Aqueous positive electrode slurry for lithium iron phosphate battery and preparation method thereof, lithium iron phosphate battery and positive electrode sheet

Through the multi-step preparation method and the use of surfactants and thickeners, the wettability and stability problems of the aqueous cathode slurry of lithium iron phosphate batteries are solved, and a uniformly dispersed and stable slurry is prepared, which reduces production costs. And improve environmental protection.

CN115579460BActive Publication Date: 2024-10-18JIANGSU TIANHE ENERGY STORAGE CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202211384770.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-07
Publication Date
2024-10-18
Estimated Expiration
2042-11-07

AI Technical Summary

Technical Problem

The existing aqueous cathode slurry for lithium iron phosphate batteries has poor wettability with water due to the nanoscale carbon-containing LFP main material and conductive agent, resulting in large particle size, poor stability and castability, and it is difficult to prepare a slurry with good stability and uniform dispersion. material.

Method used

A multi-step preparation method is adopted, including dry mixing, kneading and stirring, dispersion and high-temperature and high-viscosity stirring, adding surfactants and thickeners, controlling the solid content and stirring conditions, and preparing aqueous cathode slurry for lithium iron phosphate batteries with good stability. material.

Benefits of technology

It significantly improves the dispersion and stability of the aqueous cathode slurry, avoids environmental pollution and high costs of using organic solvents, reduces production costs, and improves environmental protection and safety.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to a lithium iron phosphate battery aqueous positive electrode slurry and a preparation method, a lithium iron phosphate battery and a positive electrode sheet. The preparation method comprises: (1) dry-mixing lithium iron phosphate powder with a conductive agent and a first part of a thickener to obtain a mixed material; (2) adding water and a surfactant to the mixed material obtained from step (1) to obtain a first mixed slurry with a solid content of 80 to 90 wt%; (3) dispersing water into the first mixed slurry obtained from step (2) to obtain a second mixed slurry with a solid content of 75 to 80 wt%; (4) dispersing the second part of the thickener and water into the second mixed slurry obtained from step (3); (5) dispersing an aqueous binder and water into a third mixed slurry. The preparation method of the lithium iron phosphate battery aqueous positive electrode slurry of the present invention obtains a lithium iron phosphate battery aqueous positive electrode slurry with uniform dispersion and good stability by adding a surfactant, a thickener and a multi-step high-viscosity, high-temperature stirring preparation method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to an aqueous positive electrode slurry for a lithium iron phosphate battery and a preparation method thereof, a lithium iron phosphate battery and a positive electrode sheet. Background Art

[0002] Lithium iron phosphate (LFP) is considered to be a new type of lithium-ion battery cathode material with broad application prospects due to its abundant raw material sources, low price, good thermal stability, and excellent cycle performance. It has been widely used in the fields of energy storage and power batteries. The current mainstream production method of lithium iron phosphate (LFP) cathode slurry adopts oil-based slurry for stirring and production, that is, a system composed of adhesive PVDF (polyvinylidene fluoride), solvent N-methylpyrrolidone (NMP) and main material LFP and conductive agent. However, the NMP organic solvent used in the oil-based cathode slurry is expensive and has certain corrosiveness. The amount used is large, it is not environmentally friendly, and the recycling cost is high; a large amount of NMP is heated and volatilized during the coating and drying process. In order to prevent the explosive and corrosive NMP from volatilizing arbitrarily, causing deflagration and environmental pollution, a large number of environmental protection equipment must be installed, which also increases production costs and is not conducive to production operations.

[0003] Therefore, the preparation of low-cost, pollution-free LFP aqueous positive electrode slurry has become a technical difficulty that lithium battery professionals urgently need to overcome. At present, the more feasible aqueous lithium iron phosphate slurry scheme mainly uses water-soluble binders and deionized water as solvents. For example, patent CN101872856B discloses a lithium iron phosphate battery positive electrode slurry, a lithium iron phosphate battery using the positive electrode slurry, and a preparation method thereof. The aqueous positive electrode slurry is composed of the following weight fractions: lithium iron phosphate, 40-55%; conductive agent, 2-5%; aqueous adhesive, 3-5%; deionized water: 40-55%; the aqueous positive electrode slurry of this scheme greatly increases the quality of the positive lithium iron phosphate active material, and there is no undesirable phenomenon such as water absorption, de-powdering, and material falling during the production process of the positive electrode sheet, and it has good softness and adhesion. However, due to the poor wettability of the nano-scale carbon-containing LFP main material and the conductive agent with water and the easy agglomeration of nanoparticles, the slurry particle size of this scheme is large, and the stability and castability are poor. Patent CN112447969A discloses an aqueous positive electrode slurry for lithium iron phosphate batteries and a preparation method thereof, wherein the aqueous positive electrode slurry comprises 90-93 parts of lithium iron phosphate, 2-3 parts of composite graphene conductive slurry, 3-5 parts of aqueous binder, 1-2 parts of conductive agent and deionized water; this solution avoids environmental pollution caused by the use of organic solvents, and is more environmentally friendly and safe; the aqueous graphene composite conductive slurry used is a conductive agent, which can reduce the battery's ohmic internal resistance and polarization internal resistance, and improve the high-power starting performance of lithium batteries. However, it does not solve the problem of poor slurry dispersion and poor slurry stability caused by the wettability of carbon materials with water and the stability of water-based suspensions.

