A method for preparing high-purity tellurium by seed crystal seeding

By using a seed crystal to guide the growth of tellurium crystals in a graphite boat, and performing multiple seedings and zone melting in a reducing atmosphere, the existing technology for preparing high-purity tellurium has solved the complicated operation, high risk of contamination, and low efficiency of impurity removal. problem, achieving the preparation and cost reduction of high-purity tellurium.

CN115584556BActive Publication Date: 2024-10-15CENT SOUTH UNIV
View PDF 0 Cites -1 Cited by

Patent Information

Application Number
CN202211124135.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-15
Publication Date
2024-10-15
Estimated Expiration
2042-09-15

Smart Images

  • Figure CN115584556B_ABST
    Figure CN115584556B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for preparing high-purity tellurium by seed crystal seeding, the method comprising the following steps: (1) loading tellurium raw material into a graphite boat, placing a seed crystal at the head of the graphite boat, loading into a zone melting furnace, and adjusting the furnace to a reducing atmosphere; (2) seeding; (3) zone melting; (4) repeating steps (2) and (3) 8 to 12 times, cooling to room temperature, taking out a high-purity tellurium sample, and cutting and processing to obtain high-purity tellurium. The present invention uses seed crystals to guide the growth of tellurium crystals, so that the gap distribution in the tellurium raw material is more uniform, and the diffusion environment of impurities in the tellurium raw material during the zone melting process is improved, thereby improving the impurity removal efficiency of the zone melting process. The seeding process of the present invention is carried out under reducing closed conditions, and the zone melting operation is directly carried out after seeding, so the risk of secondary pollution is small, the product purity is high, and the product purity reaches the 7N tellurium standard.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of semi-metal preparation, and in particular to a method for preparing high-purity tellurium by adopting seed crystal seeding. Background Art

[0002] Tellurium is a semimetal with obvious metallic properties and is widely used in the fields of light, electricity, and heat. For example, CdTe is one of the most important solar cell materials, HgCdTe, ZnCdTe, and PbSnTe are important raw materials for the preparation of infrared materials and thermal imagers, and BiTe and PbTe are good functional materials that can convert heat energy and electrical energy into each other. The purity of tellurium directly affects the performance of the material. Even trace impurities can cause the photoelectric performance of the material to deteriorate. Therefore, the purification of tellurium is of great significance.

[0003] The preparation methods of high-purity tellurium include chemical methods and physical methods. Chemical methods include aqueous solution reduction, electrolysis, extraction, etc. Physical methods include vacuum distillation, zone melting, and Czochralski purification. Tellurium is a low melting point and high vapor pressure element. In theory, vacuum distillation can effectively separate most impurities in tellurium and obtain distilled tellurium with high purity. However, practice has shown that the vacuum distillation purification effect of tellurium is not ideal. The resistivity of the materials prepared by the Czochralski purification method is uneven, and the quartz container will contaminate the melt at high temperature. The operation process is relatively cumbersome, so it is rarely used in practice. The process of zone melting is simple to operate, and the product purity is high and uniform, so it is widely used in the final process of high-purity metal preparation. However, the impurity removal efficiency of zone melting technology is low, and improving the zone melting efficiency is the current research focus. For example, non-metallic impurities in tellurium such as N, P, S, etc., and impurities Se with properties similar to Te are generally treated by electromigration or vacuum distillation. The removal efficiency of traditional zone melting is low. During the zone melting process, the crystals in the crystallization process meet the coherence. Therefore, seed crystals are used to induce crystal growth and improve the conditions for impurity diffusion during the zone melting process to improve the impurity mobility. This is beneficial to improving the impurity mobility during the zone melting process.

[0004] Chinese patent CN110894065A discloses an apparatus and method for preparing high-purity tellurium. The method is used to produce 6N high-purity tellurium. The technology includes a vacuum distillation device, a vacuum pumping device, a hydrogen purification circulation device, a high-frequency induction heating device and a product collection device. The combination of the technology and equipment is complex and the operation difficulty coefficient is high, which is not conducive to industrial production.

[0005] Chinese invention patent CN111924811A discloses a method for preparing ultra-high purity tellurium. A quartz container with a baffle inside is used to heat the raw tellurium to complete melting under a protective atmosphere. The impurities of carbon powder and oxides contained in the raw tellurium are intercepted on one side of the baffle, and the impurity content of the tellurium melt on the other side is reduced. After condensation, it is used to prepare ultra-high purity tellurium. 7N high-purity tellurium can be obtained by zone melting the purified tellurium multiple times. The above technical solution can obtain a tellurium product with high purity, but the pretreatment of the raw materials is relatively cumbersome, the risk of secondary pollution during operation is relatively high, and the energy consumption is high.

