A cathode system of a wet electrostatic precipitator

By using cathode wires made of fiberglass material, combined with specific lining resin formulation and structural design, the problems of high cost and complex installation of traditional cathode wires are solved, efficient and economical dust removal effects are achieved, and flame retardant performance is improved.

CN115582218BActive Publication Date: 2024-11-19FUJIAN HAOHUA ZHONGYI GFRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211261310.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-14
Publication Date
2024-11-19
Estimated Expiration
2042-10-14

AI Technical Summary

Technical Problem

The cathode line of traditional wet electrostatic precipitators is costly and needs to be fixed by heavy hammers, which is cumbersome to install and affects dust removal efficiency.

Method used

Using cathode wire made of fiberglass material, including inner lining, structural layer and outer protective layer, improves the mechanical properties and corrosion resistance of the cathode wire through specific inner lining resin formulation and structural design, and simplifies installation through a fixture The process eliminates the dependence on heavy hammers.

Benefits of technology

The cathode line cost is reduced by more than 60%, the mechanical strength and fatigue resistance are improved, the installation process is simplified, the dust removal efficiency and corrosion resistance are enhanced, and the flame retardant performance is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115582218B_ABST
    Figure CN115582218B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of wet electrostatic precipitators, and provides a cathode system of a wet electrostatic precipitator, which solves the problems of high cost and complicated installation of existing cathode wires. The cathode system includes a cathode wire and a fixing frame, and the cathode wire includes a cathode wire body, which is a hollow tube body, and the outer surface of the cathode wire body is provided with a plurality of grooves along the axial direction, and the outer surface of the cathode wire body is also provided with a spiral groove, and the spiral groove is connected with the groove, and a carbon fiber rope is provided in the spiral groove, and the cathode wire body includes an inner lining layer, a structural layer coated on the outer surface of the inner lining layer, and an outer protective layer coated on the outer surface of the structural layer, and the inner lining resin used in the inner lining layer is prepared by stirring and mixing an inner lining resin monomer, styrene, cobalt cyclohexane acid, methyl ethyl ketone peroxide, filler, and a leveling agent, and the inner lining resin monomer with a specific structure is synthesized through optimized design, so as to improve the strength and flame retardancy of the cathode wire body.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wet electrostatic precipitators, and in particular to a cathode system of a wet electrostatic precipitator. Background Art

[0002] Wet electrostatic precipitator is the mainstream equipment for reducing smoke emissions. It meets the environmental protection requirements of ultra-clean emissions in national purification projects and has become the preferred equipment for most thermal power stations or large thermal power plants in the country to reduce smoke indicators. The wet electrostatic precipitator is mainly composed of a shell, a cathode system, an anode system, a spray system, a high-voltage power supply, an insulation box and other equipment. The anode system usually uses a honeycomb anode tube. The working principle of the wet electrostatic precipitator is: the dust-containing flue gas passes through the anode tube in the dust collection area, and the cathode line discharges through high-voltage corona to produce a large number of negative ions and a small amount of positive ions. The dust particles entering the wet electrostatic precipitator with the flue gas collide with these positive and negative ions and become charged. The charged dust particles are captured by the anode system and then washed down by the spray system. After treatment, most of the dust in the flue gas is removed, thereby achieving ultra-clean emissions.