[0004] In summary, the carbon-containing LFP main material and the conductive agent have poor water wettability and the nanoparticles are easy to agglomerate, which leads to large particle size, poor stability and castability of this aqueous slurry. How to solve the problem of poor water wettability of the carbon-containing LFP main material and the conductive agent, so as to prepare a stable and uniformly dispersed aqueous positive electrode slurry for lithium iron phosphate batteries is a technical problem that needs to be solved urgently. Summary of the invention

[0005] The present invention provides a lithium iron phosphate battery aqueous positive electrode slurry and a preparation method thereof, a lithium iron phosphate battery and a positive electrode sheet, so as to prepare an aqueous positive electrode slurry with good stability and uniform dispersion while reducing production costs.

[0006] In a first aspect, the present invention relates to a method for preparing an aqueous positive electrode slurry for a lithium iron phosphate battery, the preparation method comprising the following steps: (1) dry-mixing lithium iron phosphate powder with a conductive agent and a first portion of a thickener to obtain a mixed material; (2) adding water and a surfactant to the mixed material obtained in step (1), and then kneading and stirring to obtain a first mixed slurry with a solid content of 80 to 90 wt %; the surfactant is selected from at least one of 2-amino-2-methyl-1-propanol, styrene-acrylate copolymer and polyvinyl pyrrolidone; (3) dispersing water into the first mixed slurry obtained in step (2) to obtain a second mixed slurry with a solid content of 75 to 80 wt %; (4) dispersing the second portion of the thickener and water into the second mixed slurry obtained in step (3) to obtain a third mixed slurry with a solid content of 70 to 75 wt %; (5) dispersing an aqueous binder and water into the third mixed slurry obtained in step (4).

[0007] Optionally, in step (1), the conductive agent is selected from at least one of carbon black, graphite, carbon nanotubes and carbon nanofibers; the first part of the thickener in step (1) and the second part of the thickener in step (4) are each independently selected from sodium carboxymethyl cellulose and / or lithium carboxymethyl cellulose; and the aqueous binder in step (5) is selected from at least one of polyacrylic acid, styrene-butadiene rubber and polyacrylonitrile.

[0008] Optionally, in step (1), the lithium iron phosphate powder is micron-sized, submicron-sized or nano-sized carbon-coated lithium iron phosphate.

[0009] Optionally, in step (1), the lithium iron phosphate powder is 92 to 98 parts by weight, the conductive agent is 0.5 to 4 parts by weight, and the first part of the thickener is 30 to 60% of the 0.5 to 2 parts by weight; the water added in step (2) is 10-30% of the 33 to 150 parts by weight, and the surfactant is 0.2 to 2 parts by weight; the water added in step (3) is 5-20% of the 33 to 150 parts by weight; the water added in step (4) is 5-20% of the 33 to 150 parts by weight, and the second part of the thickener is 40 to 70% of the 0.5 to 2 parts by weight; in step (5), the aqueous binder is 1 to 4 parts by weight, and the water added is 30-80% of the 33 to 150 parts by weight.

[0010] Optionally, in step (1), the dry mixing conditions include: carrying out the dry mixing in a mixer, with a revolution of 5-20 rpm, a rotation of 10-300 rpm and a dry mixing time of 5 to 20 min.

[0011] Optionally, in step (2), the kneading and stirring conditions include: carrying out the kneading and stirring in a mixer, with an orbital speed of 5-20 rpm, an autorotation speed of 50-500 rpm, a temperature of 40-70° C., and a kneading and stirring time of 30-100 min.

