A polylipoic acid / polyvinyl pyrrolidone composite material and its preparation method and application
Through the preparation of a double network system of polylipoic acid and polyvinylpyrrolidone composite materials, the problems of poor mechanical properties and low light transmittance of electronic or ionic skin materials are solved, high transparency and ultraviolet shielding effect are achieved, and biodegradable raw materials are used. Providing an environmentally friendly and efficient solution.
Patent Information
- Application Number
- CN202211214939.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-30
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-09-30
AI Technical Summary
Existing composite materials for preparing electronic or ionic skin have problems such as poor mechanical properties, low light transmittance, and difficulty in effectively blocking ultraviolet radiation, and most of the materials used are non-renewable or toxic resources.
The preparation method of polylipoic acid and polyvinylpyrrolidone composite materials is used to form a stable double network system by dissolving and reacting at 40~70°C. Lithium salt and inorganic cross-linking agent are added to improve the conductivity and ultraviolet shielding performance of the material.
It achieves high transparency of visible light transmittance and effective UV blocking. The material has excellent mechanical properties and self-healing ability, and the raw materials used are biodegradable and the preparation conditions are mild.
Smart Images

Figure CN115521487B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of flexible electronic materials, and in particular to a polylipoic acid / polyvinyl pyrrolidone composite material and a preparation method and application thereof. Background Art
[0002] With the popularization of smart terminals, the public has higher and higher requirements for the functions of electronic or ionic skin. In order to better meet the requirements of electronic or ionic skin, the composite materials used to prepare electronic or ionic skin should have good mechanical, self-repairing, high light transmittance and other properties.
[0003] The existing composite materials for preparing electronic or ionic skin mainly achieve the above performance requirements by combining rigid conductive nanomaterials or liquid metals into stretchable polymer networks, but they usually have defects such as limited stretchability, inability to form transparent elastomeric conductive materials, poor biocompatibility, and high preparation costs. In order to achieve the mechanical controllability and self-healing properties of transparent elastomeric conductive materials, many researchers have introduced dynamic covalent bonds or reversible non-covalent bonds, including imine bonds, disulfide bonds, hydrazone bonds, borate bonds, hydrogen bonds, coordination bonds, etc., during the material preparation process to achieve the regulation of mechanical and self-healing properties. However, in the preparation process of most conductive materials, it is inevitable that toxic substances are easily released during the synthesis process or the raw materials are used during use, which is harmful to human health. In addition, many raw materials are non-renewable or difficult to degrade resources, which greatly limits the practical application of flexible conductive materials. In order to get rid of the free radical polymerization using toxic substances, it is very important to use more composite, green and safe materials to prepare ionic or electronic skin. α-Lipoic acid (TA) is a natural short-chain fatty acid containing carboxyl groups and disulfide bonds produced by plants, animals and humans. The structure of lipoic acid contains dynamic covalent disulfide bonds and non-covalent hydrogen bonds of carboxyl groups. The ring-opening polymerization (ROP) reaction of lipoic acid (TA) can be used to prepare ionic or electronic skin, which provides a new solution to the above problems.
[0004] The prior art evenly mixes four solid raw materials, lipoic acid, conductive filler, iron salt and crosslinking agent, and reacts them at 80-120°C for 2-6 hours before pouring them into a mold for curing to obtain a composite elastic conductive material with self-healing properties. However, due to the high temperature of the lipoic acid ring-opening polymerization reaction, the stability of the prepared single-layer polylipoic acid network structure is poor, and the tensile strength, light transmittance and other properties of the prepared composite elastic conductive are reduced. Summary of the invention
[0005] The present invention provides a method for preparing a polylipoic acid / polyvinyl pyrrolidone composite material in order to overcome the problems that the composite elastic conductive material prepared by the prior art has poor mechanical properties, low light transmittance in the visible light range and is difficult to effectively block ultraviolet radiation.
[0006] Another object of the present invention is to provide a polylipoic acid / polyvinyl pyrrolidone composite material.
[0007] Another object of the present invention is to provide application of the polylipoic acid / polyvinyl pyrrolidone composite material in electronic or ionic skin.
