Negative photosensitive resin composition, patterning method and use thereof

By using a specific formula of negative photosensitive resin composition and process steps, the problem of inconsistent morphology and insufficient photosensitive sensitivity under different wavelength exposures is solved, and the stability and cost improvement is achieved, and it is suitable for semiconductors. Metal patterning in manufacturing.

CN115524923BActive Publication Date: 2024-11-19SHENZHEN RONGDA PHOTOSENSITIVE & TECH CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202211143011.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-20
Publication Date
2024-11-19
Estimated Expiration
2042-09-20

AI Technical Summary

Technical Problem

Existing negative photoresist is difficult to maintain the consistent inverted trapezoidal morphology under different wavelength exposures, resulting in poor stability, and the life of the baking hot plates dropped rapidly after high frequency use, which is high cost, and insufficient photosensitive sensitivity, making it difficult to achieve accurate Metal patterning.

Method used

采用包含不同分子量酚醛清漆树脂、光致产酸剂、光稳定剂、交联剂、溶剂、碱性化合物和其他添加剂的负性感光性树脂组合物,通过特定的配方比例和工艺步骤形成光刻胶膜层,并在不同温度下进行预烘烤、曝光和显影处理。

Benefits of technology

A similar inverted trapezoidal morphology is achieved under different wavelengths of light, which improves the stability and photosensitive sensitivity of the photoresist, maintains a good film retention rate, reduces costs, and extends the service life of the hot plate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure BDA0003854462660000041
    Figure BDA0003854462660000041
  • Figure BDA0003854462660000081
    Figure BDA0003854462660000081
Patent Text Reader

Abstract

The present invention relates to a negative photosensitive resin composition, which comprises the following components: (A) an alkali-soluble resin, which comprises at least two novolac resins with different molecular weights, 100 parts by weight; (B) a photoacid generator, 0.1-5, preferably 0.5-4, more preferably 0.5-3.5 parts by weight; (C) a light stabilizer, 0.1-20, preferably 0.5-10; (D) a crosslinking agent, 1-45, preferably 2-35, more preferably 3-30 parts by weight; ( E) solvent, 100-600, preferably 110-550, more preferably 120-500 parts by weight; (F) alkaline compound, 0.2-2, preferably 0.3-1.8, more preferably 0.4-1.6 parts by weight; and (G) optionally additives, 0.01-20, preferably 0.1-15 parts by weight, more preferably 0.1-10 parts by weight; wherein the amount of component (B)-(G) is based on 100 parts by weight of alkali-soluble resin (A). It also relates to a method for using the resin composition to pattern photoresist and the use of a negative photosensitive resin composition for metal patterning in semiconductor preparation. The resin composition can adapt to different exposure wavelengths, and can control the undercut morphology after photoresist development by controlling the exposure amount.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of photoresists, and more specifically to a negative photosensitive resin composition, a patterning method thereof and a use thereof. Background Art

[0002] In recent years, with the development of semiconductor manufacturing, Mini LED and Micro LED display panel manufacturing, the demand for reducing the size of core particles has become increasingly high. Therefore, the lines of the metal electrode pattern are required to be more and more dense and the line width is required to be smaller and smaller. Generally speaking, in semiconductor manufacturing, the metal electrode pattern can be prepared using wet etching and lift-off process. In the prior art, for the lift-off process using negative photoresist, it is difficult to maintain the same inverted trapezoidal morphology (referring to the inverted trapezoidal shape of the space stripped out) under exposure rays of different wavelengths such as g-line (436nm) and i-line (365nm), so the stability is poor; or when a higher post-exposure baking temperature is used for a long time and at a high frequency, the expected service life of the baking hot plate will drop rapidly, making the cost of the photolithography process higher. It will also cause the warping of the hot plate to be more serious, thereby increasing the difference in heat exposure between the center and edge of the wafer, and further improving the temperature sensitivity requirements of the negative photoresist composition.

[0003] In addition, when a conventional negative photoresist composition is used to form a metal pattern, the absorption of the entire photoresist for single wavelength exposure of g-line, h-line and i-line is different, so it is impossible to maintain a stable inverted trapezoidal morphology or accurately control the line width size after development. Therefore, when a target metal film is formed on a photoresist pattern, under different single wavelength exposure conditions, the size after development will have a large deviation from the design size, resulting in failure to meet the technical requirements of the process. In addition, different exposure wavelengths have different effects on the sidewall morphology of the photoresist after development, and the sidewall morphology of the photoresist will directly affect the sidewall angle of the final deposited metal, and even residues of the target metal film will appear or accumulate on the sidewall of the photoresist. These residues will cause short circuits between the electrodes formed by the metal film, and ultimately form defective devices, resulting in a decrease in product yield.

[0004] Conventional negative photoresist compositions do not have sufficiently high photosensitivity when the film layer is thin, so it is difficult to achieve effective and good patterning of the target film, and the film retention rate after development is poor. Summary of the invention

[0005] In order to overcome the above deficiencies in the prior art, the present invention provides a negative photosensitive resin composition, which comprises:

[0006] (A) an alkali-soluble resin comprising at least two novolac resins having different molecular weights, 100 parts by weight;

[0007] (B) a photoacid generator, 0.1-5 parts by weight, preferably 0.5-4 parts by weight, more preferably 0.5-3.5 parts by weight;

[0008] (C) light stabilizer, 0.1-20 parts by weight, preferably 0.5 to 10 parts by weight;

[0009] (D) a cross-linking agent, 1-45 parts by weight, preferably 2-35 parts by weight, more preferably 3-30 parts by weight;

[0010] (E) solvent, 100-600 parts by weight, preferably 110-550 parts by weight, more preferably 120-500 parts by weight;

[0011] (F) a basic compound, 0.2-2 parts by weight, preferably 0.3-1.8 parts by weight, more preferably 0.4-1.6 parts by weight; and

[0012] (G) optionally other additives, 0.01-20 parts by weight; preferably 0.1-15 parts by weight, more preferably 0.1-10 parts by weight;

[0013] The amounts of components (B) to (G) are all based on 100 parts by weight of the alkali-soluble resin (A).

[0014] On the other hand, the present invention also provides a method for forming a pattern of a photoresist, which comprises the following steps:

[0015] (i) uniformly coating the negative photosensitive resin composition of the present invention on a substrate to form a photoresist film layer,

[0016] (ii) pre-baking the photoresist film obtained in (i) at a temperature of 80 to 130° C., preferably using a hot plate, and the thickness of the photoresist after baking is 0.5 to 15 μm,

[0017] (iii) partially irradiating the photoresist film layer formed in (ii) through a mask with radiation,

[0018] (iv) post-exposure baking the film after exposure in (iii) at a temperature of 90 to 130° C., preferably using a hot plate,

[0019] (v) The photoresist film obtained in (iv) is developed using a developer.

[0020] On the other hand, the present invention also provides the use of photoresist for metal patterning in semiconductor preparation.

[0021] Advantageously, during photolithography using the negative photosensitive resin composition of the present invention, light with different wavelengths can be used for exposure, and the inverted trapezoidal morphologies formed are similar and have good stability, so as to facilitate matching with mercury lamps of different wavelengths.

[0022] The negative photosensitive resin composition of the present invention has sufficient photosensitivity even when the photoresist film is relatively thin, and can also maintain a good film retention rate. DETAILED DESCRIPTION

[0023] In the present invention, unless otherwise stated, all operations are carried out at room temperature and normal pressure.

[0024] In the present invention, unless otherwise specified, the term "alkali soluble resin" is used synonymously with "solid content of alkali water soluble resin". This is because in use, "alkali soluble resin" usually contains a solvent component (such as for reducing viscosity and easy operation), however, when it comes to calculating material ratios, determining acid values, etc., usually only the components without solvent are considered, which is well known to those skilled in the art.

[0025] As used herein, the term "undercut" refers to the process of preparing semiconductor photolithography. When the photoresist is developed after exposure, the photoresist at the bottom layer of the photoresist absorbs less light during the exposure process and is not completely cured. Therefore, the dissolution rate of the photoresist at the bottom layer during development is greater than the dissolution rate of the photoresist at the upper layer, so an undercut structure is formed at the lower edge of the photoresist. In the present invention, the undercut structure is an inverted trapezoidal structure, and the edge is not a straight line. The width of the undercut window is the depth of the photoresist close to the substrate being dissolved compared to the vertical surface of the upper photoresist.

[0026] As used herein, the term "inverted trapezoid" means that after the photoresist is developed, the cross-sectional shape of the photoresist portion that is not dissolved by the developer is perpendicular to the line groove direction, that is, an inverted trapezoid with a short lower base and a long upper base.

