A argon arc welding wire for 5Cr-0.5Mo high temperature resistant steel and its preparation method and use method

By optimizing the chemical composition and welding process of 5Cr-0.5Mo steel welding wire, cracks and corrosion problems during welding are solved, and the high-temperature crack resistance and corrosion resistance of the welding interface are improved, ensuring the reliability of the welded joints and the parent material Close mechanical properties.

CN115609187BActive Publication Date: 2024-11-05HARBIN WELL WELDING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211377073.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-04
Publication Date
2024-11-05
Estimated Expiration
2042-11-04

AI Technical Summary

Technical Problem

5%Cr-0.5%Mo steel is prone to cracks and corrosion problems during welding. The existing welding materials are difficult to meet their needs for crack resistance and corrosion resistance at high temperatures, and carbon lean and carbon-enhancing belts caused by carbon migration after welding. It affects the mechanical properties of the welding interface.

Method used

Provide a 5Cr-0.5Mo high-temperature resistant steel argon arc welding wire, whose chemical composition is optimized and contains appropriate amounts of C, Si, Mn, Cr, Mo, Ni, Ti, V and Cu, etc., to improve the resistance of the welding wire through heat treatment. Cracking, corrosion resistance and high temperature resistance, and welding process under argon protection is adopted to control welding parameters.

Benefits of technology

It significantly improves the crack resistance and corrosion resistance of the welding interface, reduces the occurrence of cold cracks, the structure and chemical composition of the welded joints are close to the base material, optimizes the mechanical properties, avoids carbon migration problems, and improves the reliability and use of welding. life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003927130280000081
    Figure BDA0003927130280000081
  • Figure BDA0003927130280000082
    Figure BDA0003927130280000082
  • Figure BDA0003927130280000091
    Figure BDA0003927130280000091
Patent Text Reader

Abstract

The invention discloses an argon arc welding wire for 5Cr-0.5Mo high temperature resistant steel and a preparation method and a use method thereof, belonging to the technical field of welding materials and preparation thereof. The chemical composition of the welding wire of the invention comprises, by weight percentage, C: 0.06-0.09%, Si: 0.20-0.50%, Mn: 0.40-0.70%, Cr: 5.00-6.00%, Mo: 0.45-0.65%, Cu: 0.10-0.20%, Ni: 0.10-0.40%, Ti: 0.01-0.05%, V: 0.01-0.03%, O≤0.005%, N≤0.010%, and the remainder is Fe and unavoidable impurities. The welding wire is suitable for argon arc welding, and its welding joint has the same organization and extremely similar chemical composition as the parent material, and can obtain mechanical properties similar to the parent material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an argon arc welding wire for 5Cr-0.5Mo high temperature resistant steel and a preparation method and a use method thereof, belonging to the technical field of welding materials and preparation methods thereof. Background Art

[0002] 5%Cr-0.5%Mo (5Cr-0.5Mo) steel is a chromium-molybdenum heat-resistant steel with high oxidation resistance and thermal strength. Its working temperature is as high as 600℃. It is widely used in steam turbines, thermal power plants, nuclear power plants, petroleum refining and other high-temperature equipment, especially large-scale oil refining and chemical plants. Most crude oil is high-sulfur crude oil, which has obvious corrosion to pipeline equipment. Existing carbon steel and low-alloy steel can no longer meet the needs of corrosion resistance of process equipment and pipelines in high-sulfur crude oil processing plants. 5%Cr-0.5%Mo steel is often used in large-scale oil refining and chemical plants and transportation pipelines due to its high resistance to high-temperature oxidation, high-temperature sulfur corrosion, hydrogen and certain cyclohexane acid corrosion. It is especially widely used in refining and chemical plants such as atmospheric and vacuum, coking, and catalysis.

[0003] However, due to the high Cr content in 5%Cr-0.5%Mo steel, the material has high hardenability and poor welding performance. During the equipment manufacturing and construction process, problems such as cracking of the base material and weld or excessive hardness are prone to occur, which poses a great safety hazard to the operation of the device. After welding, the heat-affected zone of 5%Cr-0.5%Mo steel is prone to form hardened structure, and at the same time, it is easy to form cold cracks due to the combined effects of hydrogen, residual stress and other factors. Therefore, the research on the welding performance of 5%Cr-0.5%Mo steel is one of the hot topics that people are currently concerned about.