[0008] In order to solve the above technical problems, the technical solution adopted by the present invention is:
[0009] A method for preparing a polylipoic acid / polyvinyl pyrrolidone composite material comprises the following steps:
[0010] First, lipoic acid and polyvinyl pyrrolidone are dissolved in a polar solvent, and reacted at 40-70° C. for 10-30 minutes to form a mixed solution; secondly, an organic crosslinking agent is added to the mixed solution at 40-70° C. and reacted for 20-60 minutes; finally, the temperature of the mixed solution is maintained at 40-70° C., lithium salt is added, mixed evenly, and then an inorganic crosslinking agent is added to react for 5-30 minutes and dried to obtain the polylipoic acid / polyvinyl pyrrolidone composite material; the mass ratios of lipoic acid, polyvinyl pyrrolidone, organic crosslinking agent, lithium salt and inorganic crosslinking agent in the composite electronic material are: (7-16): (4-14): (1.8-6): (1-6): (0.035-0.70).
[0011] The present invention fully dissolves polyvinyl pyrrolidone and thioctic acid monomers in a polar solvent at 40-70°C, and the disulfide bonds in the thioctic acid undergo ring-opening polymerization under heating to form polythioctic acid; secondly, in the process of adding an organic crosslinking agent, the disulfide bonds are stabilized, and the polythioctic acid molecules are crosslinked to form a stable double network system with polyvinyl pyrrolidone; the addition of lithium salt further improves the material conductivity of the material; finally, an inorganic crosslinking agent (metal ion) with coordination ability is added to form a coordination bond between the carboxyl group in the side chain structure of the polythioctic acid and the metal ion to obtain a stable composite material. The mechanical strength of the prepared composite material is adjusted by adjusting the ratio of thioctic acid to polyvinyl pyrrolidone, the molecular weight of polyvinyl pyrrolidone, and the content of different ions added.
[0012] Since only amide bond in polyvinyl pyrrolidone participates in ion coordination, amide bond coordination ability is relatively poor, so ion coordination is mainly concentrated in carboxyl and metal ions in polylipoic acid. Therefore, the polymer network cross-linked structure formed is relatively loose, so the present invention provides the polylipoic acid / polyvinyl pyrrolidone composite material with high transparency, and the light transmittance in the visible light region can reach more than 88.9%. Since dynamic disulfide bonds in the polylipoic acid network can absorb the energy of ultraviolet light, the light transmittance in ultraviolet light is close to 0, so the present invention provides the polylipoic acid / polyvinyl pyrrolidone composite material that can shield the passage of ultraviolet light in the ultraviolet region, and can play the effect of effectively blocking ultraviolet radiation.
[0013] The lipoic acid, polylipoic acid and polyvinyl pyrrolidone of the present invention are biodegradable raw materials, wherein the number average molecular weight of polyvinyl pyrrolidone is 58000-1300000.
[0014] Preferably, the mass ratio of lipoic acid to polyvinyl pyrrolidone of the present invention is (10-12):(8-10).
[0015] Preferably, the mass ratio of the organic crosslinking agent, the lithium salt and the inorganic crosslinking agent of the present invention is (2.0-2.4):4:(0.35-0.37).
[0016] Preferably, the reaction temperature of the lipoic acid and polyvinyl pyrrolidone in the polar solvent of the present invention is 60°C.
[0017] The polar solvent described in the present invention is one or more of methanol, ethanol, propanol, glycerol, N,N-dimethylformamide and dimethyl sulfoxide.
[0018] The lithium salt described in the present invention is one or more of lithium chloride, lithium perchlorate, lithium tetrafluoroborate, lithium hexafluorophosphate, lithium bis(difluorosulfonyl)imide and lithium bis(trifluoromethylsulfonyl)imide.
[0019] The organic crosslinking agent of the present invention is one or more of 1,4-butylene glycol diacrylate, 1,3-diisopropenylbenzene, divinylbenzene, styrene, itaconic acid, polyethylene glycol (600) diacrylate, hydroxyethyl methacrylate, and acrylic acid.
[0020] The inorganic crosslinking agent of the present invention is one or more of iron salts, copper salts, aluminum salts, vanadium salts, cobalt salts, nickel salts, chromium salts, manganese salts, zinc salts and zirconium salts.
[0021] Preferably, the inorganic crosslinking agent described in the present invention is one or more of zinc chloride, ferric chloride, aluminum chloride, and zirconium oxychloride.
[0022] The present invention also protects a polylipoic acid / polyvinyl pyrrolidone composite material, which is prepared by the above preparation method.
[0023] The polylipoic acid / polyvinyl pyrrolidone composite material of the present invention has a visible light transmittance of more than 88.9% and an ultraviolet light transmittance close to 0, and can achieve visible light visibility and effective ultraviolet light blocking.