[0012] Optionally, in step (3), the dispersing conditions include: carrying out in a mixer, revolution 5-20 rpm, rotation 10-800 rpm, temperature 40-70° C. and stirring time 30-75 min.

[0013] Optionally, in step (4), the dispersion conditions include: carrying out in a blender, revolution of 15-30 rpm, rotation of 800-3000 rpm, temperature of 30-45°C, vacuum degree of -20--100 kPa, and stirring time of 60-180 min; in step (5), the dispersion conditions include: carrying out in a blender, revolution of 15-30 rpm, rotation of 500-3000 rpm, temperature of 30-45°C, vacuum degree of -20--100 kPa, and stirring time of 60-180 min.

[0014] Optionally, step (5) is performed to obtain an aqueous positive electrode slurry for a lithium iron phosphate battery having a solid content of 40 to 70 wt % and a viscosity of 3000 to 15000 mPa·s.

[0015] In a second aspect, the present invention relates to an aqueous positive electrode slurry for a lithium iron phosphate battery, which is prepared by the preparation method.

[0016] In a third aspect, the present invention relates to a positive electrode sheet of a lithium iron phosphate battery, wherein a membrane in the positive electrode sheet is made of the aqueous positive electrode slurry of the lithium iron phosphate battery.

[0017] In a fourth aspect, the present invention relates to a lithium iron phosphate battery, wherein the positive electrode sheet in the lithium iron phosphate battery is the positive electrode sheet described above.

[0018] Beneficial effects:

[0019] (1) The preparation method of the aqueous positive electrode slurry for lithium iron phosphate batteries of the present invention solves the difficulty of wettability of carbon-containing LFP particles and conductive agents in aqueous positive electrode slurry of lithium iron phosphate by water through the addition of surfactants, thickeners and multi-step high viscosity and high temperature stirring preparation method, thereby improving the problems of easy agglomeration, long dispersion time and unstable slurry suspension system of aqueous positive electrode slurry;

[0020] (2) The aqueous positive electrode slurry of lithium iron phosphate battery prepared by the preparation method of the present invention is evenly dispersed and has good stability;

[0021] (3) It avoids the use of expensive and corrosive organic solvent NMP, significantly reduces the manufacturing cost of lithium iron phosphate batteries, and improves environmental protection. DETAILED DESCRIPTION

[0022] The present invention is further described in detail below through examples. Through these examples, the features and advantages of the present invention will become clearer and more specific.

[0023] The word “exemplary” is used exclusively herein to mean “serving as an example, example, or illustration.” Any embodiment described herein as “exemplary” is not necessarily to be construed as preferred or advantageous over other embodiments.

[0024] In addition, the technical features involved in different embodiments of the present application described below can be combined with each other as long as they do not conflict with each other.

[0025] In the present invention, LFP represents lithium iron phosphate, NMP represents N-methylpyrrolidone, 2-amino-2-methyl-1-propanol can be added in the form of AMP-95, AMP-95 represents an aqueous solution of 2-amino-2-methyl-1-propanol (mass fraction ≥ 95.0%) as a multifunctional amine additive, PAA represents polyacrylic acid, SBR represents styrene-butadiene rubber, and PAN represents polyacrylonitrile.

[0026] In a first aspect, the present invention relates to a method for preparing an aqueous positive electrode slurry for a lithium iron phosphate battery, the preparation method comprising the following steps: (1) dry-mixing lithium iron phosphate powder with a conductive agent and a first portion of a thickener to obtain a mixed material; (2) adding water and a surfactant to the mixed material obtained in step (1), and then kneading and stirring to obtain a first mixed slurry with a solid content of 80 to 90 wt %; the surfactant is selected from at least one of 2-amino-2-methyl-1-propanol, styrene-acrylate copolymer and polyvinyl pyrrolidone (PVP); (3) dispersing water into the first mixed slurry obtained in step (2) to obtain a second mixed slurry with a solid content of 75 to 80 wt %; (4) dispersing the second portion of the thickener and water into the second mixed slurry obtained in step (3) to obtain a third mixed slurry with a solid content of 70 to 75 wt %; (5) dispersing an aqueous binder and water into the third mixed slurry obtained in step (4).

[0027] It should be noted that in the preparation method of the present invention, mixing is carried out according to specific steps, surfactants of the several substances are added in step (2), and the amount of the mixed materials is adjusted in steps (2) to (4) to control the solid content of the materials obtained in each step, and then through step (5) a stable and uniformly dispersed aqueous positive electrode slurry for lithium iron phosphate batteries can be prepared.