[0003] The cathode system is one of the important components of the wet electrostatic precipitator, which is directly related to the dust removal efficiency of the wet electrostatic precipitator. The cathode system mainly includes a cathode wire and a weight. For example, patent No. CN201820673374.3 discloses a barbed cathode wire and a weight structure for a wet electrostatic precipitator, including a barbed cathode wire, a double nut material strip, a bolt and a weight. The barbed cathode wire includes a cathode wire barb section and a cathode wire straight section; the cathode wire straight section is connected to the double hole material strip by bolts, and the double nut material strip is welded to the weight; the weight is a conical structure, the windward wedge angle α of the weight is 110-130°, and the leeward wedge angle β is 5-15°; the cathode wire barb section is a notch structure, and the ratio of the width H1 of the cathode wire barb to the spacing H2 between the two barbs is 1:1.5-1:2. When the airflow enters from the bottom of the hammer, the larger windward wedge angle effectively disperses the disturbance of the airflow hammer, while the smaller leeward wedge angle can prevent the condensation, attachment and accumulation of water mist; the notch barbs and their width ratio control reduce the condensation attachment of airflow water, while increasing the discharge effect. The barb wire is the most common structure of the cathode wire, in addition to the sawtooth wire, spiral wire, star wire, herringbone needle wire, etc. The barb wire belongs to point discharge, and its corona inception voltage is lower than that of other forms of cathode wire, and the discharge intensity is high. Moreover, the barb point is not easy to accumulate dust, and the dust removal efficiency is high, which is very suitable for occasions with high dust concentration. The material of the cathode wire is mainly stainless steel / lead antimony alloy / titanium alloy, etc. The 2205 stainless steel cathode wire has the advantages of high mechanical strength, not easy to break, easy to clean, low cost, simple processing, etc., and has now become the first choice of cathode wire material in the industry. If the cathode wire shakes, the distance between the cathode wire and the anode tube will change, and in severe cases, it will cause a short circuit in the electric field, affecting the efficient operation of the wet electrostatic precipitator. The main function of the heavy hammer in the cathode system is to stabilize the cathode wire and prevent it from shaking during operation.

[0004] Traditional cathode wires have the following problems: first, they are expensive and costly; second, external force (such as a heavy hammer) is required to tighten the cathode wire, otherwise it is easy to shake and discharge irregularly. Summary of the invention

[0005] Therefore, in view of the above, the present invention provides a cathode system for a wet electrostatic precipitator to solve the problems that the existing cathode wire has high cost, the bottom needs to be fixed by a heavy hammer, and the installation is relatively cumbersome.

[0006] To achieve the above object, the present invention is achieved through the following technical solutions:

[0007] A cathode system of a wet electrostatic precipitator, comprising a cathode wire and a fixing frame, the fixing frame comprising an upper fixing frame and a lower fixing frame, the upper fixing frame comprising a plurality of upper cross beams, the upper cross beams being arranged in parallel at equal intervals, upper support plates being arranged at the bottom of both sides of the upper cross beams, the upper support plates being perpendicularly intersecting the upper cross beams, the lower fixing frame comprising a plurality of lower cross beams, the lower cross beams being arranged in parallel at equal intervals, lower support plates being arranged at the bottom of both sides of the lower cross beams, the lower support plates being perpendicularly intersecting the lower cross beams, the cathode wire comprising a cathode wire body, the cathode wire body being a hollow tube body, the outer surface of the cathode wire body being provided with a plurality of grooves in an axial direction, the outer surface of the cathode wire body being further provided with a spiral groove, the spiral groove being connected with the groove, a carbon fiber rope being provided in the spiral groove, an upper connecting portion and a lower connecting portion being respectively provided at both ends of the cathode wire body, threads being arranged on the outer walls of the upper connecting portion and the lower connecting portion, the upper connecting portion and the lower connecting portion respectively passing through the upper cross beam and the lower cross beam and being fixedly connected by nuts;

[0008] The cathode line body comprises an inner lining layer, a structural layer coated on the outer surface of the inner lining layer, and an outer protective layer coated on the outer surface of the structural layer, wherein the inner lining layer comprises an inner lining layer, an inner lining middle layer, and an inner lining outer layer in order from the inside to the outside, wherein the inner lining layer is composited with an inner lining resin and a glass fiber surface felt, the inner lining middle layer is composited with an inner lining resin and a chopped strand felt, the inner lining outer layer is composited with an inner lining resin and an alkali-free glass fiber cloth, the structural layer is formed by winding a glass fiber roving impregnated with a structural resin on the outer surface of the inner lining layer, and the outer protective layer is a gel coat resin layer;

[0009] The lining resin is prepared by mixing lining resin monomer, styrene, cobalt naphthenate, methyl ethyl ketone peroxide, filler and leveling agent. The lining resin monomer is prepared according to the following steps:

[0010] (1) dissolving benzidine and an acid-binding agent in a reactor filled with tetrahydrofuran, then slowly adding acryloyl chloride dropwise at room temperature, continuing the reaction for 40 to 120 minutes after the addition is completed, filtering and extracting after the reaction is completed, and concentrating under reduced pressure to obtain intermediate A;

[0011] (2) dissolving intermediate A and alkyl dithiol in dimethylformamide solvent, then adding a photoinitiator to cause a thiol-ene click chemistry reaction under ultraviolet light to obtain intermediate B;

[0012] (3) Add epibromopropane into a reactor containing ethanol, adjust the pH value of the system to 8.0-9.0, dissolve the intermediate B in ethanol and slowly add it dropwise into the reactor at room temperature, and stir the reaction for 18-25 hours after the addition is completed to obtain the intermediate C;

[0013] (4) Add intermediate C and ethyl isocyanate acrylate into a reactor filled with tetrahydrofuran, and add hydroquinone and triethylamine, and react at 50-70° C. for 6-12 hours to obtain a lining resin monomer.

