A heat treatment method for improving the comprehensive mechanical properties of low-carbon high-alloy martensitic stainless steel
Through the Q-C-T-C-T heat treatment process, the heat treatment parameters are regulated to form a structure of dispersed distribution of fine carbides on the thin film-like residual austenite phase matrix, solving the contradiction between the strength and toughness of low-carbon high alloy martensitic stainless steel The problem is that the high strength and high toughness of the material are achieved and are suitable for aerospace parts.
Patent Information
- Application Number
- CN202211282893.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-19
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-10-19
AI Technical Summary
The prior art is difficult to maintain its toughness while increasing the strength of low-carbon high-alloy martensitic stainless steels, and the strength and toughness of the material are often contradictory, resulting in the damage to the other performance when improving one aspect.
By using the Q-C-T-C-T (quenching + two deep-cold tempering) heat treatment process, the heat treatment process parameters are regulated to form a structure of dispersed fine carbides on the fine martensite slats and film-like residual austenite phase matrix, thereby improving martensite Comprehensive mechanical properties of stainless steel. Specific steps include annealing treatment, austenitization treatment, first and second tempering treatments, controlling the quenching temperature, time and cooling speed, deep cooling temperature, time and cooling speed, tempering temperature and time and other conditions.
It achieves the improvement of the strength of martensite stainless steel while ensuring its toughness and has high hardness. The comprehensive mechanical properties of the material such as tensile strength, yield strength, elongation, cross-section shrinkage and impact work have reached an excellent level, meeting the aerospace High strength and toughness requirements of aerospace parts.
Smart Images

Figure CN115612813B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of stainless steel heat treatment, and in particular relates to a heat treatment method for improving the comprehensive mechanical properties of low-carbon high-alloy martensitic stainless steel. Background Art
[0002] In order to meet the demand for structural materials in the rapid development of the aviation industry, new high-alloy ultra-high-strength steels have received great attention from scholars. Ultra-high-strength steels are widely used in the manufacture of various aerospace components due to their high strength and toughness. Due to the harsh service environment of their structural parts, higher requirements are placed on the mechanical properties of the structural materials themselves, and their performance greatly affects the service life and reliability of the structural parts.
[0003] Aviation structural parts will bear huge loads during service, so the basic materials are required to have high strength and certain toughness to ensure that they will not fail due to external loads during use. The most important performance indicators of high-strength and tough martensitic stainless steel as a structural material are yield strength and tensile strength. In industry, alloying, heat treatment and deformation strengthening are often used to improve the comprehensive mechanical properties of steel. The basic microscopic strengthening mechanisms of these strengthening methods include: solid solution strengthening, fine grain strengthening, dislocation strengthening, second phase strengthening, phase transformation strengthening, etc. The strengthening of any steel is not determined by a single strengthening mechanism, but is obtained by the superposition of several strengthening mechanisms. Therefore, the use of different strengthening mechanisms at the same time can obtain the comprehensive effect of multiple strengthening mechanisms. With the development of modern industry, the strength requirements of materials are getting higher and higher, but the strength and toughness of materials are usually contradictory. Increasing strength often reduces toughness, and conversely, increasing toughness also damages strength. It is generally believed that toughness and plasticity are related to the concentration and relaxation of stress, work hardening of materials, energy absorption and dissipation, and the formation and diffusion of cracks, and are comprehensive indicators of the fracture and deformation of reactive materials. Among them, the theory of fracture toughness is relatively mature and widely used. The toughness of materials with high plasticity is not necessarily high, because the size of toughness depends on both the amount of plastic deformation and the influence of work hardening rate. Only when both are large at the same time will the material have high toughness. In the above-mentioned strengthening mechanism, except for fine grain strengthening, the others will lead to a decrease in toughness and plasticity. The general ways to improve toughness mainly include reducing the mass fraction of carbon and the mass fraction of harmful elements, refining austenite grains, eliminating coarse carbides and grain boundary films, increasing dislocation density, reducing the mean free path of dislocations, preventing pre-existing microcracks, deformation heat treatment, Q&P heat treatment, retaining a small amount of stable residual austenite, and using phase transformation induced plasticity. Therefore, researching and developing a method to improve the comprehensive mechanical properties of low-carbon high-alloy martensitic stainless steel has become an important topic that needs to be studied urgently. Summary of the invention
[0004] In view of this, the purpose of the present invention is to provide a heat treatment method for improving the comprehensive mechanical properties of low-carbon high-alloy martensitic stainless steel. The present invention adopts a QCTCT (quenching + double deep cold tempering) heat treatment process. By adjusting the heat treatment process parameters, a structure of fine carbides dispersed on a matrix of fine martensitic laths and a film-like residual austenite phase is obtained, which can improve the strength of martensitic stainless steel while ensuring its toughness and having higher hardness.