[0006] Chinese invention patent CN103183322B provides a method for preparing high-purity tellurium, which places the tellurium raw material in a quartz boat, performs zone melting in a reducing atmosphere, removes the head and tail after completing one zone melting, and performs the next zone melting. Repeating this cycle several times can obtain 6N5 high-purity tellurium. The impurity removal process of this method is relatively complicated, and new impurities are easily introduced during the operation process, resulting in poor impurity removal effect; at the same time, its production cost is high, which is not conducive to large-scale production.

[0007] Therefore, there is currently a lack of a method for preparing high-purity tellurium with a simple process and without introducing new impurities. Summary of the invention

[0008] The technical problem to be solved by the present invention is to overcome the deficiencies and defects mentioned in the above background technology and provide a method for preparing high-purity tellurium by using seed crystal seeding.

[0009] In order to solve the above technical problems, the technical solution proposed by the present invention is:

[0010] A method for preparing high-purity tellurium by seeding, the method comprising the following steps:

[0011] (1) Loading tellurium raw materials into a graphite boat, placing seed crystals at the head of the graphite boat, loading the boat into a zone melting furnace, and adjusting the furnace to a reducing atmosphere;

[0012] (2) seeding;

[0013] (3) performing zone melting;

[0014] (4) Repeat steps (2) and (3) 8 to 12 times, cool to room temperature, take out the high-purity tellurium sample, and cut and process to obtain high-purity tellurium.

[0015] In actual crystals, particles (atoms, molecules, etc.) can be arranged in an infinite number of ways in three-dimensional space. The arrangement of atoms in metals is within the range of several atoms, which is basically consistent with the arrangement of solids, forming ordered atomic groups. The atoms within a single atomic group are arranged regularly, and there are differences between multiple atomic groups, and the atoms are arranged disorderly. Under normal circumstances, polycrystalline metals are formed after melting, and they are still polycrystalline after recrystallization. The anisotropy of polycrystalline metals is caused by the different densities of atoms arranged in various directions, which further leads to the disordered arrangement of atomic gaps, increases the migration and diffusion resistance of impurities during zone melting, and when impurities migrate from liquid phase to solid phase, the migration of impurities is affected by resistance, thereby reducing the removal efficiency of impurities. In addition, for volatile impurities such as Se, P, S, since the reducing gas can only contact the surface of the raw material, it has limited effect on the removal of impurities inside the raw material. Strengthening the migration process of such impurities in tellurium and allowing them to quickly migrate to the surface of the raw material to interact with the reducing gas is beneficial to improving their removal rate. To solve this problem and improve the impurity removal efficiency during the zone melting process, the coherence of the metal crystallization process is used to place isotropic seed crystals at the front end of the tellurium raw material to guide the crystallization of the tellurium zone melting process, reduce the resistance of the impurity migration process during the zone melting, and effectively improve the impurity removal efficiency. At the same time, seeding in a reducing atmosphere can simultaneously reduce the gas element impurities present in the tellurium raw material lattice, so as to improve the overall removal efficiency of the gas element impurities during the zone melting process.

[0016] The principle of impurity migration is as follows Figure 1 As shown, A is the initial state; B is the zone melting process; and C is the final state after zone melting.

[0017] The irregular arrangement of atoms in polycrystalline tellurium raw materials increases the diffusion resistance of impurities. For example, impurity 1 in the figure is in a relatively closed gap, and it is difficult to migrate; impurities 2 and 3 are in relatively open gaps and can migrate well in the solid and liquid phases. In actual crystals, atoms can be arranged in an infinite number of ways in three-dimensional space. Different arrangements of atoms affect the gaps between atoms in the crystal, and these gaps have an important influence on the diffusion of impurity atoms in the metal. Using seed crystals to seed polycrystalline tellurium raw materials can make the gap distribution in the tellurium raw materials more uniform, thereby promoting the diffusion of impurities and improving the efficiency of regional melting and impurity removal.