[0004] The existing technology uses a new type of low-chromium high-manganese austenitic welding material to weld 5%Cr-0.5%Mo steel, and obtains relatively satisfactory results. However, the chemical composition of the weld metal and the base material are different during heterogeneous welding, and the physical and mechanical properties are also different. After long-term service at high temperatures, carbon migration and changes in the carbide structure will occur on the welding interface. Carbon migration causes the appearance of carbon-poor bands and carbon-enriched bands on both sides of the fusion line. The strength of the carbon-poor band decreases, the hardness of the carbon-enriched band increases, and the toughness decreases or low-temperature brittleness occurs. Therefore, it is very necessary to provide a welding wire suitable for 5%Cr-0.5%Mo high-temperature resistant steel to make it have the characteristics of crack resistance, corrosion resistance, and high temperature resistance. Summary of the invention

[0005] In order to solve the above problems existing in the prior art, the present invention provides a welding wire for argon arc welding of 5% Cr-0.5% Mo steel which has the characteristics of crack resistance, corrosion resistance and high temperature resistance and is suitable for use in steam turbines, thermal power stations, nuclear power plants, petroleum refining and other high-temperature equipment.

[0006] The technical solution of the present invention:

[0007] One of the purposes of the present invention is to provide an argon arc welding wire for 5Cr-0.5Mo high temperature resistant steel. The chemical composition of the welding wire, measured by weight percentage, includes: C: 0.06-0.09%, Si: 0.20-0.50%, Mn: 0.40-0.70%, S≤0.005%, P≤0.006%, Cr: 5.00-6.00%, Mo: 0.45-0.65%, Cu: 0.10-0.20%, Ni: 0.10-0.40%, Ti: 0.01-0.05%, V: 0.01-0.03%, As≤0.005%, Sn≤0.005%, Pb≤0.003%, O≤0.005%, N≤0.010%, and the balance is Fe and unavoidable impurities.

[0008] In the invention, the chemical composition range of 5Cr-0.5Mo high temperature resistant steel argon arc welding wire is set for the following reasons:

[0009] C: 0.06-0.09%; The increase of carbon content increases the strength and hardness of carbon steel, but reduces the plasticity, toughness and welding performance. As a high alloy steel for heat resistance at high temperature, the carbon content should be greater than or equal to 0.04%, but the corrosion resistance will decrease at this time. Therefore, the carbon content must be strictly controlled. Therefore, the C content in the present invention is 0.06%-0.09%.

[0010] Ni: 0.10-0.40%; Ni is a commonly used element for obtaining excellent low-temperature toughness. It strengthens ferrite and refines and increases pearlite, improves the strength of steel, and has little effect on the plasticity of steel. It can improve hardenability, promote the formation of acicular ferrite, improve the strength and toughness of welds, especially medium and low temperature impact toughness, and reduce the tough-brittle transition temperature. The carbon content of nickel-containing steel can be appropriately reduced, thereby improving toughness and plasticity. Nickel does not increase the creep resistance of steel, so it is generally not used as a strengthening element in heat-resistant steel. Nickel is an element with a certain corrosion resistance, and has a certain corrosion resistance to acids, alkalis, salts and atmosphere. Therefore, the Ni content in the present invention is 0.10%-0.40%.

[0011] V: 0.01-0.03%; Vanadium has a strong affinity with carbon, ammonia and oxygen, and forms corresponding stable compounds with them. Vanadium exists mainly in the form of carbides in steel. Its main function is to refine the structure and grains of steel and improve the strength and toughness of steel. When dissolved into solid solution at high temperature, it increases hardenability; Vanadium can refine grains in ordinary low-carbon alloy steel, improve the strength and yield ratio after normalizing and low-temperature characteristics, and improve the welding performance of steel. Therefore, the V content in the present invention is 0.01%-0.03%.

[0012] Cu: 0.10-0.20%; The prominent role of Cu in steel is to improve the corrosion resistance of ordinary low alloy steel. Adding copper can also improve the strength of steel, and at the same time it has the effect of refining grains and significantly improving low temperature impact toughness. When the copper content exceeds 0.75%, after solution treatment and aging, it can produce an aging strengthening effect. When the content is low, its effect is similar to that of nickel, but weaker. When the content is high, it may cause copper brittleness and brittle fracture. Therefore, the Cu content in the present invention is 0.10%-0.20%, which can not only ensure low temperature impact performance, but also improve corrosion resistance.