[0027] As used herein, "line groove" refers to the gap left after the non-irradiated part of the photoresist is dissolved by the developer after development.

[0028] In the present invention, unless otherwise specified, the terms used have the meanings understood by those of ordinary skill in the art.

[0029] In one aspect, the present invention provides a photosensitive resin composition comprising the following components:

[0030] (A) an alkali-soluble resin comprising at least two novolac resins having different molecular weights, 100 parts by weight;

[0031] (B) a photoacid generator, 0.1-5 parts by weight, preferably 0.5-4 parts by weight, more preferably 0.5-3.5 parts by weight;

[0032] (C) light stabilizer, 0.1-20 parts by weight, preferably 0.5 to 10 parts by weight;

[0033] (D) a cross-linking agent, 1-45 parts by weight, preferably 2-35 parts by weight, more preferably 3-30 parts by weight;

[0034] (E) solvent, 100-600 parts by weight, preferably 110-550 parts by weight, more preferably 120-500 parts by weight;

[0035] (F) a basic compound, 0.2-2 parts by weight, preferably 0.3-1.8 parts by weight, more preferably 0.4-1.6 parts by weight; and

[0036] (G) optional additives, 0.01-20 parts by weight; preferably 0.1-15 parts by weight, more preferably 0.1-10 parts by weight;

[0037] The components (B) to (G) are all based on 100 parts by weight of the alkali-soluble resin (A).

[0038] In a preferred embodiment of the present invention,

[0039] Alkali soluble resin (A)

[0040] The alkali-soluble resin (A) includes a novolac resin (A-1) and other novolac resins (A-2). More specifically, the novolac-based polymer may be a copolymer represented by formula (1), and the novolac resin (A-1) and other novolac resins (A-2) are described in detail below:

[0041]

[0042] Wherein m and n represent the degree of polymerization of each repeating unit, wherein m:n=1:9 to 9:1

[0043] Novolac resin (A-1)

[0044] The preparation method of the novolac resin (A-1) is not particularly limited. All methods that can obtain the novolac resin (A-1) having the target weight average molecular weight and molecular weight distribution can be used. Among them, it is preferably obtained by the condensation reaction of a phenolic compound and an aldehyde compound.

[0045] In the present invention, the phenolic compound used to prepare the novolac resin (A-1) can be phenol; methylphenols such as o-cresol, m-cresol, p-cresol; dimethylphenols such as 2,3-xylenol, 2,5-xylenol, 3,5-xylenol, 3,4-xylenol; other alkylphenols such as m-ethylphenol, p-ethylphenol, o-ethylphenol, o-butylphenol, m-butylphenol, p-butylphenol, 2,3,5-trimethylphenol, 2, 3,5-triethylphenol; alkoxyphenols such as p-methoxyphenol, m-methoxyphenol, p-ethoxyphenol, m-ethoxyphenol, p-propoxyphenol; isopropenylphenols such as o-isopropenylphenol, p-isopropenylphenol, 2-methyl-4-isopropenylphenol; arylphenols such as phenylphenol, α-naphthol, β-naphthol; polyhydroxyphenols such as bisphenol A, m-quinone, p-quinone, and the above compounds can be used alone or in combination.

[0046] In the present invention, the aldehyde compound used to prepare the novolac resin (A-1) can be formaldehyde, paraformaldehyde, trioxymethylene, acetaldehyde, triacetaldehyde, propionaldehyde, butyraldehyde, trimethylacetaldehyde, acrolein, crotonaldehyde, cyclohexanal, benzaldehyde, furanaldehyde, furanyl acrolein, terephthalaldehyde, phenylacetaldehyde, α-phenylpropionaldehyde, β-phenylpropionaldehyde, o-hydroxybenzaldehyde, m-hydroxybenzaldehyde, p-hydroxybenzaldehyde, o-methylbenzaldehyde, m-methylbenzaldehyde, p-methylbenzaldehyde, o-chlorobenzaldehyde, m-chlorobenzaldehyde, p-chlorobenzaldehyde, and cinnamaldehyde.

[0047] In the present invention, the molar ratio of the phenolic compound to the aldehyde compound used to prepare the novolac resin (A-1) is 0.33 to 1.00, preferably 0.35 to 1.00, and more preferably 0.6 to 1.0. When the molar ratio of phenolic compounds to aldehyde compounds is less than 0.33, the yield of the phenolic resin composition that may be prepared may be greatly reduced, and when the molar ratio is greater than 1.00, a phenolic resin composition with a wide molecular weight distribution may be obtained, thereby failing to obtain the target novolac resin (A-1) with a desired molecular weight distribution. Specifically, when the molar ratio of the phenolic compound to the aldehyde compound is 0.6 to 1.0, the total content of dimers of phenols contained in the novolac resin (A-1) is determined by gel permeation chromatography (GPC) according to GB / T 7193-2008 using polystyrene as a standard curve to be 15 wt% or less, more preferably 10 wt% or less, and the dispersity (weight average molecular weight Mw / number average molecular weight Mn) in this case is 1.0 to 8.0, more preferably 3.0 to 7.0. In addition, the weight average molecular weight of the novolac resin (A-1) is preferably 1,000 to 100,000, more preferably 1,500 to 50,000, and most preferably 4,000 to 8,000.

[0048] In the present invention, the acid catalyst used to prepare the novolac resin (A-1) may be phosphoric acid or other acids, which play a key role in the phase separation reaction between phenols and aldehydes. The phosphoric acid catalyst may be polyphosphoric acids such as metaphosphoric acid, pyrophosphoric acid, orthophosphoric acid, triphosphoric acid, tetraphosphoric acid, and phosphoric anhydride, but the present invention is not limited thereto, and the above compounds may be used alone or in combination.

[0049] In the present invention, other acids used to prepare the novolac resin (A-1) may be, for example, hydrochloric acid, sulfuric acid, p-toluenesulfonic acid, carboxylic acid, organic phosphoric acid, etc., but the present invention is not limited thereto, and the above compounds may be used alone or in combination. If the phase separation reaction is promoted, carboxylic acids (carboxylic acids containing hydroxyl groups may include citric acid, tartaric acid, and malic acid; carboxylic acids containing sulfhydryl groups may include thioglycolic acid; carboxylic acids containing amino groups may include aspartic acid, iminodiacetic acid, N,N'-ethylenediaminediacetic acid, and N-hydroxyethylethylenediaminetriacetic acid) and organic phosphoric acids (diethylaminetetramethylenephosphoric acid, ethylenediaminebismethylenephosphoric acid, and aminotrimethylenephosphoric acid) are preferred.

[0050] In the method for producing the novolac resin (A-1) of the present invention, the amount of the acid catalyst is preferably greater than or equal to 5 parts by weight, preferably greater than or equal to 10 parts by weight, based on 100 parts by weight of the total amount of phenols used. When the amount of the acid catalyst is less than 5 parts by weight, the phase separation reaction is difficult to carry out, and the yield will decrease due to the great reduction of the phenol monomer. The molar ratio of phosphoric acid as the acid catalyst to the other acid is preferably 10:90 to 90:10.

[0051] In the present invention, a solvent (also called a solubilizer) that promotes phase separation reaction can be used when preparing the novolac resin (A-1), and the solubilizer is preferably selected from at least one of alcohols, polyol ethers, cyclic ethers, polyol esters, ketones and sulfoxides, or a combination of two or more thereof. Based on 100 parts by weight of the total amount of phenols used, the reaction solubilizer is preferably greater than or equal to 5 parts by weight, more preferably greater than or equal to 10 parts by weight.

[0052] In the method for producing the novolac resin (A-1) of the present invention, in order to improve production efficiency, the water content is preferably less than 40% by weight. In addition, the reaction temperature of phenols and aldehydes is preferably 40° C. to reflux temperature, more preferably 60° C. to reflux temperature, and most preferably reflux temperature. The reaction time should be maintained at 1 hour to 30 hours. In addition, the reaction can be carried out under normal pressure, preferably under pressure or reduced pressure.

[0053] The content of the novolac resin (A-1) is 30 to 100 parts by weight, preferably 35 to 90 parts by weight, and more preferably 40 to 70 parts by weight, based on 100 parts by weight of the total amount of the alkali-soluble resin (A).

[0054] Other phenolic varnish resins (A-2)

[0055] The other novolac resin (A-2) is prepared by a method similar to the preparation method of the novolac resin (A-1), except that the obtained other novolac resin (A-2) has a dispersity of 1.0 to 4.0, preferably 1.5 to 3.0, and a weight average molecular weight of preferably 1,000 to 15,000, more preferably 2,000 to 5,000.