[0028] It should be noted that, in step (2), by adding a surfactant such as 2-amino-2-methyl-1-propanol, the wettability of the carbon-coated LFP and the conductive agent with water can be improved, which is conducive to the disaggregation of the carbon-coated LFP and the conductive agent agglomerates (the surfactant is distributed on the surface of the LFP and the conductive agent, forming ionic charge isolation and steric hindrance effects to prevent the LFP and the conductive agent from agglomerating). Therefore, the addition of the surfactant during the kneading stage of step (2) can improve the wettability of the LFP and the conductive agent with water, facilitate the disaggregation of the agglomerates, and facilitate the preparation of a water-based slurry with good dispersibility.

[0029] It should be noted that in the method for preparing the aqueous positive electrode slurry for lithium iron phosphate batteries of the present invention, a relatively high solid content is controlled in steps (2), (3) and (4), respectively, thereby reducing the effect of the poor wettability of lithium iron phosphate and the conductive agent with water on the positive electrode slurry, making the slurry dispersion in the prepared aqueous positive electrode slurry for lithium iron phosphate batteries more uniform, and improving the stability of the suspended slurry system.

[0030] According to a specific embodiment of the present invention, in step (1), the conductive agent is selected from at least one of carbon black, graphite, carbon nanotubes (CNTs) and carbon nanofibers (vapor grown carbon nanofibers, VGCF); the first part of the thickener in step (1) and the second part of the thickener in step (4) are independently selected from sodium carboxymethyl cellulose and / or lithium carboxymethyl cellulose; the aqueous binder in step (5) is selected from at least one of polyacrylic acid (PAA), styrene butadiene rubber (SBR) and polyacrylonitrile (PAN). The conductive agent can also be superconducting carbon black.

[0031] It should be noted that, in this specific embodiment, by selecting and using the above-mentioned conductive agent, thickener and aqueous binder, and mixing or stirring them according to the mixing order and solid content in steps (1)-(5), the final aqueous positive electrode slurry of the lithium iron phosphate battery is evenly dispersed and has good stability.

[0032] According to a specific embodiment of the present invention, in step (1), the lithium iron phosphate powder is micron-sized, submicron-sized or nano-sized carbon-coated lithium iron phosphate.

[0033] It should be noted that the carbon coating amount in the carbon-coated lithium iron phosphate can be 0.8-2%, based on the mass of the lithium iron phosphate. The lithium iron phosphate powder used in the present invention is a commercially available finished product powder.

[0034] According to a specific embodiment of the present invention, in step (1), in step (1), the lithium iron phosphate powder is 92 to 98 parts by weight, the conductive agent is 0.5 to 4 parts by weight, and the first part of the thickener is 30 to 60% of 0.5 to 2 parts by weight; the water added in step (2) is 10-30% of 33 to 150 parts by weight, and the surfactant is 0.2 to 2 parts by weight; the water added in step (3) is 5-20% of 33 to 150 parts by weight; the water added in step (4) is 5-20% of 33 to 150 parts by weight, and the second part of the thickener is 40 to 70% of 0.5 to 2 parts by weight; in step (5), the aqueous binder is 1 to 4 parts by weight, and the water added is 30-80% of 33 to 150 parts by weight.

[0035] It should be noted that, in this specific embodiment, the aqueous positive electrode slurry for lithium iron phosphate battery obtained by compounding the above-mentioned various raw materials according to the above-mentioned weight proportions and preparing according to the steps and conditions of (1)-(5) is uniformly dispersed and has good stability.

[0036] It should be noted that in the preparation method of the present invention, the thickener is added in two steps: 30% to 60% of the thickener is added in the dry mixing stage of step (1) to coat the surface of the LFP particles; and 40% to 70% of the thickener is added in the high-speed stirring stage of step (4) to be free in the slurry system to maintain the stability of the slurry system.

[0037] According to a specific embodiment of the present invention, in step (1), the dry mixing conditions include: carrying out the dry mixing in a mixer, with an orbital speed of 5-20 rpm, an autorotation speed of 10-300 rpm and a dry mixing time of 5 to 20 min.

[0038] According to a specific embodiment of the present invention, in step (2), the kneading and stirring conditions include: carrying out in a mixer, revolution 5-20 rpm, rotation 50-500 rpm, temperature 40-70° C. and kneading and stirring time 30-100 min.