[0013] Ti: 0.01-0.05%; Ti is the strongest carbide-forming element, and has a strong affinity with nitrogen and oxygen. It is a good degasser and an effective element for fixing nitrogen and carbon. Since titanium can fix carbon, it can prevent and reduce stress corrosion of materials. Titanium can improve the oxidation resistance and thermal strength of heat-resistant steel. As a strong carbide-forming element, titanium can improve the stability of steel in high temperature, high pressure and hydrogen. Therefore, the Ti content in the present invention is 0.01%-0.05%.

[0014] S, P, O, N: Sulfur and oxygen as impurity elements often exist in carbon steel in the form of non-metallic compounds (such as FeS, FeO), forming non-metallic impurities, which leads to the deterioration of material properties, especially the presence of sulfur causes the hot brittleness of the material. Sulfur and phosphorus are elements to be controlled in steel, and the quality of carbon steel is evaluated by their content. Therefore, in the present invention, the O content is ≤0.005%, the N content is ≤0.010%, the S content is ≤0.005, and the P content is ≤0.006.

[0015] As, Sn, Pb: As impurity elements, they have a certain effect on improving the tensile strength of carbon steel, but at the same time they all increase the brittleness of steel, especially low-temperature brittleness. Harmful elements that cause serious segregation of carbon steel. It is not good for the weldability of steel and can increase the sensitivity of weld cracks. Since low-alloy steel has a high melting point, impurity elements are easy to migrate and aggregate at high temperatures, resulting in high-temperature temper brittleness of low-alloy steel. Therefore, in the present invention, the As content is ≤0.005%; the Sn content is ≤0.005, and the Pb content is ≤0.003.

[0016] It is further defined that the chemical composition of the welding wire, by weight percentage, includes: C: 0.06-0.09%, Si: 0.20-0.40%, Mn: 0.40-0.70%, S≤0.005%, P≤0.006%, Cr: 5.00-6.00%, Mo: 0.45-0.65%, Cu: 0.10-0.20%, Ni: 0.10-0.40%, Ti: 0.01-0.05%, V: 0.01-0.03%, As≤0.005%, Sn≤0.005%, Pb≤0.003%, O≤0.005%, N≤0.010%, and the balance is Fe and unavoidable impurities.

[0017] It is further defined that the chemical composition of the welding wire, by weight percentage, includes: C: 0.09%, Si: 0.30%, Mn: 0.65%, S: 0.0018%, P: 0.0049%, Cr: 5.15%, Mo: 0.51%, Cu: 0.19%, Ni: 0.25%, Ti: 0.020%, V: 0.02%, O: 0.0046%, N: 0.0092%, and the balance is Fe and unavoidable impurities.

[0018] It is further defined that the chemical composition of the welding wire, by weight percentage, includes: C: 0.08%, Si: 0.25%, Mn: 0.65%, S: 0.0022%, P: 0.0060%, Cr: 5.02%, Mo: 0.51%, Cu: 0.15%, Ni: 0.20%, Ti: 0.024%, V: 0.01%, O: 0.0049%, N: 0.0091%, and the balance is Fe and unavoidable impurities.

[0019] It is further defined that the chemical composition of the welding wire, by weight percentage, includes: C: 0.09%, Si: 0.28%, Mn: 0.60%, S: 0.0041%, P: 0.0044%, Cr: 5.01%, Mo: 0.51%, Cu: 0.15%, Ni: 0.19%, Ti: 0.029%, V: 0.02%, O: 0.0049%, N: 0.0094%, and the balance is Fe and unavoidable impurities.

[0020] It is further defined that the chemical composition of the welding wire, by weight percentage, includes: C: 0.08%, Si: 0.33%, Mn: 0.61%, S: 0.0022%, P: 0.0048%, Cr: 5.24%, Mo: 0.49%, Cu: 0.18%, Ni: 0.25%, Ti: 0.022%, V: 0.01%, O: 0.0046%, N: 0.0091%, and the balance is Fe and unavoidable impurities.

[0021] It is further defined that the chemical composition of the welding wire, by weight percentage, includes: C: 0.08%, Si: 0.25%, Mn: 0.59%, S: 0.0031%, P: 0.0052%, Cr: 5.12%, Mo: 0.53%, Cu: 0.17%, Ni: 0.23%, Ti: 0.022%, V: 0.02%, O: 0.0047%, N: 0.0093%, and the balance is Fe and unavoidable impurities.

[0022] It is further defined that after heat treatment at 745°C for 1 to 8 hours, the room temperature tensile strength of the deposited metal of the welding wire is ≥550MPa, the room temperature yield strength is ≥470MPa, the elongation after fracture is ≥17%, the yield strength at 600°C is ≥179MPa, the impact energy Akv at -30°C is 100J or more, and the impact energy Akv at room temperature is 200J or more.

