a grinder to complete the surface grinding of spraying position 2 after spraying according to the drawing requirements. The surface roughness of spraying position 2 is Ra0.8μm;
[0035] 8) Repeat step 5) to perform nondestructive testing at spraying position 2 to complete the entire process.
[0036] Step 4) The grinding parameters used are: grinding wheel speed 22~25m / s, workpiece speed: 10~12m / min, grinding wheel axial movement 380~420mm / min, grinding wheel radial feed 0.001~0.003mm.
[0037] In step 6), at least 5 points are selected to measure the microhardness of the coating, and the average hardness value is required to be between 700HV and 900HV. In step 6), at least 5 points are selected to test the bonding strength of the coating, and the average bonding strength value is required to be not less than 70MPa.
[0038] Step 6) Use the drop hammer method to test the bonding strength on the sample. Place a semicircular hammer with a diameter of 10 mm on the coating surface and use another hammer to hammer the coating to obtain a small pit of about 0.2 mm. Cracks are allowed at the edge of the small pit, but the coating on the surface of the pit is considered qualified if there is no peeling or shedding.
[0039] Step 6) The specific test steps of the thermal vibration test used are as follows: heat the coated sample to 350°C, keep it warm for 10 minutes, then quickly immerse it in room temperature water to cool it for 5 seconds to 10 seconds, which is recorded as one cycle. After 10 cycles, visually inspect the coating surface to ensure that there is no peeling or shedding of the coating.
[0040] The thermal spraying powder used in step 6) is 75% by mass of Cr3C2 and 25% by mass of NiCr.
[0041] The above process steps of the present invention are also applicable to other outer rings and shaft seal guide rings of the shaft seal main pump of a nuclear power plant, and a main pump stop seal movable ring.
Claims
1. A manufacturing process for the outer ring of the shaft seal of a nuclear power plant main pump. Its characteristics are: The following steps are involved: 1) Complete the machining of the outer ring (1) on the forging blank according to the drawing requirements, including rough turning, semi-finishing turning, and finishing turning, and leave a grinding allowance of 0.2 mm at the spraying position (2); 2) The outer ring (1) is drilled, tapped and milled on the machining center equipment; 3) Manually clean the metal burrs generated during the processing of the outer ring (1); 4) According to the requirements of the drawing, the outer ring (1) is ground at the spraying position (2) before spraying using a grinding machine, and the surface roughness reaches Ra0.8μm. The grinding parameters used are: grinding wheel speed 22~25m / s, workpiece speed: 10~12m / min, grinding wheel axial movement 380~420mm / min, grinding wheel radial feed 0.001~0.003mm; 5) Nondestructive penetrant testing of the outer ring (1) surface: first use a dye penetrant cleaning agent to remove the surface grease covering, apply a dye penetrant penetrant to the outer ring (1) surface, and the penetration time shall not be less than 20 minutes. The inspected area of the outer ring (1) surface shall remain moist during the penetration waiting time, remove the excess dye penetrant penetrant, and dry the outer ring surface by normal evaporation after removing the excess dye penetrant penetrant. Apply a dye penetrant developer to the outer ring (1) surface. There shall be no hairline, cracks, or cuts on the outer ring surface. The following are unqualified: a. Linear defect display; b. Circular defect display greater than 3 mm; c. Three or more defects are displayed in a straight line and the distance between each defect is less than 3 mm; 6) Perform surface thermal spraying on the spraying position (2), with the spraying thickness not less than 0.2 mm; 7) Use a grinder to complete the surface grinding of the spraying position (2) after spraying according to the drawing requirements. The surface roughness of the spraying position (2) is Ra0.8μm; 8) Repeat step 5) to perform non-destructive testing of the spraying position (2) to complete the entire process.
2. The manufacturing process of the shaft seal outer ring of the nuclear power plant shaft seal core main pump according to claim 1, Its characteristics are: In step 6), at least 5 points are selected to measure the microhardness of the coating, and the average hardness value is required to be between 700HV and 900HV. In step 6), at least 5 points are selected to test the bonding strength of the coating, and the average bonding strength value is required to be not less than 70MPa.
3. The manufacturing process of the shaft seal outer ring of the nuclear power plant shaft seal core main pump according to claim 1, Its characteristics are: Step 6) The bonding strength test is performed on the sample using the drop hammer method. A semicircular hammer with a diameter of 10 mm is placed on the coating surface, and the coating is hammered with another hammer to obtain a 0.2 mm small pit. Cracks are allowed at the edge of the small pit, but the coating on the surface of the pit is considered qualified if there is no peeling or shedding.
4. The manufacturing process of the shaft seal outer ring of the nuclear power plant shaft seal core main pump according to claim 1, Its characteristics are: Step 6) The specific test steps of the thermal vibration test used are as follows: heat the coated sample to 350°C, keep it warm for 10 minutes, then quickly immerse it in room temperature water to cool it for 5 seconds to 10 seconds, which is recorded as one cycle. After 10 cycles, visually inspect the coating surface to ensure that there is no peeling or shedding of the coating.
5. The manufacturing process of the shaft seal outer ring of the nuclear power plant shaft seal core main pump according to claim 1, Its characteristics are: The thermal spraying powder used in step 6) is 75% by mass of Cr3C2 and 25% by mass of NiCr.
6. The manufacturing process of the shaft seal outer ring of the nuclear power plant shaft seal core main pump according to claim 1, Its characteristics are: The above process steps are also applicable to the shaft seal guide ring of the main pump of the nuclear power plant shaft seal and the main pump shutdown seal movable ring.
Citation Information
Patent Citations
Method for providing a coating layer with protection and thermal conductivity
CN103290402A