[0005] The object of the present invention is to achieve the following:
[0006] The present invention provides a heat treatment method for improving the comprehensive mechanical properties of low-carbon high-alloy martensitic stainless steel, which mainly comprises the following steps:
[0007] (1) Martensitic stainless steel material is used, and its components and weight percentage contents are: C: 0.1-0.15%, Cr: 10-15%, Co: 10-14%, Mo: 4-6%, Ni: 1.5-3%, V: 0.5-0.8%, Nb: 0.01-0.05%, and the rest is Fe and unavoidable impurities;
[0008] (2) annealing the martensitic stainless steel of step (1) at a temperature of 900° C. to 950° C.;
[0009] (3) austenitizing the material obtained in step (2), and then oil cooling the austenitized material to room temperature;
[0010] (4) cooling the material obtained in step (3) to below the Mf point, and controlling the cooling for a period of time to allow the residual austenite to be transformed into martensite as much as possible, and then slowly heating it to room temperature;
[0011] (5) subjecting the material obtained in step (4) to a first tempering treatment to transform the martensite into tempered martensite, and air cooling to room temperature;
[0012] (6) cooling the material obtained in step (5) to below the Mf point, and controlling the cooling for a period of time, performing a second cold treatment, and slowly heating to room temperature;
[0013] (7) The material obtained in step (6) is subjected to a second tempering at a temperature between 490° C. and 515° C. for a holding time of ≥1 h, and air-cooled to room temperature after tempering.
[0014] Based on the above technical solution, further, the martensitic stainless steel material described in step (1) is melted by vacuum induction + vacuum consumable method to obtain a stainless steel billet, and then subjected to hot working forming, and the hot working forming includes high temperature homogenization treatment and forging / rolling process.
[0015] Based on the above technical solution, further, the forging / rolling process requires that the steel start forging / rolling temperature is 1050℃~1100℃, the final forging / rolling temperature is ≥900℃, the total hot working deformation is ≥80%, and the hot rolled bar grain size is 7~8 levels.
[0016] Based on the above technical solution, further, in the austenitizing process in step (3), the austenitizing temperature is 1040-1055° C., and the holding time is 1-2 hours.
[0017] Based on the above technical solution, further, the Mf in step (4) is -4°C.
[0018] Based on the above technical solution, further, the specific process of step (4) is to cool the material obtained in step (3) to ≤-80°C, control the cooling time to ≥1h, and the cooling rate is 50-100°C / h; the slow heating rate is ≤30°C / h.
[0019] Based on the above technical solution, further, the tempering temperature of the first tempering treatment described in step (5) is 525-550°C, and the heat preservation time is ≥1h.
[0020] Based on the above technical solution, further, the specific process in step (6) is to cool the material obtained in step (5) to ≤-80°C, control the cooling time to ≥1h, and the cooling rate is 50-100°C / h; the slow heating rate is ≤30°C / h.
[0021] Another aspect of the present invention provides a high-strength and tough martensitic stainless steel, which is obtained by adjusting the microstructure and properties of the high-strength and tough martensitic stainless steel through the above-mentioned heat treatment method, wherein the mechanical properties of the high-strength and tough martensitic stainless steel meet the following requirements: tensile strength ≥ 1900MPa, yield strength ≥ 1400MPa, elongation ≥ 15%, cross-sectional shrinkage ≥ 55%, impact energy AKu ≥ 70J, and Rockwell hardness HRC ≥ 53.
[0022] The present invention also provides the use of the high-strength and toughness martensitic stainless steel in the preparation of aerospace parts.