[0023] The second object of the present invention is to provide a method for preparing the above-mentioned argon arc welding wire for 5Cr-0.5Mo high temperature resistant steel, specifically, weighing each component in proportion, smelting in a 0.5t electric furnace, and then forging, drawing and copper plating in sequence, processing into a welding wire with a diameter of Φ2.4mm, and then straightening and cutting the wire, the specification of which is Φ2.4×1000mm.

[0024] The second object of the present invention is to provide a method for using the above-mentioned argon arc welding wire for 5Cr-0.5Mo high temperature resistant steel. Specifically, under argon protection, the welding parameters are: welding voltage 13~15V, welding current 180A, welding speed 50~100mm / min, interpass temperature 200~250℃, and shielding gas flow rate 13~18L / min.

[0025] The welding wire component design and mechanism of action of the present invention is to affect the weld structure and performance by adding strengthening alloy elements, and solve the crack resistance, corrosion resistance and high temperature resistance of the material by designing the composition control of C, Si, S, P, Cr, Mo, Ni, Ti and O, N content. Specifically, the present invention significantly improves the low-temperature impact toughness by adding V, Ti, and Ni elements, and improves the crack resistance of the welding material by controlling the content of elements such as C, Si, Mn, O, and N, and reduces the tendency of welding cold cracks. The corrosion resistance and high temperature resistance of the material are improved by controlling the proportion of elements such as Cr, Ni, Mo, V and Ti, and it is found through experiments that the technology has made significant progress. Compared with the prior art, the present application also has the following beneficial effects:

[0026] (1) Performance in the control of cold cracks. The main alloying elements chromium and molybdenum in 5%Cr-0.5%Mo steel can significantly improve the hardening tendency of steel. From the organizational state diagram of chromium steel, it can be seen that when the chromium content is 5% to 10% and the carbon content is above 0.1%, the organization of the steel under isothermal heat treatment is hardened martensite. This makes it easy for the heat-affected zone of the steel to form a hardened organization after welding. At the same time, it is easy to form cold cracks due to the combined action of factors such as hydrogen and residual stress. Therefore, the present application improves the crack resistance of the welding material by controlling the content of elements such as C, Si, Mn, O, and N in the welding wire. In addition, TIG welding has great advantages compared with other welding methods, and through the control of the welding process, preheating is required before welding and heat treatment is performed after welding, which solves the problem of welding cold cracks. The welding wire provided by the present invention is suitable for argon arc welding, and its welded joint has the same organization and extremely similar chemical composition as the parent material, and can obtain mechanical properties similar to the parent material. There is no obvious problem of alloy element diffusion and carbon migration during use.

[0027] (2) Performance in terms of corrosion resistance and high temperature resistance. Corrosion is a key factor affecting the reliability and service life of petrochemical equipment. At present, high-temperature oxidation, hydrogen corrosion, sulfur corrosion, hydrogen sulfide corrosion and organic acid corrosion are the main causes of damage to petrochemical pipelines and refining equipment. The 5% Cr-0.5% Mo steel matching argon arc welding wire provided by the present invention has a higher Cr and Mo content. During the oxidation process, Cr is preferentially oxidized than Fe and can form a dense oxide film on the surface, which can prevent oxygen from diffusing into the interior. At high temperatures, Cr and Mo form a Cr-Mo alloy with high high-temperature oxidation resistance. At the same time, Cr and Mo elements can also effectively prevent H from reacting with C to generate CH4 and causing embrittlement. The hydrogen sulfide corrosion of low-alloy steel is controlled by two major factors: anodic dissolution and the formation of corrosion products on the steel surface. The corrosion of carbon steel in a salt solution containing hydrogen sulfide is divided into two stages: the electron transfer process between the corrosion product and the iron matrix and the electron transfer process in the corrosion product film of iron. In addition, the failure behavior is closely related to the chemical composition, microstructure, density and hydrogen traps. It is generally believed that tempered martensitic Cr-Mo steel has good resistance to hydrogen sulfide stress corrosion cracking. Therefore, a good corrosion film can be formed by optimizing the design of the components to improve the anti-sulfur performance. However, the prior art believes that the addition of copper can change the electrochemical behavior of steel, and the dissolution behavior of the steel matrix and carbides in the hydrogen sulfide medium is an important factor affecting the anti-hydrogen sulfide corrosion performance, and the corrosion mechanism of this material in the hydrogen sulfide medium is proposed. However, the present invention significantly improves the corrosion resistance by adding Cu and Ti elements, and the technical progress is obvious. DETAILED DESCRIPTION

[0028] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0029] The experimental methods used in the following examples are conventional methods unless otherwise specified. The materials, reagents, methods and instruments used are conventional materials, reagents, methods and instruments in the art unless otherwise specified, and can be obtained through commercial channels by those skilled in the art.