[0024] The present invention also protects the use of the polylipoic acid / polyvinyl pyrrolidone composite material in preparing electronic or ionic skin.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] The preparation method of the polylipoic acid / polyvinyl pyrrolidone composite material provided by the present invention is simple, the polymerization conditions are mild, and the composite material is biodegradable. The ring-opening polymerization reaction temperature of the lipoic acid of the present invention is 40-70° C. to obtain a stable flexible polylipoic acid network, and polyvinyl pyrrolidone is used as a rigid network framework. The two are interlaced with each other to form a polylipoic acid / polyvinyl pyrrolidone composite material with excellent mechanical properties, strong self-repairing ability, high light transmittance in the visible light region, and ultraviolet light blocking in the ultraviolet region. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The XRD spectra of the polylipoic acid / polyvinyl pyrrolidone composite material prepared in the example, wherein TA represents lipoic acid, PVP represents polyvinyl pyrrolidone, PTA represents polylipoic acid, PTA@PVP3, PTA@PVP 12 ,PTA@PVP 13 They represent the polylipoic acid / polyvinyl pyrrolidone composite materials prepared in Examples 3, 12 and 13 respectively.
[0028] Figure 2 is the tensile stress-strain cycle curve of the polylipoic acid / polyvinyl pyrrolidone composite material prepared in Example 11 at strains of 50%, 100%, 200%, 300%, 400%, and 500% respectively;
[0029] Figure 3 The transmittance curves of the polylipoic acid / polyvinyl pyrrolidone composite material prepared in Example 9 at different wavelengths;
[0030] Figure 4 The change of resistance of the polylipoic acid / polyvinyl pyrrolidone composite material prepared in Example 3 after 5 cycles of cutting and healing;
[0031] Figure 5This is a digital photo of the polylipoic acid / polyvinyl pyrrolidone composite material prepared in Example 3 being cut and healed and lifting a heavy object;
[0032] Figure 6 The relative resistance change of the polylipoic acid / polyvinyl pyrrolidone composite material prepared in Example 3 as electronic or ionic skin at the human finger joints as the fingers are bent at different angles. DETAILED DESCRIPTION
[0033] The present invention will be further described below in conjunction with specific embodiments, but the embodiments do not limit the present invention in any form. Those skilled in the art will understand that the changes, replacements, and improvements made to the present invention still belong to the protection scope of the present invention. Unless otherwise specified, the raw material reagents used in the embodiments of the present invention are conventionally purchased raw material reagents.
[0034] Raw material sources: lipoic acid (McLean), polyvinyl pyrrolidone (McLean), lithium chloride (McLean), ferric chloride hexahydrate (McLean), 1,4-dibutyl 1,4-diacrylate (McLean).
[0035] Example 1
[0036] A method for preparing a polylipoic acid / polyvinyl pyrrolidone composite material comprises the following steps:
[0037] First, lipoic acid and polyvinyl pyrrolidone (number average molecular weight 220000) are dissolved in anhydrous ethanol, reacted at 60°C for 10 minutes, then cross-linked 1,4-butylene glycol diacrylate is added and reacted for 30 minutes, then lithium chloride is added and reacted for 10 minutes, and finally ferric chloride is added and reacted for 5 minutes. The mixture is poured into a mold and dried to obtain the polylipoic acid / polyvinyl pyrrolidone composite material; the mass ratio of lipoic acid, polyvinyl pyrrolidone, 1,4-butylene glycol diacrylate, lithium chloride and ferric chloride in the composite material is: 16:4:3.2:4:0.30.
[0038] Example 2
[0039] The difference from Example 1 is that the mass ratio of lipoic acid, polyvinyl pyrrolidone, 1,4-butylene glycol diacrylate, lithium chloride and ferric chloride in the composite material is: 14:6:2.8:4:0.33.
[0040] Example 3
[0041] The difference from Example 1 is that the mass ratio of lipoic acid, polyvinyl pyrrolidone, 1,4-butylene glycol diacrylate, lithium chloride and ferric chloride in the composite material is 12:8:2.4:4:0.35.
[0042] Example 4
[0043] The difference from Example 1 is that the mass ratio of lipoic acid, polyvinyl pyrrolidone, 1,4-butylene glycol diacrylate, lithium chloride and ferric chloride in the composite material is 10:10:2:4:0.37.