[0023] The beneficial effects of the present invention compared with the prior art are as follows:
[0024] 1. The present invention adopts QCTCT (quenching + twice deep cooling and tempering) heat treatment process, by strictly controlling the quenching temperature, time and cooling rate after quenching, deep cooling temperature, time and cooling rate, tempering temperature and time and other conditions, while improving the strength of martensitic stainless steel, it can ensure its toughness and have higher hardness.
[0025] 2. The present invention obtains the best heat treatment process parameters with excellent comprehensive mechanical properties, ensuring the excellent room temperature comprehensive mechanical properties of the material: tensile strength ≥1900MPa, yield strength ≥1400MPa, elongation ≥15%, cross-sectional shrinkage ≥55%, impact energy AKu ≥70J, Rockwell hardness HRC ≥53; ensuring that the material has high strength and hardness while having good toughness and plasticity. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the embodiments of the present invention, the drawings related to the embodiments are briefly introduced below.
[0027] Figure 1 This is the heat treatment process flow of the present invention.
[0028] Figure 2 This is the microstructure diagram of the high-strength and toughness stainless steel obtained in Example 1. DETAILED DESCRIPTION
[0029] The present invention is described in detail below with reference to the embodiments, but the embodiments of the present invention are not limited thereto. Obviously, the embodiments described below are only partial embodiments of the present invention. For those skilled in the art, other similar embodiments obtained without creative labor all fall within the protection scope of the present invention.
[0030] The main process of the heat treatment method for improving the comprehensive mechanical properties of low-carbon high-alloy martensitic stainless steel of the present invention is as follows: the components and weight percentage contents of martensitic stainless steel are: C: 0.1-0.15%, Cr: 10-15%, Co: 10-14%, Mo: 4-6%, Ni: 1.5-3%, V: 0.5-0.8%, Nb: 0.01-0.05%, and the rest are Fe and unavoidable impurities. In an embodiment of the present invention, the above-mentioned martensitic stainless steel can be smelted by vacuum induction + vacuum consumable to obtain a stainless steel blank, and then hot-rolled annealed martensitic stainless steel is obtained by hot working forming and annealing treatment, wherein the hot working forming may include high-temperature homogenization treatment and forging (rolling) process, for example but not limited to, requiring the steel forging temperature to be 1050-1100°C, the final forging temperature to be ≥900°C, the total deformation of hot working to be 80%, and the grain size of the obtained material structure to be 7-8 grades; the annealing temperature of the annealing treatment can be 900-950°C. It should be understood that the above melting, hot rolling and annealing parameters are intended to exemplify the process of obtaining hot-rolled annealed martensitic stainless steel, and are not intended to be a specific limitation on the heat treatment method of the present invention. Specifically, the heat treatment method for controlling the microstructure and properties of martensitic stainless steel according to the present invention may include the following steps:
[0031] 1. Heat the hot-rolled annealed martensitic stainless steel to above the complete austenitization temperature Ac3 (750°C) and keep it warm for a certain period of time to allow the material to fully complete the austenite phase transformation and allow the precipitated phase to completely dissolve back into the matrix. The holding temperature is 1040-1055°C and the holding time is 1-2h. If the temperature is lower than 1040°C, the precipitated phase cannot be fully dissolved back into the matrix, which will lead to a decrease in the number of nano-scale strengthening phases precipitated during the tempering process, affecting the final performance of the material. If the temperature is higher than 1055°C, the original austenite grains will grow excessively, and the coarse grains will lead to coarse martensite laths obtained by quenching, and the yield strength will be greatly reduced. If the holding time is less than 1h, the precipitated phase will not have enough time to dissolve back into the matrix, and if the holding time is too long, the original grains will become coarse. After the austenitization holding is completed, the material is cooled to room temperature by oil cooling. This process is to make the steel cool quickly after complete austenitization to promote the transformation of austenite into martensite. If the cooling rate is too fast, the internal stress of the material will increase, which will increase the risk of steel cracking. If the cooling rate is too slow, the martensite transformation will be incomplete, which may easily lead to high residual austenite content and coarse martensite laths. The residual austenite will undergo martensitic phase transformation during long-term use, resulting in poor dimensional stability of the material and affecting its performance. Coarse martensite laths will reduce the strength of the material.