[0030] The compositions of the welding wires in all the embodiments of the present invention are listed in Table 1, and the mechanical properties of the deposited metals of the welding wires are listed in Table 2.

[0031] Embodiment 1:

[0032] The composition of the welding wire of this embodiment is shown in the data corresponding to Embodiment 1 in Table 1;

[0033] The specific chemical composition of the welding wire, by weight percentage, includes: C: 0.09%, Si: 0.30%, Mn: 0.65%, S: 0.0018%, P: 0.0049%, Cr: 5.15%, Mo: 0.51%, Cu: 0.19%, Ni: 0.25%, Ti: 0.020%, V: 0.02%, O: 0.0046%, N: 0.0092%, and the balance is Fe and unavoidable impurities.

[0034] The preparation method of the welding wire is as follows: weigh each component in proportion, smelt the welding wire in a 0.5t electric furnace, forge and draw the welding wire and copper plate it, then process it into a welding wire with a diameter of Φ2.4mm and straighten and cut it into a wire specification of Φ2.4×1000mm.

[0035] The obtained welding wire was heat treated at 745℃ for 1h, and the mechanical properties of the deposited metal of the welding wire were tested. The results are shown in Table 2.

[0036] After heat treatment at 745℃ for 1h, the welding wire meets the engineering application requirements of 5%Cr-0.5%Mo heat-resistant steel.

[0037] The method of welding 5% Cr-0.5% Mo high temperature resistant steel using the above welding wire is to perform welding under argon protection, wherein the welding parameters are: welding voltage 13-15V, welding current 180A, welding speed 50-100mm / min, interpass temperature 200-250°C, and shielding gas flow rate 13-18L / min.

[0038] Embodiment 2:

[0039] The composition of the welding wire of this embodiment is shown in the data corresponding to Embodiment 2 in Table 1;

[0040] The specific chemical composition of the welding wire, by weight percentage, includes: C: 0.08%, Si: 0.25%, Mn: 0.65%, S: 0.0022%, P: 0.0060%, Cr: 5.02%, Mo: 0.51%, Cu: 0.15%, Ni: 0.20%, Ti: 0.024%, V: 0.01%, O: 0.0049%, N: 0.0091%, and the balance is Fe and unavoidable impurities.

[0041] The preparation method of the welding wire is as follows: weigh each component in proportion, smelt the welding wire in a 0.5t electric furnace, forge and draw the welding wire and copper plate it, then process it into a welding wire with a diameter of Φ2.4mm and straighten and cut it into a wire specification of Φ2.4×1000mm.

[0042] The obtained welding wire was heat treated at 745℃ for 1h, and the mechanical properties of the deposited metal of the welding wire were tested. The results are shown in Table 2.

[0043] The method of welding 5% Cr-0.5% Mo high temperature resistant steel using the above welding wire is to perform welding under argon protection, wherein the welding parameters are: welding voltage 13-15V, welding current 180A, welding speed 50-100mm / min, interpass temperature 200-250°C, and shielding gas flow rate 13-18L / min.

[0044] Embodiment 3:

[0045] The composition of the welding wire of this embodiment is shown in the data corresponding to Embodiment 3 in Table 1;

[0046] The specific chemical composition of the welding wire, by weight percentage, includes: C: 0.09%, Si: 0.28%, Mn: 0.60%, S: 0.0041%, P: 0.0044%, Cr: 5.01%, Mo: 0.51%, Cu: 0.15%, Ni: 0.19%, Ti: 0.029%, V: 0.02%, O: 0.0049%, N: 0.0094%, and the balance is Fe and unavoidable impurities.

[0047] The preparation method of the welding wire is as follows: weigh each component in proportion, smelt the welding wire in a 0.5t electric furnace, forge and draw the welding wire and copper plate it, then process it into a welding wire with a diameter of Φ2.4mm and straighten and cut it into a wire specification of Φ2.4×1000mm.

[0048] The obtained welding wire was heat treated at 745℃ for 1h, and the mechanical properties of the deposited metal of the welding wire were tested. The results are shown in Table 2.

