A low-loss metallization coating method and product for quartz glass hemispherical resonator
By shielding the parts that do not require metallization on the surface of the hemispheric resonator, using the magnetron sputtering process to deposit transition metal and conductive layers, and setting up conductive strip connections, the problem of large damping of the metal film layer of the hemispheric resonator is solved, and the efficiency of the hemispheric resonator is significantly improved. Quality factor and performance to meet higher accuracy requirements.
Patent Information
- Application Number
- CN202211181781.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-27
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-09-27
AI Technical Summary
In the existing technology, the damping of the metal film layer on the surface of the hemispheric resonator is large, which leads to increased energy loss and reduced measurement accuracy and performance. In addition, the large-area metal layer causes a decrease in quality factor, making it difficult to significantly reduce the damping by optimizing the coating process.
By preparing a physical mask to shield the parts that do not require metallization, a magnetron sputtering process is used to deposit a transition metal film and a conductive layer to form a composite metal conductive film layer, and conductive strip connections are set up on the inner spherical surface to reduce the area of the metallized film. Reduce damping and improve quality factor.
It significantly improves the quality factor of the hemispheric resonator, reduces energy loss, improves measurement accuracy and performance, and meets the higher quality requirements of modern quartz glass hemispheric resonators.
Smart Images

Figure CN115612982B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field related to inertial navigation hemispherical resonator gyroscopes, and more specifically, relates to a low-loss metallization coating method and product for a quartz glass hemispherical resonator. Background Art
[0002] The hemispherical resonant gyroscope uses the Coriolis effect to measure the rotation angle through the standing wave precession of the two-amplitude vibration mode of the hemispherical oscillator. Because it has no mechanical moving parts, no mechanical loss, simple structure, small size, low power consumption, high reliability, long life, etc. The accuracy of the gyroscope is only related to the processing accuracy of the resonator, and has nothing to do with the size of the resonator. Its accuracy level can cover tactical, inertial navigation and strategic levels. It has extremely broad application prospects in many fields such as unmanned driving, weapons and equipment, aerospace and space exploration, and is recognized by the inertial navigation field as the next generation of high-precision gyroscope technology.
[0003] The hemispherical resonator is the main functional component of the hemispherical resonator gyroscope. It is usually made of quartz glass with low internal damping but no conductivity. It is made conductive by metallization coating on the surface of the hemispherical oscillator. Capacitive electrodes are formed by setting inner and outer spherical or planar electrodes and the inner and outer spherical surfaces or hemispherical end faces of the hemispherical oscillator. The electrodes are used to excite the vibration of the hemispherical oscillator through electrostatic force by applying AC signals, and measure the displacement signal of the oscillator during vibration through the capacitance between the plates, and solve the position of the antinode of the working mode of the hemispherical oscillator, and then calculate the rotation angle of the hemispherical oscillator in the inertial space.
[0004] The quality factor is a physical quantity used to characterize the energy loss characteristics of a vibration system. It refers to the ratio of the total energy of the vibration system to the energy lost in one cycle. The higher the quality factor, the less energy loss of the hemispherical resonator during operation, which helps to reduce the output error of the hemispherical resonator, reduce energy consumption, and improve sensitivity. If the metal film layer on the surface of the hemispherical resonator is uneven, it will cause uneven circumferential damping of the hemispherical resonator, which will cause the hemispherical resonator to drift and reduce measurement accuracy.
[0005] However, due to the large material damping of the metal film layer, which is an inherent property of the metal film layer material, it is difficult to significantly reduce the energy loss caused by the damping introduced by the metal film layer by optimizing the coating process. On the other hand, in the prior art, the coating technology solution commonly used requires metallization coating on the entire inner spherical surface, the end surface and the support rod surface. The large area of the metal layer causes a sharp drop in the quality factor of the hemispherical oscillator, resulting in a reduction in its performance.