[0056] Based on 100 parts by weight of the total amount of the alkali-soluble resin (A), the content of the other novolac resin (A-2) is 0 to 70 parts by weight, preferably 20 to 70 parts by weight, and more preferably 30 to 60 parts by weight.

[0057] Photoacid generator (B)

[0058] The photoacid generator (B) is a compound that generates an acid after being irradiated with light. In the present invention, the acid generated by the photoacid generator (B) due to light serves as a catalyst for the polymerization reaction between the alkali-soluble resin (A) and the crosslinking agent (D) described below. Specifically, the photoacid generator (B) is, for example, an onium salt compound, a halogen-containing compound, a sulfonic acid compound, a sulfonimide compound, or a combination thereof.

[0059] In the present invention, the onium salt compound used as the photoacid generator (B) may be, for example, an iodonium salt, a sulfonium salt, a phosphonium salt, a diazonium salt, a pyridinium salt or other analogs. Examples of the onium salt compound include diphenyliodonium trifluoromethanesulfonate, diphenyliodonium p-toluenesulfonate, diphenyliodonium hexafluoroantimonate, diphenyliodonium hexafluorophosphate, diphenyliodonium tetrafluoroborate, triphenylcorbium trifluoromethanesulfonate, triphenylcorbium p-toluenesulfonate, triphenylcorbium hexafluoroantimonate or a combination thereof. In addition, the onium salt compound may also be cyclohexylmethyl (2-oxocyclohexyl)corbium trifluoromethanesulfonate, dicyclohexyl (2-oxocyclohexyl)corbium trifluoromethanesulfonate, 2-cyclohexylsulfonylcyclohexanone, dimethyl (2-oxocyclohexyl)corbium trifluoromethanesulfonate, phenyl p-toluenesulfonate or a combination thereof.

[0060] In the present invention, the halogen-containing compound as the photoacid generator (B) may be, for example, tris(2,3-bromopropyl)phosphate, tris(2,3-dibromo-3-chloropropyl)phosphate, 2-[2-(3,4-dimethoxyphenyl)vinyl]-4,6-bis(trichloromethane)-s-triazine, 2-[2-(4-methoxyphenyl-2-yl)vinyl]-4,6-bis(trichloromethane)-s-triazine, 2,4-bis(trichloromethyl)-6-[2-(2-furyl)vinyl]-s-triazine, 2,4-bis(trichloromethyl)-6-[2-(5-methyl-2-furyl)vinyl]-s-triazine, 2,4-bis(trichloromethyl)-6-[2-(5-ethyl-2-furyl)vinyl]-s-triazine, 2,4-bis(trichloromethyl)-6-[2-(5-propyl-2-furyl)vinyl]-s-triazine, 2,4-bis(trichloromethyl)-6-[2-(3,5-dimethoxyphenyl)vinyl]-s-triazine, 2,4-bis(trichloromethyl)-6-[2-(3,5-diethoxyphenyl)vinyl]-s-triazine, 2,4-bis(trichloromethyl)-6-[2-(3,5-dipropoxyphenyl)vinyl]-s-triazine, 2,4-bis(trichloromethyl)-6-[2-(3-methoxy-5-ethoxyphenyl)vinyl]-s-triazine, 2,4-bis(trichloromethyl)-6-[2-(3-methoxy-5-propoxyphenyl)vinyl]-s-triazine, 2,4-bis(trichloromethyl)-6-[2-(3-methoxy-5-propoxyphenyl)vinyl]-s-triazine, 2,4-bis(trichloromethyl) )-6-[2-(3,4-methylenedioxyphenyl)vinyl]-s-triazine, 2,4-bis(trichloromethyl)-6-(3,4-methylenedioxyphenyl)-s-triazine, 2,4-bistrichloromethyl-6-(3-bromo-4-methoxy)phenyl-s-triazine, 2,4-bistrichloromethyl-6-(2-bromo-4-methoxy)phenyl-s-triazine, 2,4-bistrichloromethyl-6-(2-bromo-4-methoxy)phenylphenyl-s-triazine, 2,4-bistrichloromethyl-6-(3-bromo-4-methoxy)phenylphenyl-s-triazine, 2-(4-methoxyphenyl)-4,6-bis(trichloromethyl)-1,3,5-triazine, 2-(4-methoxyphthalyl)-4,6-bis(trichloromethyl)-1,3,5-triazine )-1,3,5-triazine, 2-[2-(2-furyl)vinyl]-4,6-bis(trichloromethyl)-1,3,5-triazine, 2-[2-(5-methyl-2-furyl)vinyl]-4,6-bis(trichloromethyl)-1,3,5-triazine, 2-[2-(3,5-dimethoxyphenyl)vinyl]-4,6-bis(trichloromethyl)-1,3,5-triazine, 2-[2-(3,4-dimethoxyphenyl)vinyl]-4,6-bis(trichloromethyl)-1,3,5-triazine, 2-(3,4-methylenedioxyphenyl)-4,6-bis(trichloromethyl)-1,3,5-triazine, tris(1,3-dibromopropyl)-1,3,5-triazine and tris(2,3-dibromopropyl)-1,3,5-Triazine or a combination of the above compounds,

[0061] In the present invention, the sulfone compound used as the photoacid generator (B) may be, for example, a β-ketosulfone compound, a sulfone compound, or an α-diazo compound of the above compounds. Specific examples of the sulfone compound include 4-trismethoxyphenyl sulfone, 2,4,6-trismethylphenyl sulfone, or a combination of the above compounds.

[0062] In the present invention, the sulfonic acid compound used as the photoacid generator (B) may be, for example, alkyl sulfonates, halogenated alkyl sulfonates, aryl sulfonates, or imino sulfonates. Specific examples of the sulfonic acid compound include benzoin toluene sulfonate, o-nitrophenyl trichloromethane sulfonate, o-nitrobenzene p-toluene sulfonate, or a combination thereof. Specific examples of the sulfonimide compound include N-(trifluoromethylsulfonyloxy)succinimide, N-(trifluoromethylsulfonyloxy)diphenylmaleimide, N-(trifluoromethylsulfonyl)-1,8-naphthalene dicarboximide, or a combination thereof.

[0063] In the present invention, the photoacid generator (B) is preferably 2-[2-(4-methoxyphenyl-2-yl)vinyl]-4,6-bis(trichloromethane)-s-triazine (Formula (2), hereinafter also referred to as B-1), N-(trifluoromethylsulfonyl)-1,8-naphthalene diimide (Formula (3), hereinafter also referred to as B-2) or a combination of the above compounds.

[0064]

[0065] 2-[2-(4-methoxyphenyl-2-yl)vinyl]-4,6-bis(trichloromethane)-s-triazine (B-1)

[0066]

[0067] N-(Trifluoromethylsulfonyl)-1,8-naphthalimide (B-2)

[0068] The photoacid generator (B) can be used alone or in combination. Based on 100 parts by weight of the alkali-soluble resin (A), the amount of the photoacid generator (B) is generally 0.1 to 5 parts by weight, preferably 0.5 to 4 parts by weight, and more preferably 0.5 to 3.5 parts by weight.

[0069] Light stabilizer (C)

[0070] In the present invention, compound (C) is a light stabilizer that can absorb ultraviolet light of a specific wavelength without significantly changing its physical and chemical properties. In the present invention, light stabilizer (C) can strongly absorb ultraviolet light (wavelength of 290 to 435 nm), has good thermal stability, chemical stability and miscibility, and can form a good inverted trapezoidal profile of the photoresist. More specifically, light stabilizer (C) is, for example, salicylate, benzophenone, benzotriazole, substituted acrylonitrile, triazine and hindered amine.

[0071] In the present invention, it is desirable that the light stabilizer can absorb all i, h, and g-lines (wavelength 365 to 435 nm). In the present invention, the salicylate used as the light stabilizer (C) can be, for example, phenyl o-hydroxybenzoate, such as the trade name CHIMASSORB 81 from BASF.

[0072] In the present invention, the benzophenone used as the light stabilizer (C) may be, for example, 2,4-dihydroxybenzophenone, trade name UV-O, manufactured by Shanghai Licheng Chemical Co., Ltd.; 2-hydroxy-4-methoxybenzophenone, trade name UV-9, manufactured by Hefei Tianjian Chemical Co., Ltd.; 2-hydroxy-4-n-octyloxybenzophenone, trade name UV-531, manufactured by Guangzhou Yuanda New Materials Co., Ltd.; 2-hydroxybenzophenone, trade name CHIMASSORB 81, from BASF.