[0018] Preferably, the step (1) of adjusting the furnace to a reducing atmosphere comprises: passing an inert gas through the sealed furnace body for 15 to 30 minutes at a flow rate of 5.0 to 7.0 L / min to fully exhaust the air in the system, and then passing a reducing gas through the sealed furnace body for 60 to 90 minutes at a flow rate of 2.0 to 4.0 L / min.

[0019] Preferably, the tellurium raw material in step (1) has a purity of 5N or more and a mass of 4.0-6.0 kg; and the height of the tellurium raw material in the graphite boat is controlled to account for 60-80% of the total height of the graphite boat.

[0020] Preferably, the purity of the seed crystal in step (1) is above 7N, and the ash content of the graphite boat is less than 3 ppm.

[0021] Preferably, the seeding temperature in step (2) is controlled to be 650-700° C., and the seeding rate is controlled to be 0.1-0.3 mm / min.

[0022] Preferably, the zone melting in step (3) includes a heating stage, a heat preservation stage, and a cooling stage, specifically: in the heating stage, a reducing gas with a flow rate of 0.2 to 0.5 L / min is introduced to heat up, and when the temperature rises to 500 to 600°C, the reducing gas flow rate is controlled to 5.0 to 7.0 L / min, and the temperature continues to rise; in the heat preservation stage, the reducing gas flow rate is controlled to 5.0 to 7.0 L / min, and the zone melting is carried out from the head direction to the tail end of the graphite boat, the melting zone movement rate is controlled to 0.3 to 0.6 mm / min, the temperature is maintained at 650 to 700°C, and the melting zone width is controlled to 40 to 70 mm; after the heat preservation is completed, the temperature is cooled, and when the temperature drops below 500°C, the reducing gas flow rate is reduced to 0.2 to 0.5 L / min.

[0023] Preferably, after cooling to room temperature in step (4), an inert gas is passed for 15 to 30 minutes to fully discharge the reducing gas H2 in the system at a flow rate of 5.0 to 7.0 L / min, and a high-purity tellurium sample is taken out.

[0024] Preferably, the cutting process in step (4) is to cut off 3% to 6% of the front end of the high-purity tellurium sample and 8% to 12% of the rear end.

[0025] Preferably, the inert gas is N2 or Ar with a purity of 7N or above, and the reducing gas is H2 with a purity of 7N or above.

[0026] Preferably, the H2 tail gas that has not reacted completely during the zone melting process is treated with a torch ignition device to prevent explosion at the tail gas outlet due to excessive hydrogen concentration.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] (1) The present invention uses seed crystals to guide the growth of tellurium crystals, making the gap distribution in the tellurium raw material more uniform, improving the diffusion environment of impurities in the tellurium raw material during the zone melting process, thereby improving the impurity removal efficiency during the zone melting process. The seeding process of the present invention is carried out under reducing closed conditions, and the zone melting operation is directly carried out after seeding, with a small risk of secondary pollution and high product purity. The impurity Se can be reduced to less than 20 ppb, the impurities such as Al, Mg, Ca, Pb, and Zn can be reduced to less than 5.0 ppb, and the impurities such as Cd, Ga, and Cu can be reduced to less than 1.0 ppb, and the product purity reaches the 7N tellurium standard.

[0029] (2) Before the reducing gas is introduced, the present invention first introduces an inert gas to fully exhaust the air in the system. On the one hand, this can prevent the oxidation of the raw material tellurium by O2 in the air; on the other hand, it can prevent the explosion caused by the instability of the reducing gas and O2 when mixed, thereby improving the safety of the system. During the heating and cooling process of the system, the reducing gas flow rate is reduced, the reducing gas consumption is reduced, and the production cost is reduced.

[0030] (3) The present invention uses a hydrogen tail gas ignition device to treat the H2 that has not reacted completely during the test process, thereby improving the overall safety of the system. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0032] Figure 1 Schematic diagram of impurity migration during zone melting.

[0033] In the figure: 1, impurity 1; 2, impurity 2; 3, impurity 3. DETAILED DESCRIPTION

[0034] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and preferred embodiments of the present invention, but the protection scope of the present invention is not limited to the following specific embodiments.