[0006] Accordingly, the art urgently needs to further optimize its metallization coating process in order to meet the higher quality requirements of modern quartz glass hemispherical resonators. Summary of the invention
[0007] In view of the above defects or needs of the prior art, the object of the present invention is to provide a low-loss metallization coating method and product for a quartz glass hemispherical resonator, wherein the operating process of the entire preparation process is redesigned, and targeted improvements are made around the process parameters and requirements of some key steps. Accordingly, on the premise of fully meeting the electrification function of the quartz glass resonator, the area occupied by the metallized film on the surface of the quartz glass hemispherical resonator can be effectively reduced, and the damping introduced by the metallized film can be reduced, thereby significantly improving the quality factor of the resonator and improving its performance.
[0008] To achieve the above object, according to one aspect of the present invention, a method for low-loss metallization coating of a quartz glass hemispherical resonator is provided, characterized in that the method comprises the following steps:
[0009] Step 1: prepare a physical mask to mask the entire outer spherical surface and the inner spherical surface of the quartz glass hemispherical resonator that do not need to be metallized;
[0010] Step 2: Depositing a layer of transition metal film on the end face of the quartz glass hemispherical resonator after the above shielding, the surface of the lower support column and the inner spherical surface of the part to be metallized by magnetron sputtering process;
[0011] Step 3: Continue to use the magnetron sputtering process to deposit a conductive layer on the deposited transition metal film layer, thereby forming a composite metal conductive film layer and realizing the electrification function of the quartz glass hemispherical resonator;
[0012] Step 4: Apply a plurality of conductive strips to connect the composite metal conductive film layer formed on the end surface of the quartz glass hemispherical resonator and the composite metal conductive film layer formed on the surface of the lower support column, and these conductive strips are distributed on the inner spherical surface of the quartz glass hemispherical resonator;
[0013] Step 5: Connect the contact points between the composite metal conductive film layer formed on the end face of the quartz glass hemispherical resonator and the plurality of conductive strips using an inner spherical transition zone, thereby completing the entire low-loss metallization coating process.
[0014] As a further preference, the physical mask is preferably consistent with the curvature of the quartz glass hemispherical resonator and is firm and reliable, leaving no residue on the surface of the quartz glass hemispherical resonator after removal.
[0015] As a further preference, the composition of the transition metal thin film layer is preferably any one of chromium, tantalum, titanium or an alloy thereof.
[0016] As a further preference, the thickness of the transition metal thin film layer is preferably 5 nm to 10 nm.
[0017] As further preferred, the conductive layer is preferably composed of gold or platinum.
[0018] As further preferred, the thickness of the conductive layer is preferably 10 nm to 100 nm.
[0019] As further preferred, the number of the conductive strips is preferably 3n or 4n, wherein n is a natural number greater than or equal to 2.
[0020] As a further preferred embodiment, the main parameter indexes of each of the conductive strips are preferably designed as follows: the width is 2% to 5% of the circumference of the end face of the quartz glass hemispherical resonator, and the length occupies an angle of circumference of
[0021] As a further preference, the height of the inner spherical transition zone is preferably 0.2 mm to 1 mm.
[0022] According to another aspect of the present invention, a corresponding quartz glass hemispherical resonator product is also provided.
[0023] In general, the above technical solution conceived by the present invention has the following technical advantages compared with the prior art:
[0024] (1) The present invention redesigns the operation flow of the entire preparation process. On the premise of fully satisfying the functions of the quartz hemispherical resonator after metallization, it can further reduce the area of the metal conductive layer covering the surface of the quartz hemispherical resonator, reduce the damping of energy consumed when the quartz hemispherical resonator vibrates, greatly improve the quality factor of the quartz hemispherical resonator after metallization coating, and thus improve its performance;
[0025] (2) The present invention arranges a metalized film conductive strip between the plane electrode at the lip position of the quartz hemispherical oscillator and the metal layer of the support rod, thereby not only realizing the electrical conduction between the plane electrode at the lip position and the support rod, but also reducing the influence of the metallization process on the frequency cracking of the resonator by reasonably setting the number of conductive strips;
[0026] (3) The present invention further makes targeted designs for the process parameters and requirements of multiple key steps. For example, by reasonably setting the length and width of the conductive tape, the electrical performance indicators of the resonator metallization can be better met while reducing the coverage area of the metallization film. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is an overall process flow chart of the low-loss metallization coating method of the quartz glass hemispherical resonator according to the present invention;
[0028] Figure 2 It is a schematic diagram of a hemispherical resonator conductive film plating product designed according to the present invention;
[0029] Figure 3 It is a cross-sectional schematic diagram of the conductive film plating of the hemispherical resonator designed according to the present invention;
[0030] Figure 4 is a schematic diagram of a conductive film using 8 conductive strips according to a preferred embodiment of the present invention;
[0031] Figure 5 It is a schematic diagram of a conductive film using 6 conductive strips according to another preferred embodiment of the present invention.