[0073] The benzotriazoles as the light stabilizer (C) may be, for example, 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, trade name UV-P, manufactured by Hefei Tianjian Chemical Co., Ltd., 2-(2'-hydroxy-3'5'-di-tert-phenyl)-5-chlorobenzotriazole, trade name UV-320, manufactured by Hangzhou Xinyang Sanyou Fine Chemical Co., Ltd., trade names TINUVIN 234, TINUVIN 326, TINUVIN 328, TINUVIN 329, TINUVIN 571, TINUVIN P, from BASF.

[0074] The triazines used as the light stabilizer (C) may be, for example, triazine-5, manufactured by Yantai Hengnuo New Materials Co., Ltd.; 2,4-bis(2,4-xylyl)-6-(2-hydroxy-4-n-octyloxyphenyl)-1,3,5-triazine, trade name Chiguard 1064, manufactured by Rhein Chemie, Germany; trade name TINUVIN 1577, manufactured by BASF.

[0075] The hindered amines as the light stabilizer (C) may be, for example, trade names of TINUVINB75 and TINUVIN B97, manufactured by BASF.

[0076] In one embodiment of the present invention, the ketone light stabilizer is preferably (E,E)-1,7-bis(4-hydroxy-3-methoxyphenyl)-1,6-heptadiene-3,5-dione (Formula (4), hereinafter also referred to as C-1).

[0077]

[0078] Formula (4): Bis(4-hydroxy-3-methoxyphenyl)-1,6-heptadiene-3,5-dione (C-1)

[0079] In one embodiment of the present invention, the triazole light stabilizer may be, for example, RUVA-93 (manufactured by Otsuka Chemical Co., Ltd.) (C-2).

[0080] In the present invention, the light stabilizer (C) can be used alone or in combination. Based on 100 parts by weight of the alkali-soluble resin (A), the amount of the light stabilizer (C) is usually 0.1 to 20 parts by weight, preferably 0.5 to 10 parts by weight.

[0081] Crosslinking agent (D)

[0082] In the present invention, the crosslinking agent (D) is a compound that promotes the formation of covalent bonds or ionic bonds between linear novolac resin molecules, and can make the linear novolac resins bond to each other to form a network of high molecular polymers. The acid generated by the above-mentioned photoacid generator (B) after exposure acts as a catalyst, and under the action of heat, catalyzes the reaction of the alkali-soluble resin (A) and the crosslinking agent (D), thereby forming a high molecular polymer with a high degree of crosslinking, so that the photoresist can have a good film retention rate after exposure and development.

[0083] In the present invention, the crosslinking agent (D) is, for example, an alkoxymethylated glycoluril resin or an alkoxymethylated amino resin, an alkyl etherified melamine resin, a benzoguanamine resin, an alkyl etherified benzoguanamine resin, a urea-formaldehyde resin, an alkyl etherified urea-formaldehyde resin, an ethyl formate formaldehyde resin, an epoxy resin, an alkoxymethylated amino resin or a combination thereof, and the preferred crosslinking agent is an alkoxymethylated amino resin.

[0084] Specific examples of alkoxymethylated amino resins include, but are not limited to, methoxymethylated amino resins, ethoxymethylated amino resins, n-propoxymethylated amino resins, or combinations thereof. The crosslinking agent (D) can be used alone or in combination. The amount of the crosslinking agent (D) is generally 1 to 45 parts by weight, preferably 2 to 35 parts by weight, and more preferably 3 to 30 parts by weight, based on 100 parts by weight of the alkali-soluble resin (A).

[0085] When the above-mentioned (D) component is less than 1 weight part, the electroplating resistance, chemical resistance and heat resistance of the obtained film are reduced, but when it exceeds 45 weight parts, it will cause poor development, residual base film or unsatisfactory side wall morphology during development.

[0086] Solvent (E)

[0087] The solvent (E) used in the negative photosensitive resin composition of the present invention is an organic solvent that can dissolve the above components but does not react with the above components.

[0088] In one embodiment of the present invention, the solvent (E) is, for example, alkylene glycol monoalkyl ethers, alkylene glycol monoalkyl acetates, other ethers, ketones, alkyl lactates, aromatic hydrocarbons, amides or combinations thereof.

[0089] Specific examples of the alkylene glycol monoalkyl ethers include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monoethyl ether, diethylene glycol mono-n-propyl ether, diethylene glycol mono-n-butyl ether, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol mono-n-propyl ether, dipropylene glycol mono-n-butyl ether, tripropylene glycol monomethyl ether, tripropylene glycol monoethyl ether or the like, or a combination of the above compounds.

[0090] Specific examples of the alkylene glycol monoalkyl ether acetates include ethylene glycol methyl ether acetate, ethylene glycol ethyl ether acetate, propylene glycol methyl ether acetate, propylene glycol ethyl ether acetate or the like, or a combination of the above compounds.

[0091] Examples of ethers include diethylene glycol dimethyl ether, diethylene glycol methyl ethyl ether, diethylene glycol diethyl ether, tetrahydrofuran or the like, or a combination thereof.

[0092] Examples of ketones include methyl ethyl ketone, cyclohexanone, 2-heptanone, 3-heptanone or the like, or a combination thereof.

[0093] Examples of alkyl lactates include methyl 2-hydroxypropionate, ethyl 2-hydroxypropionate or the like, or a combination thereof.

[0094] -Examples of other esters include methyl 2-hydroxy-2-methylpropionate, ethyl 2-hydroxy-2-methylpropionate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, ethyl ethoxyacetate, ethyl hydroxyacetate, methyl 2-hydroxy-3-methylbutyrate, 3-methyl-3-methoxybutyl acetate, 3-methyl-3-methoxybutyl propionate, ethyl acetate, n-propyl acetate, isopropyl acetate, n-butyl acetate, isobutyl acetate, n-amyl acetate, isoamyl acetate, n-butyl propionate, ethyl butyrate, n-propyl butyrate, isopropyl butyrate, n-butyl butyrate, methyl pyruvate, ethyl pyruvate, n-propyl pyruvate, methyl acetoacetate, ethyl acetoacetate, ethyl 2-oxobutyrate or the like, or a combination thereof.

[0095] - Examples of aromatic hydrocarbons include toluene, xylene or the like, or a combination of the foregoing compounds.

[0096] Examples of amides include N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide or the like, or a combination of the above compounds. The solvent (E) is preferably propylene glycol methyl ether acetate, lactic acid, cyclohexanone, propylene glycol monomethyl ether, N-methylpyrrolidone or a combination of the above solvents. The solvent (E) can be used alone or in combination of multiple types.

[0097] In the present invention, the amount of the solvent (E) used is generally 100 to 600 parts by weight, preferably 110 to 550 parts by weight, and more preferably 120 to 500 parts by weight, based on 100 parts by weight of the alkali-soluble resin (A).

[0098] Basic compounds (F)

[0099] In the present invention, the addition of the alkaline compound can make the photosensitive resin composition of the present invention easy to peel off after exposure and development, that is, the un-irradiated part is easily soluble in the developer and is easier to remove; in addition, the alkaline compound (F) can also better realize the ideal inverted trapezoidal morphology of the negative photoresist; in addition, the alkaline compound (F) can also ensure better side wall smoothness and improve resolution; on the other hand, the alkaline compound (F) also helps to extend the shelf life of the negative photoresist to a certain extent.

[0100] In one embodiment of the present invention, the basic compound (F) is, for example, an aliphatic primary amine, an aliphatic secondary amine, an aliphatic tertiary amine, an amino alcohol, an aromatic amine, a quaternary ammonium hydroxide, an aliphatic amine, or a combination thereof. Specific examples of the basic compound (F) include butylamine, hexylamine, ethanolamine, triethanolamine, 2-ethylhexylamine, 2-ethylhexyloxypropylamine, methoxypropylamine, diethylaminopropylamine, N-toluidine, N-ethylaniline, N-propylaniline, dimethyl-N-toluidine, diethyl-N-toluidine, diisopropyl-N-toluidine, N-methylaminophenol, N-ethylaminophenol, N,N-dimethylaniline, N,N-diethylaniline, N,N-dimethylaminophenol, tripentylamine, tetrabutylammonium hydroxide, tetramethylammonium hydroxide, or a combination thereof. The basic compound (F) is preferably tripentylamine, N-ethylaniline, N,N-dimethylaminophenol, tetramethylammonium hydroxide, diethylaminopropylamine or a combination thereof. The basic compound (F) can be used alone or in combination of multiple compounds.