[0039] According to a specific embodiment of the present invention, in step (3), the dispersing conditions include: carrying out in a mixer, revolution 5-20 rpm, rotation 10-800 rpm, temperature 40-70° C. and stirring time 30-75 min.

[0040] It should be noted that, as a preferred embodiment, the kneading stirring in step (2) and the dispersion stirring in step (3) are both carried out at a temperature of 40 to 70°C, that is, steps (2) and (3) are both carried out at a relatively high temperature, which can further improve the wetting problem of the carbon-containing material with water, so as to further improve the dispersion uniformity of the prepared aqueous positive electrode slurry.

[0041] According to a specific embodiment of the present invention, in step (4), the dispersion conditions include: carrying out in a blender, revolution 15-30 rpm, rotation 800-3000 rpm, temperature 30-45°C, vacuum degree -20--100 kPa and stirring time 60-180 min; in step (5), the dispersion conditions include: carrying out in a blender, revolution 15-30 rpm, rotation 500-3000 rpm, temperature 30-45°C, vacuum degree -20--100 kPa and stirring time 60-180 min.

[0042] It should be noted that specific control of the stirring in each step according to the above conditions can further improve the dispersion uniformity and stability of the positive electrode slurry. In particular, as a preferred embodiment, in step (2), the temperature of the stirring process is controlled at 40 to 70°C, in step (3), the temperature is 40 to 70°C, in step (4), the temperature is 30 to 45°C, and in step (5), the temperature is 30 to 45°C; in this way, the preparation method of the present invention solves the problems of difficult particle wetting, easy agglomeration, long dispersion time and unstable slurry suspension system of lithium iron phosphate aqueous positive electrode slurry by adding surfactants, thickeners and multi-step high viscosity (high solid content) and high temperature stirring, and can reduce the manufacturing cost of lithium iron phosphate batteries.

[0043] It should be noted that the temperature of the high-temperature kneading stage in step (2) and the high-temperature high-viscosity stirring in step (3) are both 40-70° C., which is beneficial to improving the wetting problem of lithium iron phosphate and water, and is also beneficial to the dissolution, coating and depolymerization of the thickener and surfactant.

[0044] According to a specific embodiment of the present invention, a lithium iron phosphate battery aqueous positive electrode slurry having a solid content of 40 to 70 wt% and a viscosity of 3000 to 15000 mPa·s is obtained through step (5). The lithium iron phosphate battery aqueous positive electrode slurry prepared by the preparation method of the present invention has good dispersion uniformity and stability.

[0045] In a second aspect, the present invention relates to an aqueous positive electrode slurry for a lithium iron phosphate battery, which is prepared by the preparation method.

[0046] In a third aspect, the present invention relates to a positive electrode sheet of a lithium iron phosphate battery, wherein a membrane in the positive electrode sheet is made of the aqueous positive electrode slurry of the lithium iron phosphate battery.

[0047] In a fourth aspect, the present invention relates to a lithium iron phosphate battery, wherein the positive electrode sheet in the lithium iron phosphate battery is the positive electrode sheet described above.

[0048] The present invention is further described in detail by way of examples. The reagents used in the following examples are all commercially available finished reagents. The lithium iron phosphate powder used in the following examples is nano-scale carbon-coated lithium iron phosphate.

[0049] Example 1

[0050] (1) 95 parts of LFP (lithium iron phosphate) powder, 1 part of carbon black conductive agent, and 0.5 parts of sodium carboxymethyl cellulose thickener are added into a double planetary mixer, and the mixer is dry-mixed at a revolution of 20 rpm, a rotation of 300 rpm, and a mixing time of 20 min to obtain a mixed material;

[0051] (2) adding 20 parts of deionized water and 1 part of 2-amino-2-methyl-1-propanol surfactant to the mixed material, and kneading and stirring at high temperature according to the parameters of revolution 20 rpm, rotation 500 rpm, temperature 60° C., and stirring time 80 min to obtain a first mixed slurry with a solid content of 83.0 wt %;

[0052] (3) adding 10 parts of deionized water to the first mixed slurry, and stirring the mixture at high temperature and high viscosity according to the parameters of revolution 20 rpm, rotation 500 rpm, temperature 60° C., and stirring time 40 min to obtain a second mixed slurry with a solid content of 76.5 wt %;

[0053] (4) adding the 10 parts of deionized water and 0.5 parts of sodium carboxymethyl cellulose thickener to the second mixed slurry, and stirring the mixture at a high speed of 20 rpm, 2000 rpm, 45° C., a vacuum degree of −90 kPa, and a stirring time of 120 min to obtain a third mixed slurry having a solid content of 71 wt %;

[0054] (5) Add the 2 parts of aqueous SBR (styrene-butadiene rubber) binder and 40 parts of deionized water to the third mixed slurry, and disperse and stir the mixture according to the following parameters: revolution 30 rpm, rotation 3000 rpm, temperature 30°C, vacuum degree -90 kPa, and stirring time 120 min, so as to obtain an aqueous positive electrode slurry with a solid content of 55.6±2% and a viscosity of 3000-15000 mpas.