[0014] A further improvement is that the molar ratio of the benzidine, the acid binding agent and the acryloyl chloride is 1:2.0-2.5:2.4-3.

[0015] A further improvement is that the alkyl dithiol has 3 to 10 carbon atoms.

[0016] A further improvement is that the molar ratio of the intermediate A to the alkyl dithiol is 1:2.2-2.8.

[0017] A further improvement is that the photoinitiator is any one of benzoin ethyl ether, benzophenone, and 2-hydroxy-2-methyl-1-phenylacetone, and the added amount is 0.6-1.8% of the total mass of the intermediate A and the alkyl dithiol.

[0018] A further improvement is that the radiation intensity of the ultraviolet light is 600-800 mW / cm 2 The irradiation time is 3 to 6 minutes.

[0019] A further improvement is that the molar ratio of epibromohydrin to intermediate B is 1:0.35-0.45.

[0020] A further improvement is that the molar ratio of the intermediate C to ethyl isocyanate acrylate is 1:2.2-2.8.

[0021] A further improvement is that, based on 100% of the total mass of the intermediate C and ethyl isocyanate acrylate, the amount of hydroquinone added is 0.08-0.2%, and the amount of triethylamine added is 0.01-0.03%.

[0022] A further improvement is that the acid binding agent is any one of an inorganic base and an organic amine.

[0023] A further improvement is that the mass ratio of the lining resin monomer, styrene, cobalt cyclohexaneate, methyl ethyl ketone peroxide, filler and leveling agent is 55-75:16-25:0.4-0.8:2-4:10-30:0.1-0.3.

[0024] By adopting the above technical solution, the beneficial effects of the present invention are:

[0025] The cathode wire of the present invention adopts glass fiber reinforced plastic material, which has the characteristics of corrosion resistance, high strength, low deformation rate, excellent impact resistance and fatigue resistance, and solves the technical defects of cathode wires made of traditional stainless steel, lead-antimony alloy, titanium alloy and other materials, and the cost can be reduced by more than 60%. At the same time, the bottom of the cathode wire does not need to be tightened by a heavy hammer structure, which is more simple and efficient. Specifically, the cathode wire body includes an inner lining layer, a structural layer and an outer protective layer from the inside to the outside, and the inner lining layer includes an inner lining layer, an inner lining middle layer and an inner lining outer layer from the inside to the outside. The inner lining layer is composed of a composite of an inner lining resin and a glass fiber surface felt, the inner lining middle layer is composed of a composite of an inner lining resin and a chopped strand felt, the inner lining outer layer is composed of a composite of an inner lining resin and an alkali-free glass fiber cloth, and the structural layer is formed by winding a glass fiber roving impregnated with a structural resin on the outer surface of the inner lining layer. This structural design enables the cathode wire body to have excellent mechanical properties and corrosion resistance.

[0026] The present invention optimizes the formula design of the lining resin, takes benzidine as a raw material, first reacts with acryloyl chloride to generate an intermediate A containing an amide group, then the double bond of the intermediate A reacts with alkyl dithiol to undergo a thiol-ene click chemical reaction, introduces a thiol group into the molecular structure of the intermediate B, then reacts with epibromopropane to undergo a thiol-epoxy ring-opening reaction to generate an intermediate C containing a hydroxyl functional group, and finally reacts with ethyl isocyanate acrylate to undergo a nucleophilic addition reaction to generate a lining resin monomer. The lining resin monomer formed by the multi-step reaction contains a specific structure, and the lining resin formed by combining with other components can improve the strength of the glass fiber reinforced plastic, and compared with ordinary glass fiber reinforced plastic, the hoop tensile strength and axial tensile strength are greatly improved.

