Seamless aluminum tube flanging process
By optimizing the aluminum tube processing technology, using 6061-O aluminum rods to produce seamless aluminum tubes and performing T6 heat treatment, the problems of poor elongation and heat treatment deformation of aluminum-magnesium alloy are solved, and the mechanical performance improvement and lightweight effect is achieved. It is suitable for Car shock absorber skeleton.
Patent Information
- Application Number
- CN202211089249.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-07
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-09-07
AI Technical Summary
The existing aluminum-magnesium alloy materials have poor extension in the automotive shock absorber skeleton, making it difficult to produce shapes that meet the requirements, and are prone to deformation after heat treatment, resulting in product cracking and safety hazards. Conventional aluminum pipes have welded wires that affect the beauty but are prone to cause The stress of flange forming is concentrated, which is easy to cause cracking.
The 6061-O aluminum rod is used to produce seamless aluminum tubes through reverse extrusion technology, and perform necking, chamfering, reaming, molding, T6 heat treatment, shaping, edge cutting and punching to form aluminum tubes that meet the requirements. , avoid deformation after welding wire and heat treatment, optimize the process to improve mechanical properties and reduce weight.
The mechanical performance of seamless aluminum pipes is improved, which avoids deformation and cracking problems, reduces cost and weight, improves yield, and meets the mechanical performance and lightweight needs of automotive shock absorbers.
Smart Images

Figure CN115533448B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of aluminum tube processing, in particular to a seamless aluminum tube flanging processing technology. Background Art
[0002] The shock absorber of a motor vehicle is a key component in the vehicle's running parts. It can quickly attenuate the vibration transmitted from the road surface to the vehicle body, improve riding comfort, reduce fatigue of drivers and passengers, and prevent damage to goods, thus improving riding comfort. It can reduce the impact load of related parts, reduce wear, and improve economic use. It can also improve the ground contact of tires, suppress high-speed driving vibration, and improve driving safety. It can also improve the running stability of the vehicle during sudden acceleration, braking, and sharp turns. The performance of the shock absorber directly affects the driving stability, comfort, service life of vehicle components, and driving safety.
[0003] Automobile shock absorbers are composed of shock absorber frames (aluminum tubes) and rubber. The shock absorber frames are important components that meet the rigidity requirements of shock absorbers. In order to meet the mechanical properties of the shock absorber frames, iron materials are often given priority in material selection in the early stage. However, the biggest drawback of iron materials is their high material density and the produced parts are heavy. With the development trend of lightweight automobiles, it is urgent to study shock absorbers that meet both performance requirements and weight requirements.
[0004] From the perspective of production economy and mass production, aluminum is the best choice to replace iron. However, the performance of conventional aluminum cannot meet the required mechanical performance requirements. The aluminum-magnesium alloys that meet the performance requirements often have poor elongation and weak plasticity, making it difficult to produce the shapes of parts we need. For example, the conventional iron shock absorber frame material is DC01, and the material elongation standard is ≥28%. The conventional aluminum-magnesium alloy 6061-T6 state material has an elongation standard of only 8%. Forced plastic extension will cause the product to crack, which will pose a safety hazard to our driving.
[0005] The main alloying elements of 6061-T6 aluminum alloy are magnesium and silicon. It has medium strength, good corrosion resistance, weldability, and good oxidation effect. It is widely used in various industrial structural parts that require a certain strength (HW ≥ 15.5°) and high corrosion resistance. It is a more common material among 6 series aluminum profiles. The 6061-T6 aluminum tubes commonly used on the market are mostly seam tubes. The definition of seam tubes is that the profile has a welding line. The welding line is extruded from the aluminum profile splitter die with a cavity. The splitter die is divided into two upper and lower molds. When aluminum is extruded, the aluminum flowing into the splitter die will be separated and then welded through the welding chamber, and there will be welding lines on the surface of the extruded aluminum profile. The welding line is very detrimental to the appearance, but through some technical innovations and operating specifications, the welding line on the surface of the aluminum profile can be reduced, making it almost invisible to the naked eye. However, after the aluminum tube with welding lines is flanging, the position of the welding line becomes the stress concentration point of the entire flanging forming, which is easy to cause product cracking during forming.
