O3 type sodium ion battery layered positive electrode material and preparation method thereof, positive electrode sheet and sodium ion battery

Through alloying and transition metal doping technology, the prepared NaNixFeyMnzO2@M material solved the irreversible phase change and sensitivity of O3-NaNi0.5Mn0.5O2 positive electrode material, improved the rate performance and preparation efficiency of sodium ion batteries, and achieved the Double improvements in cost and performance.

CN115621458BActive Publication Date: 2024-11-08JIANGSU ZENIO NEW ENERGY BATTERY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211393635.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-08
Publication Date
2024-11-08
Estimated Expiration
2042-11-08

AI Technical Summary

Technical Problem

The complex irreversible phase change and slow kinetic problems of O3-NaNi0.5Mn0.5O2 positive electrode material in sodium ion batteries lead to capacity reduction and poor rate performance, and is sensitive to air, affecting its application.

Method used

High-electron energy alloy powders such as Bi5.6Sn0.4Zn4 or Zn6.5In3.5 are used for alloying. NaNixFeyMnzO2@M is prepared by doping transition metals such as nickel, iron and manganese, combined with extremely cold ice crystals and ultrafast laser sintering technology. Material, reduces sintering temperature and time, and improves rate performance.

Benefits of technology

While ensuring the material tap density and compaction density, the rate performance and preparation efficiency of the positive electrode material of sodium ion battery are improved, cost reduction and electrochemical performance are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115621458B_ABST
    Figure CN115621458B_ABST
Patent Text Reader

Abstract

The invention discloses an O3 type sodium ion battery layered positive electrode material and a preparation method thereof, a positive electrode sheet and a sodium ion battery, and relates to the technical field of batteries; the positive electrode material comprises: NaNi x Fe y Mn z O 2 @M, where M is a high electron energy alloy powder, and 0≤x≤1, 0≤y≤1 and 0≤z≤1, x+y+z=1. On the one hand, the positive electrode material can reduce the solution temperature and time of the material by alloying through the addition of alloy powder, so as to reduce the sintering temperature and time, thereby maintaining the tap density and compaction density of the material while improving the preparation efficiency and reducing the preparation cost; on the other hand, the rate performance of the material can be effectively improved by doping with transition metals, thereby improving the rate performance of the material while ensuring the compaction density and tap density of the material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to an O3 type sodium ion battery layered positive electrode material and a preparation method thereof, a positive electrode sheet and a sodium ion battery. Background Art

[0002] Lithium-ion batteries are widely used in the field of energy equipment. However, the existing lithium element on the earth is very limited, which has caused widespread doubts about whether lithium resources can meet future demand. One way to solve this problem is to develop energy storage devices based on other carriers. Sodium-ion batteries are expected to meet future energy storage needs due to the advantages of abundant sodium resources and low cost, as well as physical and chemical properties similar to lithium-ion batteries. However, since the relative molecular mass of sodium is higher than that of lithium, and the radius of sodium ions is also larger than that of lithium ions, the energy density of sodium-ion batteries will be lower than that of lithium-ion batteries, which greatly hinders the commercial development of sodium-ion batteries. Therefore, the development of high-performance electrode materials is the first problem that needs to be solved for sodium-ion batteries to move towards application.

[0003] Among various cathode materials for sodium-ion batteries, O3-NaNi 0.5 Mn 0.5 O2 has attracted extensive attention due to its advantages of providing sufficient sodium in full batteries, high electrochemical activity, high theoretical specific capacity and easy synthesis. However, it has complex irreversible phase transitions and slow kinetics, which lead to rapid capacity decline and poor rate performance. In addition, the limitations of O3-NaNi 0.5 Mn 0.5 Another major problem in the application of O2 is that it is particularly sensitive to air. When exposed to air, its structure will be destroyed and its electrochemical performance will deteriorate.

[0004] To this end, the existing technology usually adopts the method of doping with heterogeneous elements for improvement. However, although doping can improve the rate performance of the positive electrode material to a certain extent, doping will cause the tap density and compaction density of the material to decrease, thus limiting the application of the material.

[0005] In view of this, the present invention is proposed. Summary of the invention

[0006] The object of the present invention is to provide an O3 type sodium ion battery layered positive electrode material and a preparation method thereof, a positive electrode sheet and a sodium ion battery which can simultaneously ensure the rate performance and tap density of the material.

[0007] The embodiment of the present invention is achieved as follows:

[0008] In a first aspect, the present invention provides an O3 type sodium ion battery layered positive electrode material, comprising:

[0009] NeNix Fe y Mn z O2@M, wherein M is a high electron energy alloy powder, and 0≤x≤1, 0≤y≤1 and 0≤z≤1, x+y+z=1.

[0010] In an optional embodiment, the high electron energy alloy powder is a low melting point alloy and includes Bi2Pb2Hg6, Bi 4.5 Pb 2.3 Sn 0.8 Cd 0.5 In 1.9 、Bi 4.9 Pb 1.8 Sn 1.2 In 2.1 、Bi5Pb 2.7 CdSn 1.3 、Bi 5.2 Pb4Cd 0.8 、Bi 5.3 Pb 3.2 Sn 1.5 、Bi 5.4 Pb 2.6 Cd2、Bi 5.55 Pb 4.45 、Bi 5.6 Sn 0.4 Zn4、Pb 3.5 Zn6In 0.5 、Zn 6.5 In 3.5 At least one of .