[0049] The method of welding 5% Cr-0.5% Mo high temperature resistant steel using the above welding wire is to perform welding under argon protection, wherein the welding parameters are: welding voltage 13-15V, welding current 180A, welding speed 50-100mm / min, interpass temperature 200-250°C, and shielding gas flow rate 13-18L / min.

[0050] Embodiment 4:

[0051] The composition of the welding wire of this embodiment is shown in the data corresponding to Example 4 in Table 1;

[0052] The specific chemical composition of the welding wire, measured by weight percentage, includes: C: 0.08%, Si: 0.33%, Mn: 0.61%, S: 0.0022%, P: 0.0048%, Cr: 5.24%, Mo: 0.49%, Cu: 0.18%, Ni: 0.25%, Ti: 0.022%, V: 0.01%, O: 0.0046%, N: 0.0091%, and the balance is Fe and unavoidable impurities.

[0053] The preparation method of the welding wire is as follows: weigh each component in proportion, smelt the welding wire in a 0.5t electric furnace, forge and draw the welding wire and copper plate it, then process it into a welding wire with a diameter of Φ2.4mm and straighten and cut it into a wire specification of Φ2.4×1000mm.

[0054] The obtained welding wire was heat treated at 745℃ for 1h, and the mechanical properties of the deposited metal of the welding wire were tested. The results are shown in Table 2.

[0055] The method of welding 5% Cr-0.5% Mo high temperature resistant steel using the above welding wire is to perform welding under argon protection, wherein the welding parameters are: welding voltage 13-15V, welding current 180A, welding speed 50-100mm / min, interpass temperature 200-250°C, and shielding gas flow rate 13-18L / min.

[0056] Embodiment 5:

[0057] The composition of the welding wire of this embodiment is shown in the data corresponding to Example 5 in Table 1;

[0058] The specific chemical composition of the welding wire, by weight percentage, includes: C: 0.08%, Si: 0.25%, Mn: 0.59%, S: 0.0031%, P: 0.0052%, Cr: 5.12%, Mo: 0.53%, Cu: 0.17%, Ni: 0.23%, Ti: 0.022%, V: 0.02%, O: 0.0047%, N: 0.0093%, and the balance is Fe and unavoidable impurities.

[0059] The preparation method of the welding wire is as follows: weigh each component in proportion, smelt the welding wire in a 0.5t electric furnace, forge and draw the welding wire and copper plate it, then process it into a welding wire with a diameter of Φ2.4mm and straighten and cut it into a wire specification of Φ2.4×1000mm.

[0060] The obtained welding wire was heat treated at 745℃ for 1h, and the mechanical properties of the deposited metal of the welding wire were tested. The results are shown in Table 2.

[0061] The method of welding 5% Cr-0.5% Mo high temperature resistant steel using the above welding wire is to perform welding under argon protection, wherein the welding parameters are: welding voltage 13-15V, welding current 180A, welding speed 50-100mm / min, interpass temperature 200-250°C, and shielding gas flow rate 13-18L / min.

[0062] Comparative Example 1:

[0063] The composition of the welding wire of this comparative example is shown in the data corresponding to comparative example 1 in Table 1;

[0064] The specific chemical composition of the welding wire, by weight percentage, includes: C: 0.09%, Si: 0.34%, Mn: 0.63%, S: 0.0023%, P: 0.0050%, Cr: 5.22%, Mo: 0.42%, Cu: 0.16%, Ni: 0.30%, Ti: 0.035%, V: 0.02%, O: 0.0046%, N: 0.0091%, and the balance is Fe and unavoidable impurities.

[0065] The preparation method of the welding wire is as follows: weigh each component in proportion, smelt the welding wire in a 0.5t electric furnace, forge and draw the welding wire and copper plate it, then process it into a welding wire with a diameter of Φ2.4mm and straighten and cut it into a wire specification of Φ2.4×1000mm.

[0066] The obtained welding wire was heat treated at 745℃ for 1h, and the mechanical properties of the deposited metal of the welding wire were tested. The results are shown in Table 2.

[0067] The method of welding 5% Cr-0.5% Mo high temperature resistant steel using the above welding wire is to perform welding under argon protection, wherein the welding parameters are: welding voltage 13-15V, welding current 180A, welding speed 50-100mm / min, interpass temperature 200-250°C, and shielding gas flow rate 13-18L / min.