[0055] Example 2

[0056] (1) 93 parts of LFP powder, 1 part of carbon black conductive agent, 1 part of carbon nanotube conductive agent, and 1 part of carboxymethyl cellulose lithium thickener were added into a double planetary mixer, and the mixer was dry mixed at a revolution of 10 rpm, a rotation of 200 rpm, and a mixing time of 10 min to obtain a mixed material;

[0057] (2) adding 15 parts of deionized water and 1.5 parts of PVP (polyvinyl pyrrolidone) surfactant to the mixed material, and kneading and stirring at high temperature according to the parameters of revolution 10 rpm, rotation 300 rpm, temperature 50° C., and stirring time 100 min to obtain a first mixed slurry with a solid content of 86.7 wt %;

[0058] (3) adding 11 parts of deionized water to the first mixed slurry, and stirring the mixture at high temperature and high viscosity according to the parameters of revolution 10 rpm, rotation 800 rpm, temperature 60° C., and stirring time 50 min to obtain a second mixed slurry with a solid content of 78.9 wt %;

[0059] (4) adding 8 parts of deionized water and 0.5 parts of lithium carboxymethyl cellulose thickener to the second mixed slurry, and stirring the mixture at a high speed of 10 rpm, 3000 rpm, 40° C., vacuum degree of −80 kPa, and 180 min to obtain a third mixed slurry having a solid content of 74.2 wt %;

[0060] (5) Add 1 part of PAA (polyacrylic acid), 1 part of SBR (styrene-butadiene rubber) aqueous binder and 25 parts of deionized water to the third mixed slurry, and disperse and stir the mixture at a revolution of 20 rpm, a rotation of 2500 rpm, a temperature of 35°C, a vacuum degree of -80 kPa, and a stirring time of 150 min to obtain an aqueous positive electrode slurry with a solid content of 62.9±2% and a viscosity of 3000-15000 mpas.

[0061] Example 3

[0062] (1) 92 parts of LFP powder, 2 parts of carbon black conductive agent, 1 part of VGCF (carbon nanofiber), and 0.5 parts of lithium carboxymethyl cellulose thickener were added into a double planetary mixer, and the mixer was dry mixed at a revolution of 15 rpm, a rotation of 250 rpm, and a mixing time of 15 min to obtain a mixed material;

[0063] (2) adding 14 parts of deionized water and 0.5 parts of a styrene-acrylate copolymer surfactant to the mixed material, and kneading and stirring the mixed material at high temperature according to the parameters of revolution 15 rpm, rotation 400 rpm, temperature 45° C., and stirring time 50 min, so as to obtain a first mixed slurry with a solid content of 87.3 wt %;

[0064] (3) adding 12 parts of deionized water to the first mixed slurry, and stirring the mixture at high temperature and high viscosity according to the parameters of revolution 15 rpm, rotation 700 rpm, temperature 45° C., and stirring time 60 min to obtain a second mixed slurry with a solid content of 78.7 wt %;

[0065] (4) adding 15 parts of deionized water and 1 part of lithium carboxymethyl cellulose thickener to the second mixed slurry, and stirring the mixture at a high speed of 15 rpm, 2500 rpm, 45° C., a vacuum degree of −70 kPa, and a stirring time of 160 min to obtain a third mixed slurry having a solid content of 70.3 wt %;

[0066] (5) Add 3 parts of aqueous PAN (polyacrylic acid) binder and 95 parts of deionized water to the third mixed slurry, and disperse and stir the mixture according to the parameters of revolution 15 rpm, rotation 2800 rpm, temperature 40°C, vacuum degree -70 kPa, and stirring time 160 min to obtain an aqueous positive electrode slurry with a solid content of 42.4±2% and a viscosity of 3000-15000 mpas.