[0032] 2. Then place the material in a controlled cold cabinet and cool it down to below the end temperature Mf of the martensitic phase transformation, so as to promote the further transformation of the incompletely transformed austenite into martensite, make the transformation more thorough, reduce the residual austenite content in the material, and increase the dimensional stability of the material. The cooling rate should be controlled at 50℃ / h~100℃ / h; the controlled cooling temperature is ≤-80℃, and the controlled cooling time is ≥1h; if the cooling rate is too fast, the material will crack due to the volume shrinkage caused by rapid cooling, and if the cooling rate is too slow, the martensitic transformation will be insufficient. The controlled cooling temperature is ≤-80℃ to provide sufficient supercooling and provide sufficient phase transformation driving force for the martensitic transformation. At the same time, due to the extremely low temperature, the lattice constant of iron tends to shrink, which increases the precipitation driving force of C atoms and promotes the precipitation of fine carbides during the tempering process, which plays a role in strengthening the second phase; after the controlled cooling process, the material should be slowly heated to room temperature, and the heating rate is ≤30℃ / h to avoid cracking of the material due to rapid heating;
[0033] 3. Then, the material is placed in a box-type resistance furnace for the first tempering treatment to promote the precipitation of supersaturated carbon atoms in the martensite in the form of precipitation phase. The fine dispersed second phase is distributed in the martensite matrix to improve the strength of the material. The tempering temperature should be controlled between 525℃ and 550℃, and the holding time should be ≥1h. If the tempering temperature is less than 525℃, the heat energy provided by the tempering process is not enough to fully precipitate nano-scale carbides, which will lead to a decrease in material strength. If the temperature is greater than 550℃, the martensite lath will coarsen, seriously affecting the material performance. After tempering, the material is air-cooled to room temperature.
[0034] 4. Then, the material after the first tempering is placed in a controlled cooling cabinet for a second cold treatment, and the temperature is lowered to below the end temperature Mf of the martensitic phase transformation. The cooling rate should be controlled at 50℃ / h~100℃ / h, the controlled cooling temperature ≤-80℃, and the controlled cooling time ≥1h. If the cooling rate is too fast, the material will crack due to the volume shrinkage caused by rapid cooling, and if the cooling rate is too slow, the martensitic transformation will be insufficient. The controlled cooling temperature ≤-80℃ is to provide sufficient supercooling, provide sufficient phase transformation driving force for the martensitic transformation, and make the residual Austenite is further transformed into martensite structure, which can not only effectively refine the martensite structure, but also the residual austenite left in the matrix after cold treatment will exist in the matrix in the form of a film, which is beneficial to improve the toughness of the material. At the same time, the temperature is reduced so that C atoms precipitate from the supersaturated solid solution and gather near the martensite lath boundary and dislocation, which is beneficial to the further precipitation of nano-scale carbides during the secondary tempering process, thereby improving the strength and toughness of the material. After the insulation is completed, the temperature is slowly raised to room temperature, and the heating rate is ≤30℃ / h;
[0035] 5. Immediately after the second deep cooling, the material is placed in a box-type resistance furnace for tempering treatment, wherein the tempering temperature should be controlled between 490℃ and 515℃, the holding time should be ≥1h, and the material should be air-cooled to room temperature after tempering; if the tempering temperature is less than 490℃, the heat energy provided by the tempering process is not enough to fully precipitate the nano-scale carbides, which will lead to a decrease in material strength, while the temperature is greater than 515℃, the nano-scale carbides are fully precipitated in the matrix, although the material strength and hardness are greatly improved, the toughness will be greatly reduced, which will affect the actual use of the material.
