A honeycomb resin material and preparation method thereof

By in-situ crosslinking and heat treatment of the mixture of aqueous resin, curing agent and water in a low temperature environment, the problems of high manufacturing cost and low strength of honeycomb sheets are solved, and the preparation of honeycomb resin materials with high yield strength and elastic modulus are achieved. It has the advantages of green and environmentally friendly and low-cost production, and improves fire resistance through additives.

CN115521580BActive Publication Date: 2024-11-19UNIV OF SCI & TECH OF CHINA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211238961.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-11
Publication Date
2024-11-19
Estimated Expiration
2042-10-11

AI Technical Summary

Technical Problem

The existing honeycomb plates are costly and have low strength, and cannot achieve lightweight and high strength. The orientation refrigeration technology is economical, time-consuming and energy-consuming, and it is difficult to achieve continuous and low-cost large-scale production. The material yield strength is low, and the crosslinking agent is pollute.

Method used

The mixture of aqueous resin, curing agent and water is frozen in an orientation and crosslinked in situ in a low temperature environment and heat treatment is carried out to obtain a honeycomb resin material. By adjusting the proportion and process parameters of aqueous resin, curing agent and additives, the material density is achieved. and optimization of mechanical properties.

Benefits of technology

It realizes a green and environmentally friendly preparation method, reduces production costs, adjustable material density, excellent mechanical properties, maximum yield strength greater than 20MPa, maximum elastic modulus greater than 500MPa, and fire resistance can be improved through additives.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115521580B_ABST
    Figure CN115521580B_ABST
Patent Text Reader

Abstract

The present invention provides a honeycomb resin material and a preparation method thereof. The honeycomb resin material is obtained by orienting and freezing a mixture of a water-based resin, a curing agent and water, and then in-situ crosslinking and heat treatment in a low-temperature environment. The preparation method is green and environmentally friendly, with a simple process, mild conditions, and energy saving. The raw materials used are inexpensive, which can effectively reduce production costs and facilitate large-scale production. The density of the obtained water-based epoxy resin honeycomb material is adjustable (150-660 mg / cm 3 ), excellent mechanical properties (maximum yield strength>20MPa, maximum elastic modulus>500MPa), and the material can be made fireproof by adding additional additives.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of chemical building materials, and in particular to a honeycomb resin material and a preparation method thereof. Background Art

[0002] Water-based resin is a new type of resin system that uses water instead of organic solvents as a dispersion medium. It includes three categories: water-soluble polymers, highly absorbent resins and water-based coatings. It is widely used in many fields such as building decoration, industrial coatings, water treatment, food and daily chemicals. However, water-based resins are mainly used as floor paints or adhesives in the field of building decoration, and their use scenarios are limited. Its processing technology needs to be expanded, such as making it into three-dimensional porous materials or honeycomb materials. At present, the manufacturing cost of honeycomb panels in engineering is high, the specific strength is low, and it is impossible to achieve true light weight and high strength. Scientific research shows that at the same density, the smaller the honeycomb pore size, the higher the strength and modulus, and the better the thermal insulation performance. Oriented freezing is a technology for preparing anisotropic honeycomb materials with micron pores. This technology usually uses water as a solvent. Under a directional temperature field, the micron ice crystals solidified by water will squeeze the solute. When the ice crystals are removed, the micron pores formed by the solute are retained. However, oriented freezing technology usually relies on freeze-drying, which has the disadvantages of high economic cost and time-consuming and energy-consuming. In addition, the size of the sample is affected by the size of the machine and requires a closed production environment. It is difficult to achieve continuous, low-cost, and large-scale production, and can only be produced and applied in high value-added industries (such as the food and pharmaceutical industries).

[0003] At present, there is a report in the prior art that a thickener, a cross-linking agent, a catalyst and water are mixed to obtain a mixed sol, the mixed sol and an aqueous resin are mixed and then oriented and frozen, then in situ cross-linked in a low temperature environment, and then solvent replacement is performed in a poor solvent, and the block material finally obtained is solidified or dried to obtain a honeycomb resin material. The preparation method is simple, the conditions are mild, and the honeycomb resin material can be prepared by drying at normal pressure, and the whole process is in an open system. However, this method requires an external cross-linking agent to cross-link the aqueous resin and the thickener, and the cross-linking agent is a metal ion, which cannot react completely and will cause pollution. In addition, the yield strength of the obtained material is low and needs to be further improved. Summary of the invention

[0004] In view of this, the object of the present invention is to provide a honeycomb resin material and a preparation method thereof. The preparation method provided by the present invention is simple, green and environmentally friendly, saves energy consumption, and the obtained resin material has adjustable density, excellent mechanical properties, and high yield strength.