[0068] Comparative Example 2:

[0069] The composition of the welding wire of this comparative example is shown in the data corresponding to comparative example 2 in Table 1;

[0070] The specific chemical composition of the welding wire, measured by weight percentage, includes: C: 0.09%, Si: 0.32%, Mn: 0.60%, S: 0.0024%, P: 0.0047%, Cr: 5.17%, Mo: 0.43%, Cu: 0.19%, Ni: 0.32%, Ti: 0.035%, V: 0.05%, O: 0.0036%, N: 0.0093%, and the balance is Fe and unavoidable impurities.

[0071] The preparation method of the welding wire is as follows: weigh each component in proportion, smelt the welding wire in a 0.5t electric furnace, forge and draw the welding wire and copper plate it, then process it into a welding wire with a diameter of Φ2.4mm and straighten and cut it into a wire specification of Φ2.4×1000mm.

[0072] The obtained welding wire was heat treated at 745℃ for 1h, and the mechanical properties of the deposited metal of the welding wire were tested. The results are shown in Table 2.

[0073] The method of welding 5% Cr-0.5% Mo high temperature resistant steel using the above welding wire is to perform welding under argon protection, wherein the welding parameters are: welding voltage 13-15V, welding current 180A, welding speed 50-100mm / min, interpass temperature 200-250°C, and shielding gas flow rate 13-18L / min.

[0074] Comparative Example 3:

[0075] The composition of the welding wire of this comparative example is shown in the data corresponding to comparative example 3 in Table 1;

[0076] The specific chemical composition of the welding wire, by weight percentage, includes: C: 0.08%, Si: 0.28%, Mn: 0.58%, S: 0.0033%, P: 0.0044%, Cr: 5.26%, Mo: 0.41%, Cu: 0.19%, Ni: 0.30%, Ti: 0.034%, V: 0.001%, O: 0.0046%, N: 0.0095%, and the balance is Fe and unavoidable impurities.

[0077] The preparation method of the welding wire is as follows: weigh each component in proportion, smelt the welding wire in a 0.5t electric furnace, forge and draw the welding wire and copper plate it, then process it into a welding wire with a diameter of Φ2.4mm and straighten and cut it into a wire specification of Φ2.4×1000mm.

[0078] The obtained welding wire was heat treated at 745℃ for 1h, and the mechanical properties of the deposited metal of the welding wire were tested. The results are shown in Table 2.

[0079] The method of welding 5% Cr-0.5% Mo high temperature resistant steel using the above welding wire is to perform welding under argon protection, wherein the welding parameters are: welding voltage 13-15V, welding current 180A, welding speed 50-100mm / min, interpass temperature 200-250°C, and shielding gas flow rate 13-18L / min.

[0080] Table 1 Chemical composition of welding wire (Wt.%)

[0081]

[0082] Table 2 Mechanical properties of deposited metal of welding wire (PWHT: 745℃×1h)

[0083]

[0084]

[0085] The welding wires obtained in Examples 1 to 5 were subjected to heat treatment for different time periods, and the mechanical properties of the deposited metal were measured. The results are shown in Table 3.

[0086] Table 3

[0087]

[0088] It can be seen from Table 2 above, and through the comparison between the embodiments and the comparative examples, embodiments 1-5 all meet the design requirements. When the Ti, V, and Cu components are adjusted in comparative examples 1-3, respectively, Ti in comparative example 1 exceeds the required range, V in comparative example 2 exceeds the required range, and Cu in comparative example 3 exceeds the range, and the elongation after fracture and the impact absorption energy are both reduced.

[0089] It can be seen from Table 3 above that the welding wire obtained in Example 1 is subjected to heat treatment for different times. After heat treatment at 745°C for 1 to 8 hours, the weld metal of the welding wire can meet the design requirements of room temperature tensile strength ≥550MPa, room temperature yield strength ≥470MPa, elongation after fracture ≥17%, yield strength at 600°C ≥179MPa, impact energy Akv at -30°C of 100J or more, and impact energy Akv at room temperature of 200J or more.

[0090] Although the present invention has been disclosed as above in the preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.