[0006] Some aluminum tubes are made using the reverse extrusion process. The main advantage of this aluminum tube is that it has no welding line. It is also called a seamless tube in the industry. This type of aluminum tube can effectively avoid stress concentration during flanging, thereby preventing product cracking. However, the disadvantage of this tube is that the procurement cost is relatively high. Summary of the invention
[0007] The main technical problem solved by the present invention is to provide a seamless aluminum tube flanging processing technology, optimize the process, perform heat treatment on the tube blank after forming, and finally perform processing, so as to avoid deformation of the aluminum tube during processing, take into account the mechanical properties and weight of the product, so that the product can meet the required mechanical performance requirements and reduce the weight of the product, thereby achieving the purpose of lightweighting the product.
[0008] In order to solve the above technical problems, a technical solution adopted by the present invention is: to provide an aluminum tube flanging processing technology, comprising the following steps: a. material selection and cutting: 6061-O aluminum rod is selected as the base material, and a reverse extrusion process is adopted to produce a seamless aluminum tube, and the seamless aluminum tube is cut by a profile cutting machine to form a tube blank of a required size; b. necking: the tube blank is placed in a mold, and one end of the tube blank is necked by a punch, and the necked end forms an inner flanging; c. chamfering: the necked tube blank is turned over, and the other end of the tube blank is chamfered inside and outside; d. hole expansion: the tube blank is placed in a hole expansion mold, and the chamfered end of the tube blank is expanded by a punch, and a trumpet-shaped structure is formed at one end of the expanded tube blank; e. molding: the expanded tube blank is placed in a shaping mold, and the product is shaped into a shape of an inner flanging at one end and an outer flange at the other end by a punch; f. T6 heat treatment: put the tube into a heating furnace, heat it to the appropriate temperature, and then send it into an air furnace to keep it warm for a certain period of time, then quickly cool it in water, put the cooled parts into an aging furnace, take them out after keeping them warm in the aging furnace for a certain period of time, and then cool them to room temperature to obtain 6061-T6 tubes; g. Shaping: since the tube will be deformed after heat treatment, put the tube into a shaping die, and use a punch press to perform shaping operations to restore the shape of the tube to the state before heat treatment; h. Trimming: trim the shaped tube, punch and shear off the excess part around the outer flange of the flange to obtain the dimensional tolerance required by the drawing; i. Punching: punch the inner hole of the part after trimming, punch and shear off the excess part of the circular hole along the inner flange to obtain the dimensional tolerance required by the drawing; j. Grinding, cleaning and degreasing; grinding the trimming and punching parts of the tube blank to remove burrs, then placing the tube blank in a solution added with weak acid for degreasing, removing oil stains on the surface of the parts to obtain a finished aluminum tube.
[0009] In a preferred embodiment of the present invention, the yield strength of the 6061-O tube blank in step a is ≤150Mpa, the material elongation is ≥16%, and the Vickers hardness is ≤10°.
[0010] In a preferred embodiment of the present invention, the yield strength of the 6061-T6 tube blank in step f is ≥260MPa, the material elongation is ≥8%, and the Vickers hardness is ≥15.5°
[0011] In a preferred embodiment of the present invention, the chamfer dimensions in step c are: outer chamfer C = material wall thickness * 2 / 3, inner chamfer C = material wall thickness * 1 / 3.
[0012] In a preferred embodiment of the present invention, the heating temperature of the heating furnace in step f is 516-579°C, the insulation time in the air furnace is 20-30 minutes, and the insulation temperature of the aging furnace is 171-182°C, and the insulation time is 8-9 hours.
[0013] In a preferred embodiment of the present invention, in step j, the tube blank is placed in a vibration grinder equipped with a brown corundum grinding stone for grinding for 20-30 minutes.
[0014] In order to solve the above technical problems, another technical solution adopted by the present invention is: to provide an aluminum tube, which is made by the above aluminum tube flanging process, and the aluminum tube is used for a shock absorber frame of an automobile shock absorber.