[0005] To achieve this object, the present invention adopts the following technical solutions:

[0006] In a first aspect, the present invention provides a honeycomb resin material, which is obtained by orienting and freezing a mixture of an aqueous resin, a curing agent and water, followed by in-situ crosslinking and heat treatment in a low temperature environment.

[0007] Preferably, the maximum yield strength of the honeycomb resin material is greater than 20 MPa, and the maximum elastic modulus is greater than 500 MPa.

[0008] Preferably, the honeycomb resin material is obtained by orienting and freezing a mixture of a water-based resin, a curing agent, an additive and water, followed by in-situ crosslinking and heat treatment in a low-temperature environment.

[0009] Preferably, the additive includes any one or more of calcium silicate nanofibers, carbon nanotubes, cellulose nanofibers, glass microbeads, silicon oxide, ammonium polyphosphate or low-melting-point glass powder.

[0010] In a second aspect, the present invention provides a method for preparing the honeycomb resin material, comprising the following steps:

[0011] (1) mixing a water-based resin, a curing agent, optional additives and water to obtain a dispersion;

[0012] (2) Orienting and freezing the dispersion to obtain a frozen block;

[0013] (3) The frozen block material is cross-linked in situ in a low temperature environment and then heat treated to obtain a honeycomb resin material.

[0014] Preferably, the mass ratio of the water-based resin, curing agent, additive and water is 1.5:(0.5-2):(0.01-1):(0.5-8).

[0015] Preferably, the water-based resin includes any one or more of water-based epoxy resin, melamine ester, phenolic resin or polyurethane.

[0016] Preferably, the curing agent includes any one or more of a modified amine waterborne epoxy curing agent, a polyether-modified isocyanate-based polyurethane curing agent or a modified ester curing agent.

[0017] Preferably, the temperature of the orientation freezing is -50 to -10°C, and the time of the orientation freezing is 10 to 20 minutes.

[0018] Preferably, the in-situ crosslinking is specifically: performing in-situ crosslinking in a low temperature environment of -20 to -5°C for 24 to 72 hours.

[0019] Preferably, the heat treatment is specifically: placing the in-situ cross-linked block material into a hot water bath for treatment for 1 to 24 hours, and the temperature of the hot water bath is 40 to 100°C.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] (1) The preparation method provided in the present application is green and environmentally friendly, has a simple process, mild conditions, saves energy, and uses low-priced raw materials, which can effectively reduce production costs and facilitate large-scale production;

[0022] (2) The waterborne epoxy resin honeycomb material prepared by the preparation method provided in this application has an adjustable density (150-660 mg / cm 3 ), compared with the honeycomb material obtained by the prior art (the maximum yield strength does not exceed 5MPa, the maximum elastic modulus does not exceed 100MPa), its mechanical properties are more excellent (maximum yield strength>20MPa, maximum elastic modulus>500MPa), and additional additives can be used to make the material have fire resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a cross-sectional SEM image of the waterborne epoxy resin honeycomb material obtained in Example 1;

[0024] Figure 2 This is a longitudinal cross-sectional SEM image of the waterborne epoxy resin honeycomb material obtained in Example 1;

[0025] Figure 3 This is an axial compressive stress-strain curve of the waterborne epoxy resin honeycomb material obtained in Example 1;

[0026] Figure 4 This is a finished product picture of the waterborne epoxy resin honeycomb material obtained in Example 1 after processing;

[0027] Figure 5 This is an axial compressive stress-strain curve of the waterborne epoxy resin honeycomb material obtained in Example 2;

[0028] Figure 6 This is a comparison chart of the waterborne epoxy resin honeycomb materials obtained in Example 1 and Example 3 after combustion. DETAILED DESCRIPTION

[0029] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] The sources of all raw materials involved in the present invention are not particularly limited and can be purchased from the market or prepared according to conventional preparation methods well known to those skilled in the art.

[0031] The present invention provides a honeycomb resin material, which is preferably obtained by orienting and freezing a mixture of a water-based resin, a curing agent and water, and then in-situ crosslinking and heat treatment in a low-temperature environment.

[0032] The honeycomb resin material has honeycomb holes, an adjustable density, and excellent mechanical properties, with a maximum yield strength greater than 20 MPa and a maximum elastic modulus greater than 500 MPa. In the present invention, the honeycomb resin material may be further added with additives during the preparation process, so as to have fireproof properties. The additives preferably include any one or more of calcium silicate nanofibers, carbon nanotubes, cellulose nanofibers, glass microbeads, silicon oxide, ammonium polyphosphate, or low-melting-point glass powder.