[0027] FRP materials generally use unsaturated polyester resin, epoxy resin, phenolic resin as the matrix, glass fiber or its products as the reinforcement material, and the prepared products have excellent performance in corrosion resistance and strength. However, the existing FRP materials produced by the above resins generally have the problem of poor flame retardancy, easy to burn and release a lot of smoke and heat, which limits its application range. In order to improve the flame retardancy of FRP materials, the common practice is to add flame retardants to the resin matrix. The inventors have overcome this inertial thinking, and through the adjustment and optimization of the monomer structure, introduced specific functional groups, and achieved excellent flame retardant effects without adding flame retardants. After analysis, the reasons for this effect may be: first, the lining resin monomer has good carbonization performance, can form a continuous and dense protective carbon layer, and effectively prevent the spread of flames; the biphenyl, ether bond, and amide bond introduced in the molecular structure significantly increase the carbonization rate of the resin, effectively reducing the smoke release amount and smoke release rate. Second, the monomer structure of the lining resin contains bromine, which produces a free radical scavenger, hydrogen bromide, when heated, which can reduce the concentration of free radicals generated when the resin burns and promote the continued rapid combustion of the resin. At the same time, bromine can also improve the charring property of the resin, achieving the purpose of flame retardancy. Third, biphenyl and bromine produce a synergistic flame retardant effect, achieving the technical effect of 1+1>2, and better improving the flame retardancy of the lining resin. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 is a schematic diagram of the overall structure of the cathode system provided in Example 4 of the present invention;

[0029] Figure 2 is a top view of a cathode system provided in Example 4 of the present invention;

[0030] Figure 3 yes Figure 1 A three-dimensional view of the cathode wire body;

[0031] Figure 4 yes Figure 3 Cross-sectional view at AA in the middle. DETAILED DESCRIPTION

[0032] The following will describe the implementation methods of the present invention in detail in conjunction with specific embodiments, so that the implementation process of how the present invention applies technical means to solve technical problems and achieve technical effects can be fully understood and implemented accordingly.

[0033] Unless otherwise specified, the technical means used in the examples are conventional means well known to those skilled in the art, and the reagents and products used are all commercially available. The sources, trade names and components of the reagents used are indicated when they first appear.

[0034] Example 1

[0035] A lining resin is prepared by mixing lining resin monomer, styrene, cobalt naphthenate, methyl ethyl ketone peroxide, white carbon black, and a leveling agent in a mass ratio of 55:16:0.4:2:10:0.1. The lining resin monomer is prepared according to the following steps:

[0036] (1) dissolving benzidine and triethylamine in a reactor filled with tetrahydrofuran, and then slowly adding acryloyl chloride dropwise at room temperature, wherein the molar ratio of benzidine, triethylamine and acryloyl chloride is 1:2.0:2.4. After the addition is completed, the reaction is continued for 40 minutes. After the reaction is completed, the mixture is filtered, concentrated under reduced pressure, and then ethyl acetate and water are added for extraction. The organic phase is taken, dried over anhydrous sodium sulfate, filtered, and finally concentrated under reduced pressure to obtain intermediate A;

[0037] (2) Dissolving intermediate A and 1,3-propanedithiol in dimethylformamide solvent, then adding benzoin ethyl ether, and causing a thiol-ene click chemistry reaction under ultraviolet light to obtain intermediate B;

[0038] The molar ratio of the intermediate A to 1,3-propanedithiol is 1:2.2, and the amount of benzoin ethyl ether added is 0.6% of the total mass of the intermediate A and 1,3-propanedithiol; the radiation intensity of the ultraviolet light is 600 mW / cm 2 , irradiation time is 6min;

[0039] (3) Add epibromopropane to a reactor containing ethanol, adjust the pH value of the system to 8.0-9.0, dissolve intermediate B in ethanol and slowly add it dropwise to the reactor at room temperature, wherein the molar ratio of epibromopropane to intermediate B is 1:0.35, and stir the reaction for 18 hours after the addition is completed to obtain intermediate C;

[0040] (4) adding intermediate C and ethyl isocyanate acrylate into a reactor filled with tetrahydrofuran, and adding hydroquinone and triethylamine, and reacting at 50° C. for 12 hours to obtain a lining resin monomer;

[0041] The molar ratio of the intermediate C to ethyl isocyanate acrylate is 1:2.2, the amount of hydroquinone added is 0.08% of the total mass of the intermediate C and ethyl isocyanate acrylate, and the amount of triethylamine added is 0.01% of the total mass of the intermediate C and ethyl isocyanate acrylate.