[0015] The beneficial effects of the present invention are as follows: the flanging process of the seamless aluminum tube of the present invention uses the seamless aluminum rod of 6061-O state as the base material, and uses the performance characteristics of the material to first make a formed tube blank, and then the tube blank undergoes solid solution aging heat treatment to form a tube blank of 6061-T6 state, and then undergoes high-precision shaping, trimming and punching processes, which not only meet the use requirements of the product, but also meet the performance requirements of the product. It overcomes the defect of poor mechanical properties of aluminum tubes made of seamless aluminum rods of 6061-O state, and also avoids the problem of deformation of aluminum tubes made of seamless aluminum rods of 6061-T6 state after heat treatment, effectively improves the yield rate, and reduces the manufacturing cost at the same time, taking into account the mechanical properties and weight of the product, so that the product can meet the required mechanical performance requirements, and can also reduce the weight of the product, achieving the purpose of lightweighting the product. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative work, among which:
[0017] Figure 1 It is a process flow diagram of a preferred embodiment of the aluminum tube flanging process of the present invention; DETAILED DESCRIPTION
[0018] The technical scheme in the embodiment of the present invention will be described clearly and completely below. The structures, proportions, sizes, etc. illustrated in the drawings of this specification are only used to match the contents disclosed in the specification, so that people familiar with this technology can understand and read them, and are not used to limit the limiting conditions that the present invention can implement, so they have no substantial technical significance. Any modification of the structure, change of the proportional relationship, or adjustment of the size should still fall within the scope that the technical content disclosed by the present invention can cover without affecting the effects that the present invention can produce and the purposes that can be achieved. At the same time, the terms such as "upper", "lower", "left", "right", "middle" and so on quoted in this specification are only for the convenience of narration, and are not used to limit the scope that can be implemented. The change or adjustment of the relative relationship should also be regarded as the scope that the present invention can implement without substantially changing the technical content.
[0019] See also Figure 1 , an aluminum tube flanging process, comprising the following steps:
[0020] a. Material selection and cutting: 6061-O aluminum rods are selected as the base material, and the reverse extrusion process is used to produce seamless aluminum tubes. The seamless aluminum tubes are cut into tube blanks of the required size by the profile cutting machine. The yield strength of the 6061-O tube blank is ≤150Mpa, the material elongation is ≥16%, and the Webster hardness is ≤10°. Because the material properties of the 6061-O seamless aluminum tube are relatively soft, the material elongation is high, there is no weld line, but the mechanical properties are poor, the above characteristics are used to avoid the cracking of the tube blank during the subsequent necking, hole expansion and forming processes.
[0021] b. Neck reduction: Place the tube blank into the mold and use a punch to reduce the neck of one end of the tube blank. The reduced neck end forms an inner flange to facilitate subsequent shaping operations.
[0022] c. Chamfering: In order to reduce the cracking rate of the product after flanging, the tube blank after necking treatment is turned over, and the other end of the tube blank is processed with internal and external chamfering. The external chamfer C = material wall thickness * 2 / 3, and the internal chamfer C = material wall thickness * 1 / 3.
[0023] d. Hole expansion: Place the tube blank into the hole expansion die, and expand the chamfered end of the tube blank through a punch press. After expansion, one end of the tube blank forms a trumpet-shaped structure, which is convenient for subsequent shaping operations.
[0024] e. Forming: Put the expanded tube into the shaping mold, and use the punch press to shape the product into a shape with one end as an inner turn-up and the other end as an outer turn-up. The shape of the whole aluminum tube is completed by the forming process, and the tube with a shaped shape is obtained. The 6061-O aluminum tube will not crack during the processing of step be because there is no welding line. Compared with the 6061-T6 aluminum tube, the yield rate is higher and the cost is lower.
[0025] f. T6 heat treatment: put the tube billet into a heating furnace with a heating temperature of 516-579℃ and a holding time of 20-30 minutes in an air furnace, then quickly cool it in water, put the cooled parts into an aging furnace for holding at a holding temperature of 171-182℃ for 8-9 hours, and then cool it to room temperature to obtain a 6061-T6 tube billet with a yield strength of ≥260MPa, a material elongation of ≥8%, and a Webster hardness of ≥15.5°. The 6061-O tube billet is converted into a 6061-T6 tube billet through a solid solution aging heat treatment, and the solid solution aging heat treatment step is advanced. After the heat treatment is completed, the processing step of the position with higher dimensional accuracy requirements is carried out. Even if the tube billet is deformed during the heat treatment process, it can be reshaped and repaired later, so as not to affect the yield rate. Therefore, it is effective to avoid the problem that the finished aluminum tube formed by the 6061-T6 tube billet is deformed due to the final heat treatment, thereby causing the finished aluminum tube to be unqualified.
[0026] g. Shaping: Since the tube billet will be deformed after heat treatment, the tube billet is placed in a shaping die and shaped by a punch press to restore the shape of the tube billet to the state before heat treatment. The tube billet is repaired to ensure accuracy for subsequent processing.
[0027] h. Trimming: Trim the tube blank after shaping, and cut off the excess part around the flange fold to obtain the dimensional tolerance required by the drawing.
[0028] i. Punching: Punch the inner holes of the trimmed parts, cut off the excess part of the circular hole along the inner fold, and obtain the dimensional tolerance required by the drawing.