[0033] The present invention also provides a method for preparing the honeycomb resin material, comprising the following steps:

[0034] (1) mixing a water-based resin, a curing agent, optional additives and water to obtain a dispersion;

[0035] (2) Orienting and freezing the dispersion to obtain a frozen block;

[0036] (3) The frozen block material is cross-linked in situ in a low temperature environment and then heat treated to obtain a honeycomb resin material.

[0037] According to the present invention, first water-based resin, curing agent, optional additive and water are mixed to obtain dispersion. In this process, it is only the process of mixing water-based resin, curing agent, optional additive and water to obtain uniform dispersion. More specifically, water-based resin and curing agent and optional additive can be mixed first, then water is added, and dispersion can be obtained by sufficient stirring. In the present invention, the water-based resin preferably includes any one or more of water-based epoxy resin, melamine ester, phenolic resin or polyurethane, and the curing agent is used to cross-link with the water-based resin to form a cross-linked network, preferably including any one or more of modified amine water-based epoxy curing agent, polyether-modified isocyanate polyurethane curing agent or modified ester curing agent. It should be noted that water-based resin needs to be used in combination with supporting curing agent, such as epoxy resin and modified amine water-based epoxy curing agent, polyurethane and polyether-modified isocyanate polyurethane curing agent are used in combination, etc. In the present invention, the mass ratio of the water-based resin, curing agent, optional additives and water is preferably 1.5:(0.5-2):(0.01-1):(0.5-8), and more preferably 1.5:(1-2):(0.01-1):(0.5-5). It should be noted that in certain embodiments of the present invention, no additives are added, and in this case, the mass ratio of the water-based resin, curing agent, and water is preferably 1.5:(0.5-2):(0.5-8), and more preferably 1.5:(1-2):(0.5-5).

[0038] The present invention then performs orientation freezing on the dispersion to obtain a block material. The orientation freezing is a conventional technical means well known to those skilled in the art, specifically immersing the metal platform in a liquid nitrogen environment, and a thermocouple is connected to the surface of the metal platform. The temperature of the surface of the metal platform is regulated by controlling the amount of liquid nitrogen added. This method can control the error of the surface temperature of the metal platform within 3°C. In the present invention, the size and shape of the prepared honeycomb resin material are controlled by molds of different sizes and shapes, and the material of the mold preferably includes any one of silica gel, polydimethylsiloxane or polytetrafluoroethylene. More specifically, the present invention preferably places the metal platform in a container, adds liquid nitrogen to control the surface of the metal platform at the desired temperature, puts on the mold, and then pours the dispersion into it, waits for the dispersion to agglomerate, and obtains a block material. In a specific embodiment, the temperature of the orientation freezing is preferably -50 to -10°C, more preferably -20 to -10°C, and the time of the orientation freezing is preferably 10 to 20 minutes, more preferably 15 to 20 minutes.

[0039] After orientation freezing, the present invention then places the block material in a low temperature environment for in-situ crosslinking. In this process, the water-based resin and the curing agent of the block material are initially crosslinked in the low temperature environment to form an in-situ crosslinked network to avoid the instability and decomposition of the water-based resin during the heat treatment process. The temperature of the low temperature environment is sufficient to ensure that the block material does not melt. In a specific embodiment, the temperature of the low temperature environment is preferably -20 to -5°C, more preferably -20 to -10°C, and the time of the in-situ crosslinking is 24 to 72 hours, more preferably 48 to 72 hours.

[0040] After the frozen block material is cross-linked in situ, the block material is subjected to heat treatment, during which the heat treatment is used to decompose the ice crystals in the block material to obtain a honeycomb resin material. In a specific embodiment, the heat treatment is preferably performed in a hot water bath, and the temperature of the hot water bath is sufficient to ensure that the ice crystals can be dissolved. In a specific embodiment, the temperature of the hot water bath is preferably 40 to 100°C, more preferably 60 to 100°C, and the time of the hot water bath is preferably 1 to 24 hours, more preferably 10 to 24 hours.