[0067] Comparative Example 1

[0068] (1) 96.5 parts of LFP powder, 1.5 parts of carbon black conductive agent, and 2 parts of binder PVDF (polyvinylidene fluoride) were added into a double planetary mixer, and the mixer was dry mixed at a revolution of 15 rpm, a dispersion of 150 rpm, and a stirring time of 15 min to obtain a mixed material;

[0069] (2) adding 40 parts of NMP (N-methylpyrrolidone) to the mixed material, and kneading and stirring the mixed material at high temperature according to the parameters of revolution 15 rpm, rotation 300 rpm, temperature 45° C., and stirring time 50 min, so as to obtain a first mixed slurry with a solid content of 71.4 wt %;

[0070] (3) adding 40 parts of NMP (N-methylpyrrolidone) to the first mixed slurry, and stirring the mixture at high temperature and high viscosity according to the parameters of revolution 15 rpm, rotation 600 rpm, temperature 45° C., and stirring time 60 min to obtain a second mixed slurry with a solid content of 55.6 wt %;

[0071] (4) Add 8 parts of NMP (N-methylpyrrolidine) to the second mixed slurry, and stir the mixture at high speed according to the parameters of revolution 30 rpm, rotation 2500 rpm, temperature 45°C, vacuum degree -80 kPa, and stirring time 120 min to obtain an oil-based positive electrode slurry with a solid content of 53.2 wt ± 2% and a viscosity of 3000-15000 mpas.

[0072] Test Example 1

[0073] The viscosity of the water-based positive electrode slurry prepared in the above example and the oil-based positive electrode slurry prepared in the comparative example were tested, and the results are shown in the following Table 1:

[0074] Table 1

[0075] Example 1 Example 2 Example 3 Comparative Example 1 Viscosity mPa·s 9245 12125 4244 8542

[0076] The aqueous positive electrode slurry prepared in Example 1 has a solid content of 55.6±2% (the actual value is 55.8%) and a slurry viscosity of 9245 mPa·s;

[0077] The oil-based positive electrode slurry prepared in Comparative Example 1 has a solid content of 53.2±2% (the actual value is 53.5%) and a slurry viscosity of 8542 mPa·s;

[0078] It can be seen from the above data that the solid content and viscosity values ​​of the water-based positive electrode slurry prepared in the above embodiment and the oil-based positive electrode slurry prepared in the comparative example are both within the normal range, and the water-based slurry prepared in the above embodiment has good dispersibility.

[0079] The slurries prepared in the above examples and comparative examples were placed under the same conditions. The aqueous slurries prepared in the examples and the oil phase slurries prepared in the comparative examples were able to maintain substantially the same time without sedimentation, indicating that the aqueous slurries prepared in the examples had good stability. The viscosity of the slurry in Example 1 increased from 9245 mPa·s to 15326 mPa·s after being placed for 8 hours, and the viscosity of the slurry in Comparative Example 1 increased from 8542 mPa·s to 15468 mPa·s after being placed for 8 hours, both of which had relatively good static stability.

[0080] After the slurries prepared in the above-mentioned embodiment and comparative example were used as positive electrode slurries to combine with other positive electrode materials to make battery cells, it was found that the electrochemical performance parameters of the battery cells made of the water-based positive electrode slurry prepared in the embodiment and the battery cells made of the oily slurry in the comparative example were basically the same.

[0081] More importantly, compared with conventional oil-based positive electrode slurry, the water-based positive electrode slurry prepared in the embodiment of the present application uses low-cost water instead of the high-cost organic solvent NMP, while avoiding the environmental problems of NMP and the risk of explosion and flammability in the oven during the subsequent coating production process. While maintaining electrical properties, it can greatly reduce costs, improve safety and avoid environmental pollution.

[0082] In the description of the present application, it should be noted that the terms "upper", "lower", "inside", "outside", "front", "back", "left", "right", etc. indicate directions or positional relationships based on the directions or positional relationships in the working state of the present application. They are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific direction, be constructed and operated in a specific direction. Therefore, they should not be understood as limitations on the present application.

[0083] In the description of this application, it should be noted that, unless otherwise clearly specified and limited, the terms "install", "connect" and "connect" should be understood in a broad sense. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.

[0084] The present application has been described above in conjunction with preferred embodiments, but these embodiments are only exemplary and serve only as an illustration. On this basis, various replacements and improvements may be made to the present application, all of which fall within the scope of protection of the present application.