[0036] Example 1
[0037] A heat treatment method for improving the comprehensive mechanical properties of low-carbon high-alloy martensitic stainless steel mainly comprises the following steps:
[0038] 1. In this embodiment, a hot-rolled martensitic stainless steel bar is used, and the bar structure has a grain size of 7 to 8, and its components and weight percentage contents are: C: 0.14%, Cr: 13%, Co: 14%, Mo: 6%, Ni: 1.5%, V: 0.5%, Nb: 0.01%, and the rest is Fe and unavoidable impurities;
[0039] 2. Anneal the material at a temperature of 900°C;
[0040] 3. Then the material is quenched, the austenitizing temperature is 1055℃, and the temperature is kept for 1h. After the temperature is kept, the material is oil-cooled to room temperature;
[0041] 4. Then place the material in a controlled cold cabinet and cool it to -80℃ for 2h, with a cooling rate of 50-100℃ / h. After the insulation is completed, slowly heat it to room temperature, with a heating rate of ≤30℃ / h;
[0042] 5. Then the material is subjected to the first tempering treatment, the tempering temperature is 550℃ and kept for 1h, and then air-cooled to room temperature after the end of the heat preservation;
[0043] 6. After the first tempering is completed, the material is placed in a controlled cold cabinet for a second cold treatment. The cooling rate is 50-100℃ / h, the cold treatment temperature is -80℃, and the temperature is kept for 2h. After the insulation is completed, the temperature is slowly raised to room temperature, and the heating rate is ≤30℃ / h;
[0044] 7. Immediately after the second cold treatment, the material will be tempered for the second time. The tempering temperature is 490℃ and kept for 2h. After the insulation, it will be air-cooled to room temperature.
[0045] Example 2
[0046] A heat treatment method for improving the comprehensive mechanical properties of low-carbon high-alloy martensitic stainless steel mainly comprises the following steps:
[0047] 1. Use martensitic stainless steel hot-rolled bars, the bar structure grain size is 7-8, and its components and weight percentage content are: C: 0.11%, Cr: 14%, Co: 11%, Mo: 6%, Ni: 2.5%, V: 0.8%, Nb: 0.01%, and the rest is Fe and unavoidable impurities;
[0048] 2. Anneal the material at a temperature of 950°C;
[0049] 3. Then the material is quenched, the austenitizing temperature is 1040℃, and the temperature is kept for 1.5h. After the temperature is kept, it is oil-cooled to room temperature;
[0050] 4. Then place the material in a controlled cold cabinet and cool it to -80℃ for 2h, with a cooling rate of 50-100℃ / h. After the insulation is completed, slowly heat it to room temperature, with a heating rate of ≤30℃ / h;
[0051] 5. Then the material is subjected to the first tempering treatment, the tempering temperature is 525℃ and kept for 2h, and then air-cooled to room temperature after the end of the heat preservation;
[0052] 6. After the first tempering is completed, the material is placed in a controlled cold cabinet for a second cold treatment. The cold treatment temperature is -80°C, the cooling rate is 50-100°C / h, and the temperature is kept for 2 hours. After the insulation is completed, the temperature is slowly raised to room temperature, and the heating rate is ≤30°C / h;
[0053] 7. Immediately after the second cold treatment, the material will be tempered for the second time. The tempering temperature is 515℃ and kept for 2h. After the insulation, it will be air-cooled to room temperature.
[0054] Comparative Example 1
[0055] 1. Use martensitic stainless steel hot-rolled bars, the bar structure grain size is 7-8, and its components and weight percentage content are: C: 0.14%, Cr: 13%, Co: 14%, Mo: 6%, Ni: 1.5%, V: 0.5%, Nb: 0.01%, and the rest is Fe and unavoidable impurities;
[0056] 2. Anneal the material at a temperature of 900°C;
[0057] 3. Then the material is quenched at an austenitizing temperature of 1100°C for 1 hour, and then oil-cooled to room temperature;
[0058] 4. Then place the quenched material in a controlled cold cabinet and cool it to -80℃ for 2h, with a cooling rate of 50-100℃ / h. After the insulation is completed, slowly heat it to room temperature, with a heating rate of ≤30℃ / h;
[0059] 5. Then the material is subjected to the first tempering treatment, the tempering temperature is 540℃ for 1h, and then air-cooled to room temperature after the end of the insulation;
[0060] 6. After the first tempering is completed, the material is placed in a controlled cold cabinet for a second cold treatment. The cooling rate is 50-100℃ / h, the cold treatment temperature is -80℃, and the temperature is kept for 2h. After the insulation is completed, the temperature is slowly raised to room temperature, and the heating rate is ≤30℃ / h;
[0061] 7. Immediately after the second cold treatment, the material will be tempered for the second time. The tempering temperature is 540℃ and kept for 2h. After the insulation, it will be air-cooled to room temperature.