[0042] The test methods in GB / T2406-1993 and ISO5660 were used to test the oxygen index, heat release and smoke release of the lining resin obtained in this embodiment after curing. The test results showed that the oxygen index was 36.3%, the heat release was 64.1 MJ / m 2 , smoke release is 26.3m 3 / s.

[0043] Example 2

[0044] A lining resin is prepared by mixing lining resin monomer, styrene, cobalt naphthenate, methyl ethyl ketone peroxide, white carbon black, and a leveling agent in a mass ratio of 65:20:0.6:3:20:0.2. The lining resin monomer is prepared according to the following steps:

[0045] (1) dissolving benzidine and sodium hydroxide in a reactor filled with tetrahydrofuran, and then slowly adding acryloyl chloride dropwise at room temperature, wherein the molar ratio of benzidine, sodium hydroxide and acryloyl chloride is 1:2.2:2.7, and continuing the reaction for 80 minutes after the completion of the dropwise addition. After the completion of the reaction, filtering, extracting and concentrating under reduced pressure to obtain intermediate A;

[0046] (2) Dissolving intermediate A and 1,6-hexanedithiol in a dimethylformamide solvent, then adding benzophenone, and causing a thiol-ene click chemistry reaction under ultraviolet light to obtain intermediate B;

[0047] The molar ratio of the intermediate A to 1,6-hexanedithiol is 1:2.5, the amount of benzophenone added is 1.2% of the total mass of the intermediate A and 1,6-hexanedithiol, and the radiation intensity of the ultraviolet light is 700 mW / cm 2 , irradiation time is 5min;

[0048] (3) Add epibromopropane into a reactor containing ethanol, adjust the pH value of the system to 8.0-9.0, dissolve intermediate B in ethanol and slowly add it dropwise into the reactor at room temperature, wherein the molar ratio of epibromopropane to intermediate B is 1:0.4, and stir the reaction for 22 hours after the addition is completed to obtain intermediate C;

[0049] (4) adding intermediate C and ethyl isocyanate acrylate into a reactor filled with tetrahydrofuran, and adding hydroquinone and triethylamine, and reacting at 60° C. for 9 hours to obtain a lining resin monomer;

[0050] The molar ratio of the intermediate C to ethyl isocyanate acrylate is 1:2.5, the amount of hydroquinone added is 0.14% of the total mass of the intermediate C and ethyl isocyanate acrylate, and the amount of triethylamine added is 0.02% of the total mass of the intermediate C and ethyl isocyanate acrylate.

[0051] The oxygen index, heat release and smoke release of the lining resin obtained in this embodiment after curing were tested. The test results showed that the oxygen index was 37.7%, the heat release was 61.5 MJ / m 2 , smoke release is 24.1m 3 / s.

[0052] Example 3

[0053] A lining resin is prepared by mixing lining resin monomer, styrene, cobalt naphthenate, methyl ethyl ketone peroxide, white carbon black, and a leveling agent in a mass ratio of 75:25:0.8:4:30:0.3. The lining resin monomer is prepared according to the following steps:

[0054] (1) dissolving benzidine and an acid-binding agent in a reactor filled with tetrahydrofuran, and then slowly dropping acryloyl chloride at room temperature, wherein the molar ratio of benzidine, triethylamine, and acryloyl chloride is 1:2.5:3, and continuing the reaction for 120 minutes after the completion of the dropwise addition. After the completion of the reaction, filtering, extracting, and concentrating under reduced pressure obtain an intermediate A;

[0055] (2) dissolving intermediate A and 1,10-decanedithiol in a dimethylformamide solvent, then adding 2-hydroxy-2-methyl-1-phenylacetone, and causing a thiol-ene click chemistry reaction under ultraviolet light to obtain intermediate B;

[0056] The molar ratio of the intermediate A to 1,10-decanedithiol is 1:2.8, the amount of 2-hydroxy-2-methyl-1-phenylacetone added is 1.8% of the total mass of the intermediate A and 1,10-decanedithiol, and the radiation intensity of the ultraviolet light is 800 mW / cm 2 , irradiation time is 3min;