[0044] Example 5
[0045] The difference from Example 3 is that the reaction temperature of the polylipoic acid / polyvinyl pyrrolidone composite material is 40°C.
[0046] Example 6
[0047] The difference from Example 3 is that the reaction temperature of the polylipoic acid / polyvinyl pyrrolidone composite material is 70°C.
[0048] Example 7
[0049] The difference from Example 1 is that the mass ratio of lipoic acid, polyvinyl pyrrolidone, 1,4-butylene glycol diacrylate, lithium chloride and ferric chloride in the composite material is: 16:14:1.8:1:0.035.
[0050] Example 8
[0051] The difference from Example 1 is that the mass ratio of lipoic acid, polyvinyl pyrrolidone, 1,4-butylene glycol diacrylate, lithium chloride and ferric chloride in the composite material is 7:4:6:6:0.7.
[0052] Example 9
[0053] The difference from Example 3 is that the number average molecular weight of the polyvinyl pyrrolidone used is 600,000.
[0054] Example 10
[0055] The difference from Example 3 is that the number average molecular weight of the polyvinyl pyrrolidone used is 1,300,000.
[0056] Embodiment 11
[0057] The difference from Example 3 is that the mass ratio of lipoic acid, polyvinyl pyrrolidone, 1,4-butylene glycol diacrylate, lithium chloride and ferric chloride in the composite material is: 12:8:2.4:4:0.175.
[0058] Example 12
[0059] The difference from Example 3 is that the mass ratio of lipoic acid, polyvinyl pyrrolidone, 1,4-butylene glycol diacrylate, lithium chloride and ferric chloride in the composite material is: 12:8:2.4:4:0.07.
[0060] Example 13
[0061] The difference from Example 3 is that the mass ratio of lipoic acid, polyvinyl pyrrolidone, 1,4-butylene glycol diacrylate, lithium chloride and ferric chloride in the composite material is: 12:8:2.4:4:0.035.
[0062] Embodiment 14
[0063] The difference from Example 3 is that the number average molecular weight of the polyvinyl pyrrolidone used is 58,000.
[0064] Embodiment 15
[0065] The difference from Example 3 is that the number average molecular weight of the polyvinyl pyrrolidone used is 850,000.
[0066] Comparative Example 1
[0067] The difference from Example 3 is that first, lipoic acid and polyvinyl alcohol are fully dissolved in anhydrous ethanol at 60° C. and reacted for 10 minutes; then cross-linked 1,4-diacrylate butanediol is added and reacted for 30 minutes; secondly, lithium chloride is added and reacted for 10 minutes, and finally ferric chloride solution is added for 5 minutes, poured into a mold and dried, to obtain the polylipoic acid / polyvinyl alcohol composite material.
[0068] Comparative Example 2
[0069] The difference from Example 3 is that lipoic acid and ethyl cellulose are first dissolved in anhydrous ethanol, but after complete dissolution, they are reacted at 60°C for 10 minutes, cross-linked 1,4-diacrylate butanediol is added and reacted for 30 minutes, lithium chloride is then added and reacted for 10 minutes, and finally ferric chloride solution is added for 5 minutes, poured into a mold and dried to obtain the polylipoic acid / ethyl cellulose composite material.
[0070] Comparative Example 3
[0071] The difference from Example 3 is that the method for preparing the polylipoic acid / polyvinyl pyrrolidone composite material is to prepare the polylipoic acid flexible network and the polyvinyl pyrrolidone rigid network separately, and the specific steps are as follows:
[0072] S1: Synthesis of polylipoic acid network: adding lipoic acid monomer to ethanol, adding 1,4-dimethoxybutylene glycol diacrylate crosslinker, and stirring to form a polylipoic acid network solution;
[0073] S2: Synthesis of double network: Add polyvinyl pyrrolidone to the polylipoic acid network solution, stir at a stirring speed of 500-800 rad / min, and dry to obtain a polylipoic acid / polyvinyl pyrrolidone composite material.
[0074] Comparative Example 4
[0075] The difference from Example 3 is that the reaction temperature of the polylipoic acid / polyvinyl pyrrolidone composite material is 80°C.