[0101] The amount of the basic compound (F) used is usually 0.2 to 2 parts by weight, preferably 0.3 to 1.8 parts by weight, and more preferably 0.4 to 1.6 parts by weight, based on 100 parts by weight of the alkali-soluble resin (A) used.

[0102] In one embodiment of the present invention, the weight relationship between the photoacid generator (B) (denoted as m), the alkali-soluble resin (A) (denoted as n) and the crosslinking agent (D) (denoted as q) satisfies the following relationship:

[0103] 0.050≤m / [nq / (n+q)]≤0.300;

[0104] Best

[0105] 0.092≤m / [nq / (n+q)]≤0.250;

[0106] More preferred

[0107] 0.162≤m / [nq / (n+q)]≤0.200;

[0108] Best choice

[0109] 0.166≤m / [nq / (n+q)]≤0.170.

[0110] In one embodiment of the present invention, the weight relationship between the basic compound (F) (denoted as g), the photoacid generator (B) (denoted as m) and the light stabilizer (C) (denoted as h) satisfies the following relationship:

[0111] 0≤g / [mh / (m+h)]≤1.20;

[0112] Best

[0113] 0.28≤g / [mh / (m+h)]≤1.00;

[0114] More preferred

[0115] 0.405≤g / [mh / (m+h)]≤0.85;

[0116] Best choice

[0117] 0.79≤g / [mh / (m+h)]≤0.83.

[0118] In a preferred embodiment of the present invention, the weight relationship between the photoacid generator (B) (denoted as m), the alkali-soluble resin (A) (denoted as n) and the crosslinking agent (D) (denoted as q), and the basic compound (F) (denoted as g), the photoacid generator (B) (denoted as m) and the light stabilizer (C) (denoted as h) satisfies the following relationship at the same time:

[0119] 0.050≤m / [nq / (n+q)]≤0.300, and 0≤g / [mh / (m+h)]≤1.20

[0120] Best

[0121] 0.092≤m / [nq / (n+q)]≤0.250, and 0.28≤g / [mh / (m+h)]≤1.00;

[0122] More preferred

[0123] 0.162≤m / [nq / (n+q)]≤0.200, and 0.405≤g / [mh / (m+h)]≤0.85;

[0124] Best choice

[0125] 0.166≤m / [nq / (n+q)]≤0.170, and 0.79≤g / [mh / (m+h)]≤0.83.

[0126] Additives (G)

[0127] The negative photosensitive resin composition may further contain additives (G), such as surfactants, adhesion promoters or the like.

[0128] The bonding aid is a component that improves the bonding property between the obtained cured film and the substrate. As the bonding aid, a functional silane coupling agent having a reactive functional group such as styrene, methacrylic, methacryloyl, vinyl, isocyanate, ethylene oxide, amino, urea, etc. is preferred.

[0129] Examples of the functional silane coupling agent include vinyl trimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyl trimethoxysilane, 3-glycidyl propyl trimethoxysilane, 3-methacrylonitrile propyl trimethoxysilane, 3-methacrylonitrile propyl triethoxysilane, a hydrolysis condensate of 3-ethoxysilane-N-(1,3-dimethyl-butylene)propylamino, N-phenyl-3-aminopropyl trimethoxysilane, 3-ureidopropyl triethoxysilane, γ-methacryloyloxypropyl trimethoxysilane, vinyl triacetoxysilane, vinyl trimethoxysilane, γ-isocyanate propyl triethoxysilane, γ-glycidoxypropyl trimethoxysilane, and β-(3,4-epoxycyclohexyl)ethyl trimethoxysilane.

[0130] In one embodiment of the present invention, the resin composition of the present invention may contain a bonding aid, which may be used alone or in combination of two or more thereof, in an amount of 0.01 to 20 weight %, preferably 0.1 to 15 weight %, more preferably 0.1 to 10 %, based on the total weight of the resin composition.

[0131] In one embodiment of the present invention, the resin composition of the present invention may contain a bonding aid and a surfactant. In a preferred embodiment of the present invention, the surfactant is selected from organic fluorine-modified surfactants, (poly)siloxane-based surfactants, and other surfactants.

[0132] In a more preferred embodiment of the present invention, the fluorine-based surfactant is preferably a compound having a fluoroalkyl group and / or a fluoroalkylene group at least one of the terminal, main chain and side chain, for example, 1,1,2,2-tetrafluoro-n-octyl (1,1,2,2-tetrafluoro-n-propyl) ether, 1,1,2,2-tetrafluoro-n-octyl (n-hexyl) ether, hexaethylene glycol di(1,1,2,2,3,3-hexafluoro-n-pentyl) ether, octaethylene glycol di(1,1,2,2-tetrafluoro-n-butyl) ether, hexapropylene glycol di(1,1,2,2,2-tetrafluoro-n-butyl) ether, ,3,3-hexafluoro-n-pentyl) ether, octapropylene glycol di(1,1,2,2-tetrafluoro-n-butyl) ether, sodium perfluorododecane sulfonate, 1,1,2,2,3,3-hexafluoro-n-decane, 1,1,2,2,8,8,9,9,10,10-decafluoro-n-dodecane and / or sodium fluoroalkylbenzene sulfonate, sodium fluoroalkyl phosphate, sodium fluoroalkyl carboxylate, diglycerol tetra(fluoroalkyl polyoxyethylene ether), fluoroalkyl ammonium iodide, fluoroalkyl betaine, other fluoroalkyl polyoxyethylene ethers, perfluoroalkyl polyoxyethanol, perfluoroalkyl alkoxylate, carboxylic acid fluoroalkyl ester, etc. Commercially available fluorine-based surfactants include, for example, BM-1000 and BM01100 (available from BM CHEMIE); Megaface F142D, F172, F173, F183, F178, F191, F471 and F476 (available from Dainippon Ink and Chemicals Inc.); Surflon S-112, SC-102, SC-103 and SC104 (available from Asahi Glass); Eftop EF301, EF303 and EF352 (available from Shin-Akita Chemical Co., Ltd.); Ftergent FT-100, FT-110, FT-140A, FT-150, FTX-218 and FTX-251 (available from NEOS).

[0133] In a preferred embodiment of the present invention, commercially available (poly)siloxane surfactants include, for example, Toray silicone DC3PA, DC7PA, SH11PA, SH21PA, SH28PA, SH29PA, DC-57, DC-190 (available from DowCorning Toray Silicone Co., Ltd.); organosiloxane polymer KP341 (available from Xinyue Chemical); BYK-310, 320, 322, 323, 330, 333, 377, 378, 3760 (available from BYK).

[0134] In the present invention, other surfactants that can be used are, for example, ammonium salts and organic amine salts of alkyl diphenyl ether disulfonic acid; ammonium salts and organic amine salts of alkyl diphenyl ether sulfonic acid; ammonium salts and organic amine salts of alkyl benzene sulfonic acid; ammonium salts and organic amine salts of polyoxyethylene alkyl ether sulfate; and ammonium salts and organic amine salts of alkyl sulfate.

[0135] In one embodiment of the present invention, the resin composition of the present invention may contain a surfactant, which may be used alone or in combination of two or more thereof, and the amount of the surfactant is 0.005 to 0.5 wt %; preferably 0.01 to 0.4 wt %, more preferably 0.1 to 0.4 wt %, based on the total weight of the resin composition.

[0136] Another aspect of the present invention provides a method for forming a pattern of a photoresist, comprising the following steps:

[0137] (i) uniformly coating the negative photosensitive resin composition on a substrate to form a photoresist film layer,

[0138] (ii) pre-baking the photoresist film obtained in (i) at a temperature of 80 to 130° C. using a hot plate, wherein the thickness of the photoresist after baking is 0.5 to 15 μm,

[0139] (iii) partially irradiating the photoresist formed in (ii) with radiation through a mask, preferably, the radiation is selected from g-line, h-line, i-line or a combination thereof, preferably g-line, h-line or i-line,

[0140] (iv) performing post-exposure baking on the film after exposure in (iii) at a temperature of 90 to 130° C. using a hot plate,

[0141] (v) The photoresist film obtained in (iv) is developed using a developer.

[0142] In the method for forming a pattern using a photoresist of the present invention, the aforementioned description about the negative photosensitive resin composition is equally applicable and need not be repeated here.