[0041] Compared with the prior art, the preparation method of the present invention does not need to add thickener, has no metal ion pollution, is green and environmentally friendly, has a simple process (no freeze dryer and protective atmosphere are required), mild conditions (normal pressure open system), saves energy consumption, and the raw materials used are cheap, which can effectively reduce production costs and facilitate large-scale production. The mechanical properties of the prepared material are excellent (maximum yield strength is greater than 20MPa, and maximum elastic modulus is greater than 500MPa), which is much higher than the honeycomb material provided by the prior art (maximum yield strength does not exceed 5MPa, and maximum elastic modulus does not exceed 100MPa). At the same time, the prepared water-based epoxy resin honeycomb material can be adjusted by adjusting the parameters in the orientation freezing process, so that the density and mechanical strength of the material can be adjusted to meet the needs of different working scenarios. In addition, the material can also be made fireproof by introducing additional additives.

[0042] To further illustrate the present invention, the following examples are used to provide a detailed description. The water-based epoxy resin used in the following examples of the present invention is a general commercial product, which can be purchased from Shandong Ruisan Chemical Technology Co., Ltd., model WE-8217; the curing agent is a modified water-based amine curing agent used in conjunction with the water-based epoxy resin, purchased from Shandong Ruisan Chemical Technology Co., Ltd., model 247. The remaining experimental raw materials, unless otherwise specified, can be purchased from the market or prepared according to conventional preparation methods well known to those skilled in the art.

[0043] Example 1

[0044] This embodiment provides a waterborne epoxy resin honeycomb material, and the preparation method thereof is as follows:

[0045] Mix 6g of waterborne epoxy resin and 4g of curing agent, stir evenly, then slowly add 8g of water, stir thoroughly to obtain a light yellow emulsion with high viscosity;

[0046] Place the metal platform connected to the thermocouple in a plastic foam container, pour liquid nitrogen into the plastic foam container, and control the amount of liquid nitrogen poured to stabilize the temperature of the metal platform at -20°C; cut a small block with a bottom of about 1.5cm*1.5cm from the middle of a 1.5cm thick silica gel plate as a template and place it on the surface of the low-temperature copper block platform; pour the light yellow emulsion obtained above into the template, and control the temperature of the metal platform to stabilize at about -20°C by adding liquid nitrogen. After 20 minutes, all the samples are frozen. Store the sample in a -15°C refrigerator for three days, then heat it in 50°C water for 12 hours, take out the sample, and dry it to obtain a water-based epoxy resin honeycomb material.

[0047] The cross-section and longitudinal sections of the waterborne epoxy resin honeycomb material were observed using a scanning electron microscope. Figures 1-2 As shown, Figure 1 This is a cross-sectional SEM image of a waterborne epoxy resin honeycomb material. It can be seen that the material has a honeycomb pore structure. Figure 2 This is the longitudinal section of the water-based epoxy resin honeycomb material, and the SEM image of the oriented pore structure of the material can be seen.

[0048] The waterborne epoxy resin honeycomb material was subjected to mechanical testing using an Instron 5565A universal testing machine at a compression rate of 2 mm / min. The test showed that the waterborne epoxy resin honeycomb material had excellent mechanical strength and a density of 473 mg / cm 3 The compressive yield strength in the orientation direction is 16.0MPa and the elastic modulus is 490MPa. The axial compressive stress-strain curve of the material is shown in Figure 3 shown.

[0049] The obtained waterborne epoxy honeycomb material can be processed using commercial wood carving tools to obtain customized shapes, such as Figure 4 shown.

[0050] Example 2

[0051] This embodiment provides a waterborne epoxy resin honeycomb material, and the preparation method thereof is as follows:

[0052] 6 g of waterborne epoxy resin and 4 g of curing agent were mixed and stirred evenly, and then 8 g of water (containing 1 wt % xonotlite nanofibers) was slowly added dropwise and stirred thoroughly to obtain a light yellow emulsion with high viscosity;

[0053] Place the metal platform connected to the thermocouple in a plastic foam container, pour liquid nitrogen into the plastic foam container, and control the amount of liquid nitrogen poured to stabilize the temperature of the metal platform at -20°C; cut a small block with a bottom of about 1.5cm*1.5cm from the middle of a 1.5cm thick silica gel plate as a template and place it on the surface of the low-temperature copper block platform; pour the light yellow emulsion obtained above into the template, and control the temperature of the metal platform to stabilize at about -20°C by adding liquid nitrogen. After 20 minutes, all the samples are frozen. Store the sample in a -15°C refrigerator for three days, then heat it in 50°C water for 12 hours, take out the sample, and dry it to obtain a water-based epoxy resin honeycomb material.

[0054] Scanning electron microscope observation showed that the obtained waterborne epoxy resin honeycomb material also had a honeycomb pore structure and an oriented pore structure.

[0055] Referring to the above mechanical test method, it was determined that the density of the waterborne epoxy resin honeycomb material was 435 mg / cm 3 The compressive yield strength in the orientation direction is 18.3MPa and the elastic modulus is 520MPa. The axial compressive stress-strain curve of the material is shown in Figure 5 shown.