[0057] (3) Add epibromopropane into a reactor containing ethanol, adjust the pH value of the system to 8.0-9.0, dissolve intermediate B in ethanol and slowly add it dropwise into the reactor at room temperature, wherein the molar ratio of epibromopropane to intermediate B is 1:0.45, and stir the reaction for 25 hours after the addition is completed to obtain intermediate C;

[0058] (4) adding intermediate C and ethyl isocyanate acrylate into a reactor filled with tetrahydrofuran, and adding hydroquinone and triethylamine, and reacting at 70° C. for 6 hours to obtain a lining resin monomer;

[0059] The molar ratio of the intermediate C to ethyl isocyanate acrylate is 1:2.8, the amount of hydroquinone added is 0.2% of the total mass of the intermediate C and ethyl isocyanate acrylate, and the amount of triethylamine added is 0.03% of the total mass of the intermediate C and ethyl isocyanate acrylate.

[0060] The oxygen index, heat release and smoke release of the lining resin obtained in this embodiment after curing were tested. The test results showed that the oxygen index was 36.9%, the heat release was 62.8 MJ / m 2 , smoke release is 25.0m 3 / s.

[0061] Comparative Example 1

[0062] The difference from Example 1 is that the lining resin monomer is replaced with a commercially available unsaturated polyester resin.

[0063] The oxygen index, heat release and smoke release of the lining resin obtained in this comparative example after curing were tested. The test results showed that the oxygen index was 21.6%, the heat release was 95.9 MJ / m 2 , smoke release is 42.1m 3 / s.

[0064] Comparative Example 2

[0065] The difference from Example 1 is that the raw material benzidine for synthesizing the lining resin monomer is replaced by p-phenylenediamine.

[0066] The oxygen index, heat release and smoke release of the lining resin obtained in this comparative example after curing were tested. The test results showed that the oxygen index was 27.4%, the heat release was 81.0 MJ / m 2 , smoke release is 33.5m 3 / s.

[0067] Comparative Example 3

[0068] The difference from Example 1 is that the raw material epibromopropane for synthesizing the lining resin monomer is replaced by propylene oxide.

[0069] The oxygen index, heat release and smoke release of the lining resin obtained in this comparative example after curing were tested. The test results showed that the oxygen index was 29.2%, the heat release was 77.3 MJ / m 2 , smoke release is 31.6m 3 / s.

[0070] Comparative Example 4

[0071] The difference from Example 1 is that the raw material benzidine for synthesizing the lining resin monomer is replaced by 1,3,5-tri(4-aminophenyl)benzene, and the raw material epibromopropane is replaced by propylene oxide.

[0072] The oxygen index, heat release and smoke release of the lining resin obtained in this comparative example after curing were tested. The test results showed that the oxygen index was 30.3%, the heat release was 75.5 MJ / m 2 , smoke release is 30.7m 3 / s.

[0073] Comparative Example 5

[0074] The difference from Example 1 is that the raw material benzidine for synthesizing the lining resin monomer is replaced by p-phenylenediamine, and the raw material epibromopropane is replaced by 3,4-dibromo-1,2-epoxy-butane.

[0075] The oxygen index, heat release and smoke release of the lining resin obtained in this comparative example after curing were tested. The test results showed that the oxygen index was 28.7%, the heat release was 78.4 MJ / m 2 , smoke release is 32.2m 3 / s.

[0076] It can be seen from the above test results that compared with the commonly used lining resins in existing FRP, the lining resins prepared in Examples 1 to 3 have good flame retardancy, showing a higher oxygen index, lower heat release and smoke release performance. Combining Example 1 and Comparative Examples 2 to 3, it can be seen that there is a synergistic promotion effect between the biphenyl group and the bromine element, which improves the flame retardant effect. Replacing the biphenyl group or the bromine group in the lining resin monomer significantly deteriorates the flame retardancy; while lacking one of the functional groups in the phenyl group or the bromine group and increasing the content of the other functional group, the improvement in flame retardancy is limited, which is far inferior to the flame retardancy of the lining resin in Example 1.