[0076] Performance Testing
[0077] (1) XRD detection
[0078] Figure 1 The XRD spectra of the polythioic acid / polyvinyl pyrrolidone composite material prepared in Example 3, Example 12 and Example 13. The crystallization peak test results of the raw material thioctic acid and the PTA@PVP polymer are shown in the figure. There are obvious differences in the crystallization peaks of the raw material thioctic acid and the PTA@PVP polymer. It can be judged that thioctic acid no longer exists in the form of small molecules in the polymer, but exists in the form of a polymer. It can be found in the XRD image of thioctic acid that there is a sharp diffraction peak at 23°, and there is a small diffraction peak in the range of 5°~35°. By comparing the crystallization peak of the PTA@PVP polymer, it has no obvious diffraction peak at 23°, indicating that thioctic acid has been polymerized, no crystalline state exists, and there is almost no depolymerization.
[0079] (3) Tensile performance test at different strains
[0080] Tensile properties test method:
[0081] The samples were tested using a universal tensile testing machine of model UTM6103. Before the test, the samples of Examples 1 to 13 and Comparative Examples 1 to 5 were prepared into strips with a specification of 100*10*2 mm for testing. The test speed was 100 mm / min. The stress-strain data and the cyclic tensile data of stress-strain under different strains were tested respectively, and there was no interval in the cyclic test sampling time.
[0082] from Figure 2 It can be seen that the material is accompanied by a certain amount of energy loss during the stretching process. During the stretching process, the internal structure is disconnected and the cross-linked double network gradually loosens; the first thing to be destroyed is the hydrogen bond, followed by the covalent bond and the coordination bond. During the recovery process, hydrogen bonds are formed first due to their smaller bond energy, followed by the formation of dynamic covalent bonds and ionic bonds. Under different strains, the looseness of the double network structure varies with the degree of bond damage, and the proportion of energy loss is also different. The material can have the energy to rebound in the case of large deformation, thanks to the construction of the double network system, which forms a good energy dissipation network, ensuring the structure of the network while also giving it stretchable and rebound properties.
[0083] (4) Light transmission performance test
[0084] Light transmittance test method:
[0085] The sample was prepared into a film with a thickness of 1 mm, and placed on an ultraviolet spectrophotometer with a spherical aberration accessory for wavelength scanning. The scanning range was 200-800 nm, the scanning speed was 2 nm / min, and the number of scans was 1.
[0086] Figure 3 The transmittance data of the polylipoic acid / polyvinyl pyrrolidone composite material at different wavelengths prepared in Example 9 show that the transmittance of the composite material is greater than 88.9%, and when the wavelength is less than 400nm, the transmittance is close to 0%. The composite material can effectively block ultraviolet rays while ensuring transparency. The main reason is that due to the relatively high ultraviolet energy, the energy of the photoelectron can be absorbed by the disulfide bond, causing the disulfide bond to be homolytically split to form two sulfur free radicals. When there is no ultraviolet light, the disulfide bond will spontaneously reform and release energy in other forms (such as heat, etc.). After the ultraviolet energy is absorbed, it plays the role of blocking ultraviolet rays, so the polylipoic acid / polyvinyl pyrrolidone composite material can achieve the technical effect of effectively blocking ultraviolet rays while achieving high transmittance.
[0087] (5) Self-healing performance
[0088] Conductivity test method:
[0089] The conductive self-healing performance was tested using the Geely K2400 digital source meter: the spline in Example 3 (size 10*5*2mm) was connected to the digital source meter. When power was on, the LED bulbs in series could be lit. The spline was then cut in the middle with a blade, and the cuts of the spline were spliced together to observe the brightness of the LED bulbs and the change in resistance after 5 cycles of cutting and healing of the test spline.
[0090] Figure 4 The resistance change of the polylipoic acid / polyvinyl pyrrolidone composite material prepared in Example 3 after 5 cycles of cutting and healing. The dual dynamic cross-linked polymer network also gives the PTA@PVP-LiCl conductive elastomer real-time electrical self-healing ability. First, the PTA@PVP-LiCl conductive elastomer is connected in series with the red diode in the circuit. Then it is cut in half, and the LED indicator in the disconnected circuit immediately dims. After putting the two cut parts together, the LED lights up immediately, indicating the rapid and effective electrical self-healing ability between the re-contacted interfaces. Figure 5 This is a photograph of the composite material prepared in Example 3 being cut and healed for lifting heavy objects. It can be seen that the polylipoic acid / polyvinyl pyrrolidone composite material can still stably lift heavy objects after being cut and healed, and has excellent self-healing properties. The self-healing properties of the composite materials prepared in the other examples are similar to those in Example 3.