[0035] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0036] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0037] Embodiment 1:

[0038] (1) Load 4.6 kg of tellurium raw material into a graphite boat. The raw material composition is shown in Table 1, and the raw material purity is 5N4; place a seed crystal at the head of the graphite boat, load it into the zone melting furnace, and seal it. (2) Pass N2 for 20 minutes, control the flow rate to 5.5 L / min, and fully exhaust the air in the system. (3) Pass H2 for 60 minutes, control the flow rate to 2.0 L / min, control the seeding temperature to 650°C, and the seeding rate to 0.3 mm / min. (4) Directly zone melt the tellurium raw material after seeding, which includes three stages: heating stage, insulation stage, and cooling stage. 1) Heating stage: control the H2 flow rate to 0.2 L / min. When the temperature rises to 500°C, control the H2 flow rate to 5.0 L / min and continue to heat up. 2) Insulation stage: The insulation process is the main impurity removal stage, the H2 flow rate is controlled at 5.0L / min, the melting zone movement rate is controlled at 0.6mm / min, the temperature is maintained at 670℃, and the melting zone width is controlled at 50mm. 3) Cooling stage: After the insulation is completed and the temperature drops below 500℃, the H2 flow rate is reduced to 0.2L / min; the heater returns to the original point.

[0039] During the test, the flare ignition device was kept in the open state to ensure that the unreacted H2 tail gas could be fully treated.

[0040] Repeat the operation 8 times, cool to room temperature after zone melting, pass N2 for 15 minutes, and the flow rate is 5.0L / min. Take the sample out of the graphite boat, and cut off 10cm at the head and tail ends. Take samples in the middle high-purity area and do GDMS detection. The test results are shown in Table 2. The contents of impurities not listed in the table are all below the detection limit of the GDMS instrument, and the total amount is less than 10ppb. The product purity reaches 7N.

[0041] Table 1 Raw material test results (ppb)

[0042]

[0043] Table 2 Product test results (ppb)

[0044]

[0045] Example 2

[0046] (1) Load 5.5 kg of tellurium raw material into a graphite boat. The raw material composition is shown in Table 3, and the raw material purity is 5N5; place a seed crystal at the head of the graphite boat, load it into the zone melting furnace, and seal it. (2) Pass N2 for 25 minutes, control the flow rate to 6.0 L / min, and fully exhaust the air in the system. (3) Pass H2 for 90 minutes, control the flow rate to 4.0 L / min, control the seeding temperature to 650°C, and the seeding rate to 0.1 mm / min. (4) Directly zone melt the tellurium raw material after seeding, which includes three stages: heating stage, insulation stage, and cooling stage. 1) Heating stage: control the H2 flow rate to 0.2 L / min. When the temperature rises to 500°C, control the H2 flow rate to 7.0 L / min and continue to heat up. 2) Insulation stage: The insulation process is the main impurity removal stage, the H2 flow rate is controlled at 7.0L / min, the melting zone movement rate is controlled at 0.3mm / min, the temperature is maintained at 700℃, and the melting zone width is controlled at 60mm. 3) Cooling stage: After the insulation is completed, when the temperature drops below 500℃, the H2 flow rate is reduced to 0.2L / min; the heater returns to the original point.

[0047] During the test, the flare ignition device was kept in the open state to ensure that the unreacted H2 tail gas could be fully treated.

[0048] Repeat the operation 12 times, cool to room temperature after zone melting, pass N2 for 15 minutes, and the flow rate is 5.0L / min. Take the sample out of the graphite boat, and cut off 10cm at the head and tail ends. Take samples in the middle high-purity area and do GDMS detection. The test results are shown in Table 4. The contents of impurities not listed in the table are all below the detection limit of the GDMS instrument, and the total amount is less than 10ppb. The product purity reaches 7N3.

[0049] Table 3 Raw material test results (ppb)

[0050]

[0051] Table 4 Product test results (ppb)

[0052]

[0053] Comparative Example 1

[0054] As a comparative example of Example 1, this example does not use seeding, and becomes a melting process with the same conditions, including three processes: sample loading, atmosphere control and heat preservation.

[0055] (1) Load 4.8 kg of tellurium raw material into a graphite boat. The raw material composition is shown in Table 5, and the raw material purity is 5N3; load it into the zone melting furnace and seal it. (2) Pass N2 for 20 minutes, control the flow rate to 5.5 L / min, and fully exhaust the air in the system. (3) Pass H2 for 60 minutes, control the flow rate to 2.0 L / min, control the seeding temperature to 650°C, and the seeding rate to 0.3 mm / min. (4) Directly zone melt the tellurium raw material after the melt, which includes three stages: heating stage, insulation stage, and cooling stage. 1) Heating stage: control the H2 flow rate to 0.2 L / min. When the temperature rises to 500°C, control the H2 flow rate to 5.0 L / min and continue to heat up. 2) Insulation stage: The insulation process is the main impurity removal stage, the H2 flow rate is controlled at 5.0L / min, the melting zone movement rate is controlled at 0.6mm / min, the temperature is maintained at 670℃, and the melting zone width is controlled at 50mm. 3) Cooling stage: After the insulation is completed and the temperature drops below 500℃, the H2 flow rate is reduced to 0.2L / min; the heater returns to the original point.