Claims

1. A method for preparing aqueous positive electrode slurry for lithium iron phosphate batteries, characterized in that: The preparation method comprises the following steps: (1) dry-mixing lithium iron phosphate powder, a conductive agent, and a first part of a thickener to obtain a mixed material; the lithium iron phosphate powder is micron-, submicron-, or nanometer-scale carbon-coated lithium iron phosphate; the lithium iron phosphate powder is 92 to 98 parts by weight, the conductive agent is 0.5 to 4 parts by weight, and the first part of a thickener is 30 to 60% of 0.5 to 2 parts by weight; (2) adding water and a surfactant to the mixed material obtained in step (1), and then kneading and stirring to obtain a first mixed slurry with a solid content of 80 to 90 wt %; the surfactant is selected from at least one of 2-amino-2-methyl-1-propanol, styrene-acrylate copolymer and polyvinyl pyrrolidone; the water added is 10 to 30% of 33 to 150 parts by weight, and the surfactant is 0.2 to 2 parts by weight; (3) dispersing water into the first mixed slurry obtained in step (2) to obtain a second mixed slurry with a solid content of 75-80 wt %; the amount of water added is 5-20% of 33-150 parts by weight; (4) dispersing the second part of thickener and water into the second mixed slurry obtained in step (3) to obtain a third mixed slurry with a solid content of 70-75 wt %; the added water is 5-20% of 33-150 parts by weight, and the second part of thickener is 0.5-2 parts by weight of 40-70%; (5) dispersing an aqueous binder and water into the third mixed slurry obtained from step (4); the aqueous binder is 1 to 4 parts by weight, and the added water is 30-80% of 33 to 150 parts by weight; After step (5), a lithium iron phosphate battery aqueous positive electrode slurry with a solid content of 40 to 70 wt% and a viscosity of 3000 to 15000 mPa·s is obtained.

2. The preparation method according to claim 1, characterized in that: In step (1), the conductive agent is selected from at least one of carbon black, graphite, carbon nanotubes and carbon nanofibers; the first part of the thickener in step (1) and the second part of the thickener in step (4) are each independently selected from sodium carboxymethyl cellulose and / or lithium carboxymethyl cellulose; and the aqueous binder in step (5) is selected from at least one of polyacrylic acid, styrene-butadiene rubber and polyacrylonitrile.

3. The preparation method according to claim 1, characterized in that: In step (1), the dry mixing conditions include: The mixture is mixed in a mixer at a revolution of 5-20 rpm and an autorotation of 10-300 rpm for 5-20 min.

4. The preparation method according to claim 1, characterized in that: In step (2), the kneading and stirring conditions include: The kneading and stirring is carried out in a mixer at a revolution of 5-20 rpm, a rotation of 50-500 rpm, a temperature of 40-70°C and a kneading and stirring time of 30-100 min.

5. The preparation method according to claim 1, characterized in that: In step (3), the dispersion conditions include: The mixture is prepared in a mixer at a revolution of 5-20 rpm, a rotation of 10-800 rpm, a temperature of 40-70°C and a stirring time of 30-75 min.

6. The preparation method according to claim 1, characterized in that: In step (4), the dispersion conditions include: The mixture is carried out in a mixer at a revolution of 15-30 rpm, a rotation of 800-3000 rpm, a temperature of 30-45°C, a vacuum degree of -20 to -100 kPa, and a stirring time of 60-180 min; In step (5), the dispersion conditions include: The stirring is carried out in a mixer at a revolution of 15-30 rpm, a rotation of 500-3000 rpm, a temperature of 30-45°C, a vacuum degree of -20 to -100 kPa and a stirring time of 60-180 min.

7. A lithium iron phosphate battery aqueous positive electrode slurry, characterized in that: The aqueous positive electrode slurry for lithium iron phosphate battery is prepared by the preparation method described in any one of claims 1 to 6.

8. A positive electrode sheet for a lithium iron phosphate battery, characterized in that: The membrane in the positive electrode sheet is made of the aqueous positive electrode slurry for lithium iron phosphate batteries as described in claim 7.

9. A lithium iron phosphate battery, characterized in that: The positive electrode sheet in the lithium iron phosphate battery is the positive electrode sheet described in claim 8.

Citation Information

Patent Citations

  • Lithium iron phosphate battery positive electrode pulp, lithium iron phosphate battery using positive electrode pulp and preparation method thereof

    CN101872856B

  • Aqueous cathode slurry of lithium iron phosphate battery and preparation method thereof

    CN112447969A

  • Method for doping graphene in lithium iron phosphate battery anode slurry

    CN104409729A

  • Lithium ion battery slurry, slurring merging process and lithium ion battery

    CN109524664A