[0091] (4) Sensing performance
[0092] Geely K2400 digital source meter was used to conduct tests related to human body sensing applications: the splines were attached to the finger joints of the human body, and the digital source meter was connected in the middle to monitor the changes in resistivity of the finger joints at different bending angles.
[0093] Figure 6 The test results of the sensing performance of the composite material prepared in Example 3 show that the composite material can identify different bending angles of human finger joints. By monitoring the strain of the finger joints at different angles, different bending angles can be distinguished, and the motion state of the human body can be further monitored remotely. Therefore, the sensing performance of the polylipoic acid / polyvinyl pyrrolidone composite material prepared in Example 3 is excellent, and the sensing performance effects of the other examples are similar to those of Example 3.
[0094] Table 1 shows the test results of the structural characteristics, mechanical properties and light transmittance of the composite materials prepared in Examples 1 to 6, 9 to 15 and Comparative Examples 1 to 4. For the composite materials prepared in the present invention, the prepared and synthesized materials are required to be stable. Whether the complete dissolution mentioned in Table 1 refers to whether there is a coagulation phenomenon after ion crosslinking to make a judgment; the mechanical properties of the composite materials must meet the requirements of preparation and application: they can adapt to large strain conditions (strain exceeding 400%), the material stress range is 200KPa-3MPa, and they have good elasticity, that is, they can recover after stretching.
[0095] Table 1 Performance characteristics of the composite materials prepared in Examples 1-6, 9-15 and Comparative Examples 1-4
[0096]
[0097] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A method for preparing a polylipoic acid / polyvinyl pyrrolidone composite material, characterized in that: The following steps are involved: First, lipoic acid and polyvinyl pyrrolidone are dissolved in a polar solvent and reacted at 40-70°C for 10-30 minutes to form a mixed solution; Secondly, an organic crosslinking agent is added to the mixed solution at 40-70° C. and reacted for 20-60 minutes; finally, a lithium salt is added to the mixed solution while maintaining the temperature at 40-70° C., mixed evenly, and then an inorganic crosslinking agent is added and reacted for 5-30 minutes, followed by drying to obtain the polylipoic acid / polyvinyl pyrrolidone composite material; the mass ratio of lipoic acid, polyvinyl pyrrolidone, organic crosslinking agent, lithium salt, and inorganic crosslinking agent in the composite material is: (7-16):(4-14):(1.8-6):(1-6):(0.035-0.70); The organic crosslinking agent is one or more of 1,4-butylene glycol diacrylate, 1,3-diisopropenylbenzene, divinylbenzene, styrene, itaconic acid, polyethylene glycol 600 diacrylate, hydroxyethyl methacrylate, and acrylic acid; The inorganic crosslinking agent is one or more of iron salts, copper salts, aluminum salts, vanadium salts, cobalt salts, nickel salts, chromium salts, manganese salts, zinc salts, and zirconium salts.
2. The method for preparing a polylipoic acid / polyvinyl pyrrolidone composite material according to claim 1, wherein: The number average molecular weight of the polyvinyl pyrrolidone is 58,000-1,300,000.
3. The method for preparing a polylipoic acid / polyvinyl pyrrolidone composite material according to claim 1, wherein: The mass ratio of lipoic acid to polyvinyl pyrrolidone is (10-12):(8-10).
4. The method for preparing a polylipoic acid / polyvinyl pyrrolidone composite material according to claim 1 or 3, wherein: The mass ratio of the organic crosslinking agent, the lithium salt and the inorganic crosslinking agent is (2.0-2.4):4:(0.35-0.37).
5. The method for preparing a polylipoic acid / polyvinyl pyrrolidone composite material according to claim 1, wherein: The reaction temperature of the lipoic acid and polyvinyl pyrrolidone in a polar solvent is 60°C.
6. The method for preparing a polylipoic acid / polyvinyl pyrrolidone composite material according to claim 1, wherein: The polar solvent is one or more of methanol, ethanol, propanol, glycerol, N,N-dimethylformamide, and dimethyl sulfoxide.
7. The polylipoic acid / polyvinyl pyrrolidone composite material prepared by the preparation method according to any one of claims 1 to 6.
8. The polylipoic acid / polyvinyl pyrrolidone composite material according to claim 7, characterized in that: The light transmittance of the polylipoic acid / polyvinyl pyrrolidone composite material in the visible light range reaches more than 88.9%.
9. Use of the polylipoic acid / polyvinyl pyrrolidone composite material according to claim 7 or 8 in electronic or ionic skin.