[0032] Throughout the drawings, the same reference numerals are used to denote the same elements or structures, wherein:
[0033] 1- hemispherical resonator, 2- unmetallized inner sphere, 3- transition zone, 4- plane electrode, 5- conductive strip, 6- lower support column, 7- connecting circle. DETAILED DESCRIPTION
[0034] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] Figure 1 The following is a flow chart of the overall process of the low-loss metallization coating method of the quartz glass hemispherical resonator according to the present invention. Figure 1 To explain the present invention in more detail.
[0036] First, a physical mask is prepared to cover the entire outer spherical surface and the partial surface of the inner spherical surface of the quartz glass hemispherical resonator that does not need to be metallized.
[0037] In this step, the physical mask is preferably consistent with the curvature of the quartz glass hemispherical resonator and is firm and reliable, leaving no residue on the surface of the quartz glass hemispherical resonator after removal.
[0038] Next, a layer of transition metal film is deposited on the end face of the quartz glass hemispherical resonator after the above shielding, the surface of the lower support column and the part of the inner spherical surface that needs to be metallized by using a magnetron sputtering process.
[0039] More specifically, a layer of transition metal film is deposited on the unshielded end surface, part of the inner spherical surface and the surface of the lower support rod of the quartz glass resonator using a magnetron sputtering process to increase the adhesion of the conductive layer; the transition metal layer should have Figure 2 The same pattern in the middle.
[0040] Next, a magnetron sputtering process is continued to be used to deposit a conductive layer on the deposited transition metal thin film layer, thereby forming a composite metal conductive film layer together, and at the same time realizing the electrification function of the quartz glass hemispherical resonator.
[0041] According to a preferred embodiment of the present invention, the material of the transition layer metal can be any one of chromium, tantalum, titanium or their alloys; more preferably chromium; the transition layer is prepared by a magnetron sputtering process; the thickness of the transition layer film is 5nm to 10nm, and more preferably the thickness is 5nm.
[0042] According to another preferred embodiment of the present invention, the conductive layer should completely cover the transition layer and have a pattern size consistent with the transition layer; the material of the conductive layer metal can be any one of the precious metals platinum or gold, and gold is more preferably used; the thickness of the conductive layer is 10nm to 100nm, and the thickness is more preferably 50nm.
[0043] Next, a plurality of conductive strips are applied to connect the composite metal conductive film layer formed on the end surface of the quartz glass hemispherical resonator and the composite metal conductive film layer formed on the surface of the lower support column, and these conductive strips are distributed on the inner spherical surface of the quartz glass hemispherical resonator;
[0044] Finally, the contact points between the composite metal conductive film layer formed on the end face of the quartz glass hemispherical resonator and the plurality of conductive strips are connected by an inner spherical transition zone, thereby completing the entire low-loss metallization coating process.
[0045] More specifically, if Figure 2 and Figure 3 As shown in , the resonator plane electrode 4 is connected to the conductive strip 5 through the transition zone 3, the height of the transition zone 3 is 0.2mm-1mm, preferably, the height of the transition zone 3 is 0.2mm; the transition zone 3 is connected to the connecting circle 7 through the conductive strip 5, the number of the conductive strips 5 is 4n (n≥2) or 3n (n≥2), preferably, the number of the conductive strips 5 is 8, see Figure 3 As shown; the width of the conductive strip 5 is 2% to 5% of the circumference of the end face of the resonator. Preferably, the width of the conductive strip 5 occupies an angle of 5 degrees; the length of the conductive strip 5 occupies an angle of Preferably, the length of the conductive strip 5 is the circumferential angle
[0046] The present invention will be explained in more detail below through a number of specific embodiments.