[0143] In one embodiment of the present invention, a coating film is formed on a substrate using the resin composition of the present invention. More specifically, a solution of the resin composition is applied to the surface of the substrate, preferably pre-baked to remove the solvent to form a coating film. Suitable substrates may be glass substrates, silicon substrates, sapphire substrates, silicon carbide substrates, compound semiconductor substrates, and substrates obtained by forming various metal films or oxide films on their surfaces.

[0144] As the coating method, for example, spray coating, roll coating, spin coating, slit coating, bar coating, and inkjet coating can be used. The pre-baking conditions can be adjusted according to the types and usage ratios of the components.

[0145] In a preferred embodiment of the present invention, in step (ii), the coating film in step (i) can be pre-baked by heating. The heating method is not particularly limited, for example, a hot plate can be used to pre-bake the film, the pre-bake temperature is 80° C. to 130° C., and the baking time is 10 seconds to 180 seconds, and a photoresist film layer of 0.5 μm to 15 μm can be obtained. In another embodiment of the present invention, a contact hot plate can also be used for pre-bake.

[0146] In a preferred embodiment of the present invention, in step (iii), a portion of the photosensitive photoresist film in step (ii) is irradiated with radiation. Specifically, the coating film formed in step (ii) is irradiated with radiation through a mask having a specific pattern. Preferably, the radiation is ultraviolet light, for example, g-line (wavelength 436nm), h-line (wavelength 405nm), i-line (wavelength 365nm). Preferably, the radiation contains g-line, h-line and i-line. The exposure amount of the radiation is 0.1J / m 2 Up to 10000J / m 2 .

[0147] In a preferred embodiment of the present invention, in step (iv), the exposed film in step (iii) is subjected to post exposure baking, which can be performed by a hot plate / oven. Generally speaking, the temperature of the hot plate is set at 90° C. to 130° C., and the photoresist film layer is subjected to heating treatment for 10 seconds to 200 seconds. The temperature of the oven is set at 110° C. to 140° C., and the photoresist film layer is subjected to heating treatment for 90 seconds to 1200 seconds to enhance the degree of cross-linking reaction.

[0148] In a preferred embodiment of the present invention, in step (v), the coating film irradiated with radiation in step (iv) is developed. Specifically, the coating film irradiated with radiation in step (iv) is developed with a developer to remove the portion not irradiated with radiation (negative photoresist). Among them, suitable developers that can be used in the present invention are inorganic bases such as sodium hydroxide, potassium hydroxide, sodium carbonate, sodium bicarbonate, sodium silicate, ammonia or the like; primary amines such as ethylamine, n-propylamine or the like, polyamines such as diethylamine, diethylaminoethanol, di-n-propylamine, trimethylamine, triethylamine, methyldiethylamine or the like; dimethylethanolamine, diethylethanolamine, triethanolamine or the like amino alcohols; quaternary ammonium hydroxides such as tetramethylammonium hydroxide (TMAH), tetraethylammonium hydroxide, triethylhydroxymethylammonium hydroxide, trimethylhydroxyethylammonium hydroxide or the like; aqueous solutions of bases (basic compounds) such as pyrrole, piperidine, 1,8-diazabis[5,4,0]-7-undecene, 1,5-diazaoxabicyclo[4,3,0]-5-nonane, etc. Alternatively, an aqueous solution obtained by adding an appropriate amount of a water-soluble organic solvent such as methanol or ethanol and / or a surfactant to the above-mentioned aqueous alkali solution, or an aqueous alkali solution containing a small amount of various organic solvents capable of dissolving the negative photosensitive resin composition of the present invention may be used as a developer.

[0149] In a preferred embodiment of the present invention, suitable developing methods of the present invention are, for example, a spinning immersion method, an immersion method, a shaking immersion method, and a spray method. The developing time in the present invention can be determined according to the dissolution rate of the negative photosensitive resin composition of the present invention in the developer, for example, 30 to 120 seconds.

[0150] In a preferred embodiment of the present invention, after the photoresist is developed, the patterned coating film is preferably cleaned by washing with running water.

[0151] Another aspect of the present invention provides the use of the photoresist of the present invention in preparing light-emitting diode core particles. The photoresist pattern formed by the negative photosensitive resin composition can be used as a mask to form metal electrodes required in the manufacture of light-emitting diode core particles.

[0152] Another aspect of the present invention also provides a method for preparing a light-emitting diode core particle using the photoresist of the present invention. More specifically, a semiconductor epitaxial layer is first formed on a substrate (e.g., a sapphire substrate), including an aluminum nitride buffer layer, a gallium nitride buffer layer, an N-type conductive Si-doped gallium nitride layer, an InGaN / GaN multiple quantum trap, a P-type conductive Mg-doped gallium nitride layer, and an indium tin oxide transparent conductive layer (ITO), in this order from bottom to top.

[0153] Then, a photoresist pattern is formed on the ITO layer by a method of transferring a pattern through photoresist development imaging. In a preferred embodiment of the invention, the pattern after the photoresist exposure and development is an inverted trapezoidal shape that is wide at the top and narrow at the bottom. Then, a metal layer is formed on both sides of the photoresist on the ITO layer by electron beam evaporation (E-beam deposition) or magnetron sputtering (Magnetron sputtering) or other suitable methods, so that the metal layer covers the ITO and the photoresist film layer. The electrode covering the ITO layer is a P electrode, and the electrode covering the n-GaN is an N electrode. The material of the metal layer is, for example, gold, silver, aluminum, copper or other suitable metal materials. Then, a stripping method is used to remove the film layer formed by the negative photosensitive resin composition and the metal pattern formed thereon, leaving only the metal electrode pattern on the ITO film layer and the n-GaN. It is worth noting that in a preferred embodiment of the present invention, since the photoresist pattern is a morphology that is wide at the top and narrow at the bottom, the metal layer covering the ITO layer and the metal layer covering the photoresist pattern are discontinuous, and therefore are easily separated from each other. In another preferred embodiment of the present invention, the photoresist pattern may also be designed to be narrow at the top and wide at the bottom, or to be of equal width at the top and bottom.

[0154] The resin composition of the present invention is used as a photoresist in a metal electrode manufacturing stripping process in, for example, manufacturing a semiconductor element. The semiconductor element can be formed by using a known method. Since the semiconductor element needs to be processed using such materials, it can be preferably used in electronic devices such as display elements, LEDs, and solar thin-film batteries, as well as power devices, charging piles, and other power devices.

[0155] Advantageously, during photolithography using the negative photosensitive resin composition of the present invention, light with different wavelengths can be used for exposure, and the inverted trapezoidal morphologies formed are similar and have good stability, so as to match the mercury lamps of different wavelengths used by customers.

[0156] Advantageously, using the negative photoresist composition of the present invention, large, medium and small coverage of the undercut morphology can be achieved under different exposure amounts at the same exposure wavelength, that is, the undercut morphology can change with the exposure amount, so that the corresponding exposure amount can be selected according to customer needs to control the undercut morphology.

[0157] It should be noted that in this specification, the various features, parameters, conditions and combinations thereof described for the alkali-soluble resin and its composition products and their applications in semiconductor metal patterning are all applicable to their preparation methods and uses.

[0158] The present invention is further illustrated by the following examples, but the present invention is not limited thereto.

[0159] Example

[0160] Preparation Example 1

[0161] In a four-necked flask, a stirring device, a thermometer, an air guide tube, and a reflux condenser are installed, and the flask is placed in a constant temperature oil bath and clamped with an iron stand. Under a nitrogen atmosphere, 129.8g of m-methylphenol (purchased from Shanghai Yanze Chemical Co., Ltd.), 86.5g of p-methylphenol (purchased from Shanghai Yanze Chemical Co., Ltd.), 61.8g of polyformaldehyde (95% purity, mass fraction) (purchased from Shanghai Yanze Chemical Co., Ltd.), and 4g of dihydrate oxalic acid (purchased from Shanghai Yien Chemical Technology Co., Ltd.) are added to the reaction bottle under stirring, and the reaction liquid is heated to 60°C to start the condensation reaction. The temperature is slowly increased for 3 hours until the reaction liquid refluxes. After maintaining at reflux temperature for 6 hours, the reaction liquid is distilled at normal pressure to remove water and solvent. When the reaction liquid reaches 222°C, the system is decompressed by 7 mmHg for distillation to remove the unreacted monomer phenol. The distillation is terminated when the reaction liquid reaches 228°C. The mixture is placed in a stainless steel tank under nitrogen protection and cooled to obtain a yellow transparent solid resin (A-1) with Mw=4500 and Mw / Mn=4.6.