[0056] Example 3

[0057] This embodiment provides a waterborne epoxy resin honeycomb material, and the preparation method thereof is as follows:

[0058] 6 g of waterborne epoxy resin, 4 g of curing agent, 0.066 g of ammonium polyphosphate and 0.66 g of low-melting-point glass powder were mixed and stirred evenly, and then 8 g of water was slowly added dropwise and stirred thoroughly to obtain a light yellow emulsion with high viscosity.

[0059] Place the metal platform connected to the thermocouple in a plastic foam container, pour liquid nitrogen into the plastic foam container, and control the amount of liquid nitrogen poured to stabilize the temperature of the metal platform at -20°C; cut a small block with a bottom of about 1.5cm*1.5cm from the middle of a 1.5cm thick silica gel plate as a template and place it on the surface of the low-temperature copper block platform; pour the light yellow emulsion obtained above into the template, and control the temperature of the metal platform to stabilize at about -20°C by adding liquid nitrogen. After 20 minutes, all the samples are frozen. Store the sample in a -15°C refrigerator for three days, then heat it in 50°C water for 12 hours, take out the sample, and dry it to obtain a water-based epoxy resin honeycomb material.

[0060] Scanning electron microscope observation showed that the obtained waterborne epoxy resin honeycomb material also had a honeycomb pore structure and an oriented pore structure.

[0061] Combustion experiments were carried out on the materials obtained in Example 1 and Example 3. The results are as follows: Figure 6As shown, it can be seen that by adding additives during the preparation process, the prepared water-based epoxy resin honeycomb material can have fire-retardant properties.

[0062] In addition, the present application also refers to the above-mentioned preparation method, and obtains different waterborne epoxy resin honeycomb materials by adjusting the mass of waterborne epoxy resin, curing agent and water, and the corresponding physical properties thereof are shown in Table 1 below:

[0063] Table 1

[0064]

[0065]

[0066] From the data in Table 1 above, it can be seen that the density of the honeycomb resin material provided by the present application is adjustable, and when the amount of water added is large, the yield strength of the obtained material decreases, but the thermal conductivity is low, and it can be used as a thermal insulation material. Therefore, according to the actual application needs, a honeycomb resin material with specific excellent properties can be obtained by adjusting the mass of water-based epoxy resin, curing agent and water.

[0067] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A honeycomb resin material, characterized in that: The mixture of water-based resin, curing agent and water is frozen after orientation, and then cross-linked in situ and heat-treated in a low-temperature environment; The heat treatment specifically comprises: placing the in-situ cross-linked block material in a hot water bath for 1 to 24 hours; The maximum yield strength of the honeycomb resin material is greater than 20 MPa, and the maximum elastic modulus is greater than 500 MPa.

2. The honeycomb resin material according to claim 1, characterized in that: The composite material is obtained by orienting and freezing a mixture of water-based resin, curing agent, additives and water, and then in-situ crosslinking and heat treatment in a low-temperature environment.

3. The honeycomb resin material according to claim 2, characterized in that: The additives include any one or more of calcium silicate nanofibers, carbon nanotubes, cellulose nanofibers, glass microbeads, silicon oxide, ammonium polyphosphate or low-melting-point glass powder.

4. The method for preparing a honeycomb resin material according to any one of claims 1 to 3, characterized in that: The following steps are involved: (1) mixing a water-based resin, a curing agent, optional additives and water to obtain a dispersion; (2) Orienting and freezing the dispersion to obtain a frozen block; (3) The frozen block material is cross-linked in situ in a low temperature environment and then heat treated to obtain a honeycomb resin material.

5. The preparation method according to claim 4, characterized in that: The mass ratio of the water-based resin, curing agent, additive and water is 1.5:(0.5-2):(0.01-1):(0.5-8).

6. The preparation method according to claim 4, characterized in that: The water-based resin includes any one or more of water-based epoxy resin, melamine ester, phenolic resin or polyurethane; The curing agent includes any one or more of a modified amine waterborne epoxy curing agent, a polyether-modified isocyanate-based polyurethane curing agent or a modified ester curing agent.

7. The preparation method according to claim 4, characterized in that: The temperature of the orientation freezing is -50 to -10°C, and the time of the orientation freezing is 10 to 20 minutes.

8. The preparation method according to claim 4, characterized in that: The in-situ crosslinking is specifically: performing in-situ crosslinking in a low temperature environment of -20 to -5°C for 24 to 72 hours.