Claims

1. A argon arc welding wire for 5Cr-0.5Mo high temperature resistant steel, characterized in that: The chemical composition, by weight percentage, includes: C: 0.06-0.09%, Si: 0.20-0.50%, Mn: 0.40-0.70%, S≤0.005%, P≤0.006%, Cr: 5.00-6.00%, Mo: 0.45-0.65%, Cu: 0.10-0.20%, Ni: 0.10-0.40%, Ti: 0.01-0.05%, V: 0.01-0.03%, As≤0.005%, Sn≤0.005%, Pb≤0.003%, O≤0.005%, N≤0.010%, and the balance is Fe and unavoidable impurities; After heat treatment at 745°C for 1 to 8 hours, the room temperature tensile strength of the deposited metal of the welding wire is ≥550MPa, the room temperature yield strength is ≥470MPa, the elongation after fracture is ≥17%, the yield strength at 600°C is ≥179MPa, the impact energy Akv at -30°C is 100J or more, and the impact energy Akv at room temperature is 200J or more.

2. The argon arc welding wire for 5Cr-0.5Mo high temperature resistant steel according to claim 1, characterized in that: The chemical composition, by weight percentage, includes: C: 0.06-0.09%, Si: 0.20-0.40%, Mn: 0.40-0.70%, S≤0.005%, P≤0.006%, Cr: 5.00-6.00%, Mo: 0.45-0.65%, Cu: 0.10-0.20%, Ni: 0.10-0.40%, Ti: 0.01-0.05%, V: 0.01-0.03%, As≤0.005%, Sn≤0.005%, Pb≤0.003%, O≤0.005%, N≤0.010%, and the balance is Fe and unavoidable impurities.

3. The argon arc welding wire for 5Cr-0.5Mo high temperature resistant steel according to claim 1, characterized in that: The chemical composition, by weight percentage, includes: C: 0.09%, Si: 0.30%, Mn: 0.65%, S: 0.0018%, P: 0.0049%, Cr: 5.15%, Mo: 0.51%, Cu: 0.19%, Ni: 0.25%, Ti: 0.020%, V: 0.02%, O: 0.0046%, N: 0.0092%, and the balance is Fe and unavoidable impurities.

4. The argon arc welding wire for 5Cr-0.5Mo high temperature resistant steel according to claim 1, characterized in that: The chemical composition, by weight percentage, includes: C: 0.08%, Si: 0.25%, Mn: 0.65%, S: 0.0022%, P: 0.0060%, Cr: 5.02%, Mo: 0.51%, Cu: 0.15%, Ni: 0.20%, Ti: 0.024%, V: 0.01%, O: 0.0049%, N: 0.0091%, and the balance is Fe and unavoidable impurities.

5. The argon arc welding wire for 5Cr-0.5Mo high temperature resistant steel according to claim 1, characterized in that: The chemical composition, by weight percentage, includes: C: 0.09%, Si: 0.28%, Mn: 0.60%, S: 0.0041%, P: 0.0044%, Cr: 5.01%, Mo: 0.51%, Cu: 0.15%, Ni: 0.19%, Ti: 0.029%, V: 0.02%, O: 0.0049%, N: 0.0094%, and the balance is Fe and unavoidable impurities.

6. The argon arc welding wire for 5Cr-0.5Mo high temperature resistant steel according to claim 1, characterized in that: The chemical composition, by weight percentage, includes: C: 0.08%, Si: 0.33%, Mn: 0.61%, S: 0.0022%, P: 0.0048%, Cr: 5.24%, Mo: 0.49%, Cu: 0.18%, Ni: 0.25%, Ti: 0.022%, V: 0.01%, O: 0.0046%, N: 0.0091%, and the balance is Fe and unavoidable impurities.

7. The argon arc welding wire for 5Cr-0.5Mo high temperature resistant steel according to claim 1, characterized in that: The chemical composition, by weight percentage, includes: C: 0.08%, Si: 0.25%, Mn: 0.59%, S: 0.0031%, P: 0.0052%, Cr: 5.12%, Mo: 0.53%, Cu: 0.17%, Ni: 0.23%, Ti: 0.022%, V: 0.02%, O: 0.0047%, N: 0.0093%, and the balance is Fe and unavoidable impurities.

8. A method for preparing the argon arc welding wire for 5Cr-0.5Mo high temperature resistant steel according to claim 1, characterized in that: The components were weighed in proportion, and the welding wire was smelted in a 0.5t electric furnace. After forging, drawing and copper plating, it was processed into welding wire with a diameter of Φ2.4mm, and then straightened and cut into wires with specifications of Φ2.4×1000mm.

9. A method for using the argon arc welding wire for 5Cr-0.5Mo high temperature resistant steel according to claim 1, characterized in that: Under argon protection, the welding parameters are: welding voltage 13~15V, welding current 180A, welding speed 50~100mm / min, interpass temperature 200~250℃, and shielding gas flow rate 13~18L / min.