[0162] Preparation Example 2

[0163] Preparation Example 2 is prepared by the same steps as Preparation Example 1, except that the type of catalyst used and the reaction time are changed, and the molecular weight and molecular weight distribution obtained are different. The reactants are 129.8g of m-cresol, 86.5g of p-cresol, 61.8g of paraformaldehyde aqueous solution (95% by weight), 25.9g of phosphoric acid aqueous solution (89% by weight) (purchased from Nanjing Chemical Reagent Co., Ltd.) and 10.7g of thioglycolic acid (purchased from Anshida (Shandong) New Material Technology Co., Ltd.), kept at reflux temperature for 8 hours, and a yellow transparent solid resin (A-2) is obtained, whose Mw=1750 and Mw / Mn=2.4.

[0164] Negative photosensitive resin composition

[0165] Examples 1-4 and Comparative Examples 1-2

[0166] The photosensitive resins A-1 and A-2 prepared above were added to a sample bottle and mixed with other components according to the formula shown in Table 1. After mixing and stirring evenly with a standard reciprocating circular oscillator (model WS-100D purchased from Wiggens Company) (oscillation frequency 200 rpm, oscillation amplitude 30 mm, oscillation time 12 h), a negative photosensitive resin composition was obtained.

[0167] Test Example

[0168] The properties of the negative photosensitive resin compositions prepared in Examples 1-4 and Comparative Examples 1-2 were tested by the following methods, and the results are shown in Table 1.

[0169] Development film retention rate test

[0170] The negative photosensitive resin composition of the above embodiment was applied to a silicon wafer substrate by spin coating to form a coating film. Then, it was baked on a hot plate at 100°C for 90 seconds to form a photoresist film layer with a thickness of about 3.5 μm. Then, a mask with a line-to-line spacing ratio of 1:1 was used to apply 80 mJ / cm 2 The photoresist film layer was patterned exposed to ultraviolet light (the exposure machine model was Nikon NSR-2005i9C, manufactured by Nikon Corporation). Then, it was baked at 110° C. for 90 seconds on a hot plate to strengthen the degree of polymer crosslinking. Then, the photoresist film layer after the above treatment was developed with a 2.38% tetramethylammonium hydroxide (TMAH) aqueous solution at 23° C. for 60 seconds to remove the photoresist film layer in the unexposed area on the substrate. After the developed photoresist in the photolithography development step was washed with ultrapure water for 1 minute, an optical film thickness meter (Filmetrics F20, manufactured by FILMETRICS, Inc.) was used to test the thickness of the developed film layer with different exposure amounts, and the average value was taken as the film thickness after stabilization (after sufficient exposure). At this time, the numerical value of the film retention rate is set as follows: A: film retention rate ≥ 95%, B: 90% ≤ film retention rate < 95%, C: 80% ≤ film retention rate < 90%, D: film retention rate < 80%. In the case of A or B, the development film retention rate is evaluated as good, and in the case of C or D, it is evaluated as poor.

[0171] Shape stability assessment of inverted trapezoidal sections

[0172] The negative photosensitive resin composition of the above embodiment is applied to a silicon wafer substrate by spin coating to form a coating film. Then, a hot plate is used to bake at 100°C for 90 seconds to form a photoresist film layer with a thickness of about 3.5μm. Then, a mask with a line-to-line spacing ratio of 5:1 is used, and a filter is used to emit ultraviolet light of different wavelengths (mainly g-line and i-line), and the unexposed photoresist film layer is patterned and exposed under the optimal exposure dose under each wavelength, and soft contact (the exposure gap is uniformly set to 0μm) (exposure machine model MA-1400, manufactured by Japan Science Co., Ltd.). Then, a hot plate is used to bake at 110°C for 90 seconds to strengthen the degree of polymer crosslinking. Next, the above-mentioned treated photoresist film layer is developed for 60 seconds with a 2.38% tetramethylammonium hydroxide (TMAH) aqueous solution at 23°C to remove the photoresist film layer in the unexposed area on the substrate. The photoresist developed in the photolithography development step is washed with ultrapure water for 1 minute and then dried. The cross section is photographed and measured by a scanning electron microscope to determine the morphological changes under different exposure wavelengths. At this time, the difference ratio of the bottom cut width and height of the inverted trapezoid exposed by i-line and g-line is evaluated, and a horizontal comparison is made, that is, the difference in bottom cut height after the same composition is exposed with different i-line / g-line, A: bottom cut height difference ≤30%, bottom cut width difference ≤30%; B: 30% bottom cut height difference ≤60%, 30%<bottom cut width difference ≤60%; C: bottom cut height difference>60%, bottom cut width difference>60%, in the case of A, the shape stability of the inverted trapezoidal cross section is evaluated as excellent, in the case of B, the shape stability of the inverted trapezoidal cross section is evaluated as good, and in the case of C, it is evaluated as poor.

[0173] Critical Dimension Resolution Evaluation Test

[0174] Repeat the steps of the development retention rate test, and finally use a scanning electron microscope to measure the line width of the ISO Trench (individual line groove) area (this area has a large area of ​​photoresist after the photoresist is developed, and a line groove is formed in a small part (there is no photoresist at the position of the line groove)). The minimum measurable line width (CD) is used as the standard for evaluating the critical dimension resolution, A: CD ≤ 1μm; B: 1μm < CD ≤ 2.0μm; C: 2.0μm < CD ≤ 5.0μm; D: CD > 5.0μm. In the case of A, the resolution is evaluated as excellent, in the case of B, it is evaluated as good, in the case of C, it is evaluated as fair, and in the case of D, it is evaluated as poor.

[0175] Table 1

[0176]

[0177] Note 1: Alkali soluble resin, the phenolic varnish resin obtained in Preparation Example 1, homemade

[0178] Note 2: Alkali soluble resin, the phenolic varnish resin obtained in Preparation Example 2, homemade

[0179] Note 3: Photoacid generator, 2-[2-(4-methoxyphenyl-2-yl)vinyl]-4,6-bis(trichloromethane)-s-triazine, purchased from West Asia Chemical Technology (Shandong) Co., Ltd.

[0180] Note 4: Light stabilizer, bis(4-hydroxy-3-methoxyphenyl)-1,6-heptadiene-3,5-dione, purchased from TCI (Shanghai) Chemical Industry Development Co., Ltd.

[0181] Note 5: Light stabilizer, RUVA-93, purchased from Otsuka Chemical Co., Ltd.

[0182] Note 6: Cross-linking agent, hexamethoxymethyl melamine resin, purchased from Anaiji Chemical (Anhui Zesheng Technology Co., Ltd.)

[0183] Note 7: Solvent, propylene glycol methyl ether acetate, purchased from Yancheng Supul Chemical Technology Co., Ltd.

[0184] Note 8: Alkaline compound, triamylamine, purchased from TCI (Shanghai) Chemical Industry Development Co., Ltd.

[0185] Note 9: Surfactant, organosiloxane polymer, purchased from BYK Chemical Co., Ltd.

[0186] Table 2 Stability results of inverted trapezoidal sections

[0187]

[0188] As can be seen from Table 2, the inverted trapezoidal profile stability obtained using the negative photosensitive resin composition of Example 4 is the best. And the side of the obtained inverted trapezoidal shape has a certain curvature. Compared with the patterning using the 365nm exposure wavelength and the 436nm exposure wavelength, the difference in the undercut width obtained by the two is ≤30%, the difference in the undercut height is 0, and the stability of the inverted trapezoidal profile is evaluated as excellent. For Comparative Examples 1 and 2, the undercut height is 0, that is, there is almost no undercut, which is not conducive to the stripping process, because the metal coating thickness corresponding to the high resolution is generally thinner, the evaporation direction is relatively vertical, and the corresponding pattern will be denser, and it is necessary to ensure that there is an inverted trapezoidal morphology, so only a smaller undercut is required. A smaller undercut can ensure that the line will not be bleached due to the smaller bottom line width, and Comparative Examples 1 and 2 have almost no inverted trapezoidal morphology, so high resolution cannot be achieved. Therefore, the negative photosensitive resin composition using Example 4 can be suitable for exposure with light of different wavelengths, and a suitable undercut morphology can be obtained.

[0189] Table 3 Line width after photoresist exposure and development

[0190]

[0191] The data in Table 3 are obtained by using a wavelength of 365nm (i-line) and an exposure dose of 33mJ / cm 2 The results of exposure to light with an exposure time of 66 ms) show that the patterned photoresist film obtained by using the negative photosensitive resin composition of Example 4 has the smallest line width as shown in Table 3. In the critical dimension resolution test of Example 4, that is, the line width test, it can be concluded that in the ISO Trench area, the line width is 0.85 μm, and the position here achieves high resolution, close to the standard inverted trapezoid, with the side wall diagonally straight down.