[0029] j. Grinding, cleaning and degreasing: Grind the trimmed and punched parts of the tube blank, put the tube blank into a vibration grinder equipped with a brown corundum grinding stone, and grind for 20-30 minutes to remove the burrs. Then put the tube blank into a solution added with weak acid to degrease and remove the oil stains on the surface of the parts to obtain the finished aluminum tube.
[0030] An aluminum tube is manufactured by the aluminum tube flanging process, and the aluminum tube is used for a shock absorber frame of an automobile shock absorber.
[0031] The flanging process of the seamless aluminum tube of the present invention first uses 6061 aluminum rod as a base material to be processed into an O-state tube blank, thereby avoiding the problem of deformation of the 6061-T6-state seamless aluminum rod before being used as a base material for molding in various process processes. Then, the 6061-O-state tube blank is transformed into a 6061-T6-state tube blank through heat treatment, and the 6061-T6-state tube blank is finely processed to obtain a finished aluminum tube, thereby avoiding the problem of deformation of the finished aluminum tube caused by directly processing the 6061-O-state tube blank into the finished aluminum tube and then performing heat treatment. The aluminum tube finally obtained not only meets the use requirements of the product, but also meets the performance requirements of the product.
[0032] Different from the prior art, the seamless aluminum tube flanging processing technology of the present invention optimizes the process, performs heat treatment on the tube blank after forming, and finally performs processing, so as to avoid deformation of the aluminum tube during processing, and take into account the mechanical properties and weight of the product, so that the product can meet the required mechanical performance requirements and reduce the weight of the product, thereby achieving the purpose of lightweighting the product.
[0033] The present invention and its embodiments are described schematically above, and the description is not restrictive. The drawings show only one embodiment of the present invention, and the actual structure is not limited thereto. Therefore, if a person skilled in the art is inspired by it and designs a structural method and an embodiment similar to the technical solution without creativity without departing from the purpose of the invention, they shall all fall within the protection scope of the present invention.
Claims
1. A flanging process for an aluminum tube, characterized in that: The following steps are involved: a. Material Selection and Cutting: 6061-O aluminum bars are used as the base material. Seamless aluminum tubes are produced through reverse extrusion. The seamless aluminum tubes are then cut into tube blanks of the required size using a profile cutter. The yield strength of the 6061-O tube blanks is ≤150Mpa, the material elongation is ≥16%, and the Webster hardness is ≤10°. b. Necking: The tube is placed in a die and one end of the tube is necked by a punch press, forming an inward flange on the necked end. c. Chamfering: Turn the necked tube over and perform internal and external chamfering on the other end of the tube; d. Hole expansion: The tube is placed in the hole expansion die, and the chamfered end of the tube is expanded by a punch press. After expansion, one end of the tube forms a trumpet-shaped structure. e. Forming: The expanded tube is placed into a shaping die and the punch press is used to shape the product into a shape with an inward turning edge at one end and an outward turning edge at the other end. f. T6 heat treatment: The tube billet is placed in a heating furnace, heated to the appropriate temperature, and then placed in an air furnace for a certain period of time. It is then quickly cooled in water. The cooled parts are placed in an aging furnace and kept in the aging furnace for a certain period of time. The parts are then removed and cooled to room temperature to obtain the 6061-T6 state tube billet. The yield strength of the 6061-T6 state tube billet is ≥260MPa, the material elongation is ≥8%, and the Webster hardness is ≥15.5°. The heating temperature of the heating furnace is 516-579°C, the holding time in the air furnace is 20-30 minutes, and the holding temperature of the aging furnace is 171-182°C for 8-9 hours. g. Shaping: Since the tube billet will be deformed after heat treatment, the tube billet is placed in a shaping die and shaped by a punch press to restore the tube billet's shape to its pre-heat treatment state. h. Trimming: Trim the shaped tube blank by punching and shearing off the excess part around the flange to obtain the dimensional tolerance required by the drawing; i. Punching: Punch the inner holes of the trimmed parts. Shear off the excess portion of the circular hole along the inner flange to obtain the dimensional tolerance required by the drawing. j. Grinding, cleaning and degreasing: Grind the trimmed and punched areas of the tube to remove burrs. Then, place the tube in a solution containing a weak acid to degrease the surface of the parts to obtain the finished aluminum tube.
2. The aluminum tube flanging process according to claim 1, characterized in that: The chamfer dimensions in step c are: outer chamfer C = material wall thickness * 2 / 3, inner chamfer C = material wall thickness * 1 / 3.
3. The aluminum tube flanging process according to claim 1, characterized in that: In the step j, the tube blank is placed in a vibration grinder equipped with a brown corundum grinding stone and subjected to grinding operation for 20-30 minutes.