[0077] Example 4

[0078] refer to Figures 1 to 4 A cathode system of a wet electrostatic precipitator, comprising a cathode line and a fixing frame, wherein the fixing frame comprises an upper fixing frame and a lower fixing frame, wherein the upper fixing frame comprises a plurality of upper beams 1, wherein the upper beams 1 are arranged in parallel at equal intervals, and upper support plates 2 are arranged at the bottom of both sides of the upper beams 1, wherein the upper support plates 2 intersect the upper beams 1 perpendicularly, wherein the lower fixing frame comprises a plurality of lower beams 3, wherein the lower beams 3 are arranged in parallel at equal intervals, and lower support plates 4 are arranged at the bottom of both sides of the lower beams 3, wherein the lower support plates 4 intersect the lower beams 3 perpendicularly, wherein the cathode line comprises a cathode line body 5, wherein the cathode line body 5 is a hollow structure The outer surface of the cathode wire body 5 is provided with a plurality of grooves 6 along the axial direction, and the outer surface of the cathode wire body is also provided with a spiral groove (not shown in the figure), the spiral groove is connected with the groove 6, the depth of the spiral groove is the same as the depth of the groove 6, a carbon fiber rope 7 is provided in the spiral groove, the thickness of the carbon fiber rope 7 is greater than the depth of the spiral groove, and the two ends of the cathode wire body 5 are respectively provided with an upper connecting part 8 and a lower connecting part 9, the outer walls of the upper connecting part 8 and the lower connecting part 9 are provided with threads, and the upper connecting part 8 and the lower connecting part 9 respectively pass through the upper crossbeam and the lower crossbeam and are fixedly connected by nuts 10;

[0079] The cathode line body 5 includes an inner lining layer, a structural layer 11 coated on the outer surface of the inner lining layer, and an outer protective layer 12 coated on the outer surface of the structural layer 11. The inner lining layer includes an inner lining layer 13, an inner lining middle layer 14, and an inner lining outer layer 15 from the inside to the outside. The inner lining layer 13 is composited with an inner lining resin and a glass fiber surface felt. The inner lining middle layer 14 is composited with an inner lining resin and a chopped strand felt. The inner lining outer layer 15 is composited with an inner lining resin and an alkali-free glass fiber cloth. The structural layer 11 is formed by winding a glass fiber roving impregnated with a structural resin on the outer surface of the inner lining layer. The outer protective layer 12 is a gel coat resin layer. The depth of the groove 6 does not exceed the thickness of the outer protective layer.

[0080] The lining resin is the lining resin prepared in Example 1, the structural resin is prepared using unsaturated polyester resin as the main raw material, and the gel coat resin layer is prepared using gel coat resin as the main raw material. This is a well-known technology, and specific details can be found in patent application number 202110183143.0.

[0081] Mechanical properties of the cathode wire body prepared in this embodiment were tested, and the test results were as follows: the circumferential tensile strength was 308 MPa, and the axial tensile strength was 164 MPa.

[0082] The cathode wire body was prepared by using the lining resin described in Example 2, and the mechanical properties were tested. The test results were as follows: the hoop tensile strength was 309 MPa, and the axial tensile strength was 162 MPa.

[0083] The cathode wire body was prepared by using the lining resin described in Example 3, and the mechanical properties were tested. The test results were as follows: the hoop tensile strength was 306 MPa, and the axial tensile strength was 160 MPa.

[0084] The cathode wire body was prepared by using the lining resin described in Comparative Example 1, and the mechanical properties were tested. The test results were as follows: the hoop tensile strength was 279 MPa, and the axial tensile strength was 146 MPa.

[0085] The above records are only embodiments of the present invention. Any modification or change made by a person familiar with the present technology using the present invention shall fall within the patent scope claimed by the present invention and shall not be limited to those disclosed in the embodiments.