[0192] Therefore, in the process of photolithography using the negative photosensitive resin composition of the present invention, light with different wavelengths can be used for exposure, and the inverted trapezoidal morphologies formed are similar and have good stability, so as to match mercury lamps with different wavelengths.

[0193] Furthermore, the negative photosensitive resin composition of the present invention has sufficient photosensitivity even when the photoresist film is relatively thin, and can also maintain a good film retention rate.

Claims

1. A negative photosensitive resin composition, comprising: (A) an alkali-soluble resin comprising at least two novolac resins having different molecular weights, 100 parts by weight; (B) a photoacid generator, 0.1-5 parts by weight; (C) light stabilizer, 0.1-20 parts by weight; (D) a cross-linking agent, 1-45 parts by weight; (E) solvent, 100-600 parts by weight; (F) a basic compound, 0.2-2 parts by weight; and (G) optional additives, 0.01-20 parts by weight; The amounts of components (B) to (G) are based on 100 parts by weight of the alkali-soluble resin (A). The light stabilizer is selected from ketone light stabilizers and triazole light stabilizers. The at least two novolac resins are A-1 and A-2, and both have the structure of formula (1), Among them, m:n is 1:9 to 9:1, The weight average molecular weight of A-1 is 1,000 to 100,000, and the molecular weight distribution is 1.0 to 8.0; the weight average molecular weight of A-2 is 1,000 to 15,000, and the molecular weight distribution is 1.0 to 4.0, and the weight average molecular weight of A-1 is greater than that of A-2.

2. The negative photosensitive resin composition according to claim 1, wherein the photoacid generator as component (B) is 0.5-4 parts by weight.

3. The negative photosensitive resin composition according to claim 2, wherein the photoacid generator as component (B) is 0.5-3.5 parts by weight. 4 . The negative photosensitive resin composition according to claim 1 , wherein the light stabilizer of component (C) is 0.5 to 10 parts by weight. 5 . The negative photosensitive resin composition according to claim 1 , wherein the component (D) crosslinking agent is 2-35 parts by weight. 6 . The negative photosensitive resin composition according to claim 5 , wherein the component (D) crosslinking agent is 3-30 parts by weight. 7 . The negative photosensitive resin composition according to claim 1 , wherein the component (E) solvent is 110-550 parts by weight. 8 . The negative photosensitive resin composition according to claim 7 , wherein the component (E) solvent is 120-500 parts by weight. 9 . The negative photosensitive resin composition according to claim 1 , wherein the basic compound of component (F) is 0.3-1.8 parts by weight. 10 . The negative photosensitive resin composition according to claim 9 , wherein the basic compound of component (F) is 0.4-1.6 parts by weight. 11 . The negative photosensitive resin composition according to claim 1 , wherein the component (G) additive is 0.1-15 parts by weight. 12 . The negative photosensitive resin composition according to claim 1 , wherein the component (G) additive is 0.1-10 parts by weight.

13. The negative photosensitive resin composition according to any one of claims 1 to 12, wherein the light stabilizer is selected from bis(4-hydroxy-3-methoxyphenyl)-1,6-heptadiene-3,5-dione and RUVA-93.

14. The negative photosensitive resin composition according to any one of claims 1 to 12, wherein the weight relationship between the basic compound (F) (denoted as g), the photoacid generator (B) (denoted as m) and the light stabilizer (C) (denoted as h) satisfies the following relationship: 0.28≤g / [mh / (m+h)]≤1.

00.

15. The negative photosensitive resin composition according to claim 14, wherein the weight relationship between the basic compound (F) (denoted as g), the photoacid generator (B) (denoted as m) and the light stabilizer (C) (denoted as h) satisfies the following relationship: 0.405≤g / [mh / (m+h)]≤0.

85.

16. The negative photosensitive resin composition according to claim 15, wherein the weight relationship between the basic compound (F) (denoted as g), the photoacid generator (B) (denoted as m) and the light stabilizer (C) (denoted as h) satisfies the following relationship: 0.79≤g / [mh / (m+h)]≤0.

83.

17. The negative photosensitive resin composition according to any one of claims 1 to 12, wherein the weight relationship between the photoacid generator (B) (denoted as m), the alkali-soluble resin (A) (denoted as n) and the crosslinking agent (D) (denoted as q) satisfies the following relationship: 0.162≤m / [nq / (n+q)]≤0.

200.

18. The negative photosensitive resin composition according to claim 17, wherein the weight relationship between the photoacid generator (B) (denoted as m), the alkali-soluble resin (A) (denoted as n) and the crosslinking agent (D) (denoted as q) satisfies the following relationship: 0.166≤m / [nq / (n+q)]≤0.

170. 19 . The negative photosensitive resin composition according to claim 1 , wherein the weight average molecular weight of A-1 is 1,500 to 50,000. 20 . The negative photosensitive resin composition according to claim 19 , wherein the weight average molecular weight of A-1 is 4,000 to 8,000. 21 . The negative photosensitive resin composition according to claim 1 , wherein the molecular weight distribution of the A-1 is 3.0 to 7.

0. 22 . The negative photosensitive resin composition according to claim 1 , wherein the weight average molecular weight of A-2 is 2,000 to 5,000. 23 . The negative photosensitive resin composition according to claim 1 , wherein the molecular weight distribution of A-2 is 1.5 to 3.

0.

24. The negative photosensitive resin composition according to any one of claims 1 to 12, wherein the amount of A-1 is 30 to 100 wt% based on 100 wt% of the total amount of A-1 and A-2. 25 . The negative photosensitive resin composition according to claim 24 , wherein the amount of A-1 is 35 to 90 wt % based on 100 wt % of the total amount of A-1 and A-2. 26 . The negative photosensitive resin composition according to claim 25 , wherein the amount of A-1 is 40 to 70 wt % based on 100 wt % of the total amount of A-1 and A-2. 27 . The negative photosensitive resin composition according to claim 1 , wherein the ratio of the photoacid generator to the light stabilizer is 0.01-0.80:

1. 28 . The negative photosensitive resin composition according to claim 27 , wherein the ratio of the photoacid generator to the light stabilizer is 0.02-0.60:

1. 29 . The negative photosensitive resin composition according to claim 1 , wherein the photoacid generator and the crosslinking agent are used in an amount ratio of 0.01 to 0.

30. 30 . The negative photosensitive resin composition according to claim 29 , wherein the photoacid generator and the crosslinking agent are used in an amount ratio of 0.08 to 0.

23. 31 . The negative photosensitive resin composition according to claim 30 , wherein the photoacid generator and the crosslinking agent are used in an amount ratio of 0.13 to 0.

18.

32. The negative photosensitive resin composition according to any one of claims 1 to 12, wherein the basic compound is selected from aliphatic amines, amino alcohols, aromatic amines, quaternary ammonium hydroxides or combinations thereof. 33 . The negative photosensitive resin composition according to claim 32 , wherein the basic compound is tripentylamine, N-ethylaniline, N,N-dimethylaminophenol, tetramethylammonium hydroxide, diethylaminopropylamine or a combination thereof.

34. A method for forming a pattern from a negative photosensitive resin composition, comprising the following steps: (i) uniformly coating the negative photosensitive resin composition according to any one of claims 1 to 33 on a substrate to form a photoresist film layer, (ii) pre-baking the photoresist film obtained in (i) at a temperature of 80 to 130° C. using a hot plate, and the thickness of the photoresist after baking is 0.5 to 15 μm, (iii) partially irradiating the photoresist film layer formed in (ii) through a mask with radiation, (iv) performing a post-exposure bake on the exposed film in (iii) at a temperature of 90 to 130° C. using a hot plate, (v) The photoresist film obtained in (iv) is developed using a developer.

35. Use of the negative photosensitive resin composition according to any one of claims 1 to 33 for metal patterning in semiconductor preparation.

Citation Information

Patent Citations

  • Composition, pattern forming method, and manufacturing methods of crystal particles and display device

    CN104238270A

  • Negative photosensitive resin composition and application thereof

    CN104345557A

  • Negative resist composition for thick film and laminate thereof

    JP2010026278A

  • Negative photoresist composition having characteristics possible to perform organic pattern coating process on pattern formed with the composition, method for manufacturing optical sensors using the composition and the optical sensors manufactured thereby

    KR1020170022611A

  • Negative photosensitive resin composition and application thereof

    TW201925917A