[0062] Comparative Example 2
[0063] 1. Use martensitic stainless steel hot-rolled bars, the bar structure grain size is 7-8, and its components and weight percentage content are: C: 0.11%, Cr: 14%, Co: 11%, Mo: 6%, Ni: 2.5%, V: 0.8%, Nb: 0.01%, and the rest is Fe and unavoidable impurities;
[0064] 2. Anneal the material at a temperature of 950°C;
[0065] 3. Then the material is quenched, the austenitizing temperature is 1050℃, and the temperature is kept for 1h. After the temperature is kept, the material is oil-cooled to room temperature;
[0066] 4. Then place the quenched material in a controlled cold cabinet and cool it to -80℃ for 2h, with a cooling rate of 50-100℃ / h. After the insulation is completed, slowly heat it to room temperature, with a heating rate of ≤30℃ / h;
[0067] 5. Then the material is subjected to the first tempering treatment at 500°C for 2 hours, and then air-cooled to room temperature after the end of the tempering treatment;
[0068] 6. After the first tempering is completed, the material is placed in a controlled cold cabinet for a second cold treatment. The cold treatment temperature is -80°C, the cooling rate is 50-100°C / h, and the temperature is kept for 2 hours. After the insulation is completed, the temperature is slowly raised to room temperature, and the heating rate is ≤30°C / h;
[0069] 7. Immediately after the second cold treatment, the material will be tempered for the second time. The tempering temperature is 500℃ and kept for 2h. After the insulation, it will be air-cooled to room temperature.
[0070] Table 1. Performance test results of high-strength and tough stainless steel prepared in Example 1-2
[0071]
[0072] It can be seen from Table 1 that Examples 1-2 of the present invention can improve the yield strength, tensile strength and hardness of the material while ensuring that the material has sufficiently high toughness, so that the material achieves a good match between strength and toughness and can meet actual use requirements.
[0073] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A heat treatment method for improving the comprehensive mechanical properties of low-carbon high-alloy martensitic stainless steel, characterized in that: The following steps are involved: (1) Martensitic stainless steel material is used, and its components and weight percentage are: C: 0.1~0.15%, Cr: 10~15%; Co: 10~14%; Mo: 4~6%; Ni: 1.5~3%; V:0.5~0.8%; Nb: 0.01~0.05%, the rest is Fe and unavoidable impurities; (2) annealing the martensitic stainless steel obtained in step (1) at a temperature of 900° C. to 950° C.; (3) austenitizing the material obtained in step (2), and then oil cooling the austenitized material to room temperature; (4) cooling the material obtained in step (3) to below the Mf point, and controlling the cooling for a period of time to allow the residual austenite to be transformed into martensite as much as possible, and then slowly heating it to room temperature; (5) subjecting the material obtained in step (4) to a first tempering treatment to transform the martensite into tempered martensite, and air cooling to room temperature; (6) cooling the material obtained in step (5) to below the Mf point, and controlling the cooling for a period of time, performing a second cold treatment, and slowly heating the material to room temperature; (7) subjecting the material obtained in step (6) to a second tempering at a temperature between 490°C and 515°C for a holding time of ≥1h, and air cooling to room temperature after tempering; In step (3), the austenitizing temperature during the austenitizing treatment is 1040-1055° C., and the holding time is 1-2 hours; The specific process of step (4) is to cool the material obtained in step (3) to ≤-80°C, control the cooling time to ≥1h, and the cooling rate is 50-100°C / h; the heating rate of slow heating is ≤30°C / h; The first tempering treatment in step (5) has a tempering temperature of 525-550°C and a heat preservation time of ≥1h; The specific process in step (6) is to cool the material obtained in step (5) to ≤-80°C, control the cooling time to ≥1h, and the cooling rate is 50~100°C / h; the heating rate of slow heating is ≤30°C / h.
2. A high-strength and high-toughness martensitic stainless steel, characterized in that: The high-strength and toughness martensitic stainless steel is obtained by regulating the microstructure and properties of the heat treatment method according to claim 1, wherein the mechanical properties of the high-strength and toughness martensitic stainless steel meet the following requirements: tensile strength ≥1900 MPa, yield strength ≥1400 MPa, elongation ≥15%, cross-sectional shrinkage ≥55%, impact energy AKu ≥70J, and Rockwell hardness HRC ≥53.
3. Use of the high-strength and toughness martensitic stainless steel according to claim 2 in the preparation of aerospace parts.