[0047] Example 1
[0048] The method for metallization coating of a hemispherical resonator provided in the first embodiment comprises the following steps: making a physical mask on the surface of the resonator, wherein the mask should cover the surface of the hemispherical resonator that does not need to be coated; using a magnetron sputtering process to deposit a 10 nm thick metal chromium layer on the end surface of the hemispherical resonator, part of the inner spherical surface and the surface of the lower support rod, wherein the metal chromium layer should have a thickness similar to Figure 4 The number of the conductive strips 5 is 8, the width of the conductive strips 5 occupies a circumferential angle of 5 degrees; the length of the conductive strips 5 occupies a circumferential angle A conductive layer with the same pattern size is deposited on the surface of the transition layer by using a magnetron sputtering process; the metal of the conductive layer is gold; and the thickness of the conductive layer is 50 nm.
[0049] Example 2
[0050] The method for metallization coating of a hemispherical resonator provided in the second embodiment comprises the following steps: making a physical mask on the surface of the resonator, wherein the mask should cover the surface of the hemispherical resonator that does not need to be coated; using a magnetron sputtering process to deposit a 5 nm thick metal chromium layer on the end face of the hemispherical resonator, part of the inner spherical surface and the surface of the lower support rod, wherein the metal chromium layer should have a thickness similar to Figure 5 The number of the conductive strips 5 is 6, the width of the conductive strips 5 occupies an angle of 8 degrees; the length of the conductive strips 5 occupies an angle of A conductive layer with the same pattern size is deposited on the surface of the transition layer by using a magnetron sputtering process; the metal of the conductive layer is gold; and the thickness of the conductive layer is 50 nm.
[0051] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A low-loss metallization coating method for a quartz glass hemispherical resonator, characterized in that: The method comprises the following steps: Step 1: prepare a physical mask to mask the entire outer spherical surface and the inner spherical surface of the quartz glass hemispherical resonator that do not need to be metallized; Step 2: Depositing a layer of transition metal film on the end face of the quartz glass hemispherical resonator after the above shielding, the surface of the lower support column and the inner spherical surface of the part to be metallized by magnetron sputtering process; Step 3: Continue to use the magnetron sputtering process to deposit a conductive layer on the deposited transition metal film layer, thereby forming a composite metal conductive film layer and realizing the electrification function of the quartz glass hemispherical resonator; Step 4: A plurality of conductive strips are applied to connect the composite metal conductive film layer formed on the end face of the quartz glass hemispherical resonator and the composite metal conductive film layer formed on the surface of the lower support column, and these conductive strips are distributed on the inner spherical surface of the quartz glass hemispherical resonator; the number of the conductive strips is 3n or 4n, where n is a natural number greater than or equal to 2; the main parameter indicators of each of the conductive strips are designed as follows: the width is 2% to 5% of the circumference of the end face of the quartz glass hemispherical resonator, and the length occupies an angle of circumference of Step 5: Connect the contact points between the composite metal conductive film layer formed on the end face of the quartz glass hemispherical resonator and the plurality of conductive strips using an inner spherical transition zone, thereby completing the entire low-loss metallization coating process.
2. The method according to claim 1, characterized in that The transition metal film layer is composed of any one of chromium, tantalum, titanium or their alloys.
3. The method according to claim 2, characterized in that The thickness of the transition metal thin film layer is 5nm-10nm.
4. The method according to claim 3, characterized in that The conductive layer is made of either gold or platinum.
5. The method according to claim 4, characterized in that The thickness of the conductive layer is 10 nm to 100 nm.
6. The method according to claim 1, characterized in that The height of the inner spherical transition zone is 0.2 mm to 1 mm.
7. A quartz glass hemispherical resonator product, characterized in that: It is prepared by the method according to any one of claims 1 to 6.
8. A hemispherical resonant gyroscope, characterized in that: It has the quartz glass hemispherical resonator as claimed in claim 7.