[0056] During the test, the flare ignition device was kept in the open state to ensure that the unreacted H2 tail gas could be fully treated.

[0057] Repeat the operation 8 times. After the zone melting is completed, cool to room temperature and pass N2 for 15 minutes at a flow rate of 5.0L / min. Take the sample out of the graphite boat and cut off 10cm at the head and tail ends. Take samples in the middle high-purity area and perform GDMS detection. The test results are shown in Table 6. The contents of impurities not listed in the table are all below the detection limit of the GDMS instrument, and the product purity reaches 6N7.

[0058] Table 5 Raw material test results (ppb)

[0059]

[0060]

[0061] Table 6 Product test results (ppb)

[0062]

Claims

1. A method for preparing high-purity tellurium by seeding, characterized in that: The method comprises the following steps: (1) Load tellurium raw materials into a graphite boat, place seed crystals at the head of the graphite boat, load it into the zone melting furnace, and adjust the furnace to a reducing atmosphere; (2) seeding; in step (2), the seeding temperature is controlled to be 650-700°C, and the seeding rate is controlled to be 0.1-0.3 mm / min; (3) performing zone melting; the zone melting includes a heating stage, a heat preservation stage, and a cooling stage, specifically: in the heating stage, a reducing gas with a flow rate of 0.2-0.5 L / min is introduced to increase the temperature. When the temperature rises to 500-600°C, the reducing gas flow rate is controlled to 5.0-7.0 L / min, and the temperature continues to rise; in the heat preservation stage, the reducing gas flow rate is controlled to 5.0-7.0 L / min, and zone melting is performed along the direction of the head of the graphite boat toward the tail end. The moving rate of the melting zone is controlled to 0.3-0.6 mm / min, the temperature is maintained at 650-700°C, and the width of the melting zone is controlled to 40-70 mm; after the heat preservation is completed, the temperature is cooled. When the temperature drops below 500°C, the reducing gas flow rate is reduced to 0.2 L / min; (4) Repeat steps (2) and (3) 8 to 12 times, cool to room temperature, take out the high-purity tellurium sample, and cut and process to obtain high-purity tellurium.

2. The method for preparing high-purity tellurium by seed crystal seeding according to claim 1, characterized in that: The step (1) of adjusting the furnace to a reducing atmosphere is as follows: the sealing area of ​​the furnace body is passed through an inert gas for 15 to 30 minutes at a flow rate of 5.0 to 7.0 L / min to fully exhaust the air in the system, and then the reducing gas is passed through for 60 to 90 minutes at a flow rate of 2.0 to 4.0 L / min.

3. The method for preparing high-purity tellurium by seed crystal seeding according to claim 1, characterized in that: The tellurium raw material in step (1) has a purity of 5N or more and a mass of 4.0-6.0 kg; the height of the tellurium raw material in the graphite boat is controlled to account for 60-80% of the total height of the graphite boat.

4. The method for preparing high-purity tellurium by seed crystal seeding according to claim 1, characterized in that: The purity of the seed crystal in step (1) is above 7N, and the ash content of the graphite boat is less than 3 ppm.

5. The method for preparing high-purity tellurium by seed crystal seeding according to claim 1, characterized in that: After cooling to room temperature as described in step (4), an inert gas is passed for 15 to 30 minutes at a flow rate of 5.0 to 7.0 L / min, and a high-purity tellurium sample is taken out.

6. The method for preparing high-purity tellurium by seeding with seed crystals according to claim 1, characterized in that: The cutting process described in step (4) is to cut off 3% to 6% of the front end of the high-purity tellurium sample and 8% to 12% of the rear end.

7. The method for preparing high-purity tellurium by seed crystal seeding according to claim 2 or 5, characterized in that: The inert gas is N2 or Ar with a purity of 7N or more, and the reducing gas is H2 with a purity of 7N or more.