Claims

1. A cathode system of a wet electrostatic precipitator, comprising a cathode line and a fixing frame, characterized in that: The fixing frame comprises an upper fixing frame and a lower fixing frame, the upper fixing frame comprises a plurality of upper cross beams, the upper cross beams are arranged in parallel with equal intervals, upper support plates are arranged at the bottom of both sides of the upper cross beam, the upper support plates are perpendicularly intersected with the upper cross beam, the lower fixing frame comprises a plurality of lower cross beams, the lower cross beams are arranged in parallel with equal intervals, lower support plates are arranged at the bottom of both sides of the lower cross beam, the lower support plates are perpendicularly intersected with the lower cross beam, the cathode wire comprises a cathode wire body, the cathode wire body is a tube body with a hollow structure, a plurality of grooves are arranged along the axial direction on the outer surface of the cathode wire body, a spiral groove is also arranged on the outer surface of the cathode wire body, the spiral groove is connected with the groove, a carbon fiber rope is arranged in the spiral groove, an upper connecting part and a lower connecting part are respectively arranged at both ends of the cathode wire body, threads are arranged on the outer walls of the upper connecting part and the lower connecting part, the upper connecting part and the lower connecting part respectively pass through the upper cross beam and the lower cross beam and are fixedly connected by nuts; The cathode line body comprises an inner lining layer, a structural layer coated on the outer surface of the inner lining layer, and an outer protective layer coated on the outer surface of the structural layer, wherein the inner lining layer comprises an inner lining layer, an inner lining middle layer, and an inner lining outer layer in order from the inside to the outside, wherein the inner lining layer is composited with an inner lining resin and a glass fiber surface felt, the inner lining middle layer is composited with an inner lining resin and a chopped strand felt, the inner lining outer layer is composited with an inner lining resin and an alkali-free glass fiber cloth, the structural layer is formed by winding a glass fiber roving impregnated with a structural resin on the outer surface of the inner lining layer, and the outer protective layer is a gel coat resin layer; The lining resin is prepared by mixing lining resin monomer, styrene, cobalt naphthenate, methyl ethyl ketone peroxide, filler and leveling agent. The lining resin monomer is prepared according to the following steps: (1) dissolving benzidine and an acid-binding agent in a reactor filled with tetrahydrofuran, then slowly adding acryloyl chloride dropwise at room temperature, continuing the reaction for 40 to 120 minutes after the addition is completed, filtering and extracting after the reaction is completed, and concentrating under reduced pressure to obtain intermediate A; (2) dissolving intermediate A and alkyl dithiol in dimethylformamide solvent, then adding a photoinitiator to cause a thiol-ene click chemistry reaction under ultraviolet light to obtain intermediate B; (3) Add epibromopropane into a reactor containing ethanol, adjust the pH value of the system to 8.0-9.0, dissolve the intermediate B in ethanol and slowly add it dropwise into the reactor at room temperature, and stir the reaction for 18-25 hours after the addition is completed to obtain the intermediate C; (4) Add intermediate C and ethyl isocyanate acrylate into a reactor filled with tetrahydrofuran, and add hydroquinone and triethylamine, and react at 50-70° C. for 6-12 hours to obtain a lining resin monomer.

2. The cathode system of a wet electrostatic precipitator according to claim 1, characterized in that: The molar ratio of the benzidine, the acid binding agent and the acryloyl chloride is 1:2.0-2.5:2.4-3.

3. The cathode system of a wet electrostatic precipitator according to claim 1, characterized in that: The alkyl dithiol has 3 to 10 carbon atoms.

4. The cathode system of a wet electrostatic precipitator according to claim 1, characterized in that: The molar ratio of the intermediate A to the alkyl dithiol is 1:2.2-2.

8.

5. The cathode system of a wet electrostatic precipitator according to claim 1, characterized in that: The photoinitiator is any one of benzoin ethyl ether, benzophenone and 2-hydroxy-2-methyl-1-phenylacetone, and the added amount is 0.6-1.8% of the total mass of the intermediate A and the alkyl dithiol.

6. The cathode system of a wet electrostatic precipitator according to claim 1, characterized in that: The radiation intensity of the ultraviolet light is 600-800 mW / cm 2 The irradiation time is 3 to 6 minutes.

7. The cathode system of a wet electrostatic precipitator according to claim 1, characterized in that: The molar ratio of epibromopropane to intermediate B is 1:0.35-0.

45.

8. The cathode system of a wet electrostatic precipitator according to claim 1, characterized in that: The molar ratio of the intermediate C to ethyl isocyanate acrylate is 1:2.2-2.

8.

9. The cathode system of a wet electrostatic precipitator according to claim 1, characterized in that: Based on 100% of the total mass of the intermediate C and ethyl isocyanate acrylate, the added amount of the hydroquinone is 0.08-0.2%, and the added amount of the triethylamine is 0.01-0.03%.

10. The cathode system of a wet electrostatic precipitator according to claim 1, characterized in that: The mass ratio of the lining resin monomer, styrene, cobalt cyclohexane acid, methyl ethyl ketone peroxide, filler and leveling agent is 55-75:16-25:0.4-0.8:2-4:10-30:0.1-0.3.