[0011] In an alternative embodiment, the high electron energy alloy powder includes Bi 5.6 Sn 0.4 Zn4, and x=y=z=0.33;

[0012] or,

[0013] High electron energy alloy powder including Zn 6.5 In 3.5 , and x=0.4, y=z=0.3.

[0014] In a second aspect, the present invention provides a method for preparing an O3 type sodium ion battery layered positive electrode material according to any one of the aforementioned embodiments, comprising:

[0015] Prepare NaNi x Fe y Mn z The raw materials of O2@M are added with alcohol in proportion and mixed evenly to obtain a mixture;

[0016] The mixture is extremely cold to form ice crystals;

[0017] Breaking ice crystals into powder;

[0018] The powder is sintered to obtain NaNi x Fe y Mn z O2@M.

[0019] In a third aspect, the present invention provides a method for preparing an O3 type sodium ion battery layered positive electrode material according to the aforementioned embodiment, preparing NaNi x Fe y Mn z The raw materials of O2@M include (0.01-1 mol) of nickel-iron-manganese precursor salt, (0.01-1.5 mol) of sodium-containing precursor and (0.01-1 mol) of M metal powder;

[0020] Alternatively, prepare NaNi x Fe y Mn z The raw materials of O2@M include (0.01-1 mol) of transition metal precursors containing nickel, iron and manganese, (0.5-2.5 mol) of sodium-containing precursors and (0.01-1 mol) of M metal powder.

[0021] In an optional embodiment, when preparing NaNi x Fe y Mn z When the raw materials of O2@M include nickel-iron-manganese precursor salt, sodium-containing precursor and M metal powder, the sodium-containing precursor includes at least one of sodium carbonate, sodium hydroxide, sodium oxide, sodium peroxide, sodium phosphate, sodium sulfate, sodium dihydrogen phosphate, sodium dihydrogen sulfate and sodium phenol.

[0022] In an optional embodiment, when preparing NaNi x Fe y Mn z When the raw materials of O2@M include a transition metal precursor containing nickel, iron and manganese, a sodium-containing precursor and M metal powder, the sodium-containing precursor includes at least one of sodium carbonate, sodium hydroxide, sodium oxide, sodium peroxide, sodium phosphate, sodium sulfate, sodium dihydrogen phosphate, sodium dihydrogen sulfate and sodium phenol; the transition metal precursor containing nickel, iron and manganese includes at least one of nickel oxide, nickel-iron oxide, nickel-iron-manganese oxide, manganese oxide, iron oxide, manganese-iron oxide, nickel-manganese oxide, nickel hydroxide, iron hydroxide, manganese hydroxide, nickel-iron hydroxide, nickel-iron-manganese hydroxide and nickel-manganese hydroxide.

[0023] In an optional embodiment, the process of extremely cooling the mixture to form ice crystals is completed by freezing it in a refrigerator for 0.5-3.2 hours;

[0024] And / or, the process of crushing the ice crystals into powder is completed in a crusher for 0.15-1.8 hours;

[0025] And / or, the sintering operation is carried out under the action of mutually intersecting ultrafast laser fields, the sintering temperature is 425-1125° C., and the holding time is 0.5-36 hours.

[0026] In a third aspect, the present invention provides a positive electrode plate, comprising the O3 type sodium ion battery layered positive electrode material of any one of the aforementioned embodiments; or, comprising the O3 type sodium ion battery layered positive electrode material prepared by the preparation method of the O3 type sodium ion battery layered positive electrode material of any one of the aforementioned embodiments.

[0027] In a fourth aspect, the present invention provides a sodium ion battery comprising the positive electrode sheet of the aforementioned embodiment.

[0028] The embodiments of the present invention have at least the following advantages or beneficial effects:

[0029] The layered positive electrode material of an O3 type sodium ion battery provided by the embodiment of the present invention comprises: NaNi x Fe y Mn z O2@M, wherein M is a high electron energy alloy powder, and 0≤x≤1, 0≤y≤1 and 0≤z≤1, x+y+z=1. On the one hand, the positive electrode material can reduce the solution temperature and time of the material by alloying through the addition of alloy powder, so as to reduce the sintering temperature and time, thereby maintaining the tap density and compaction density of the material while improving the preparation efficiency and reducing the preparation cost; on the other hand, the rate performance of the material can be effectively improved by doping with transition metals, thereby improving the rate performance of the material while ensuring the compaction density and tap density of the material.

[0030] The method for preparing the O3 type sodium ion battery layered positive electrode material provided in the embodiment of the present invention can quickly synthesize the above-mentioned O3 type sodium ion battery layered positive electrode material, which can further improve the preparation efficiency and reduce the preparation cost.

[0031] The positive electrode sheet and sodium ion battery provided by the embodiments of the present invention include the above-mentioned positive electrode material. Therefore, they also have the advantages of high rate performance, low manufacturing cost and high efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0033] Figure 1 The first cycle charge and discharge characteristic curve of the O3 type sodium ion battery layered positive electrode material in the sodium ion battery provided in Example 1 of the present invention;

[0034] Figure 2 The scanning electron microscope image of the layered positive electrode material of the O3 type sodium ion battery provided in Example 1 of the present invention;

[0035] Figure 3 The transmission electron microscope spectrum of the O3 type sodium ion battery layered positive electrode material provided in Example 1 of the present invention;

[0036] Figure 4 The XRD (X-ray diffraction pattern) spectrum of the O3 type sodium ion battery layered positive electrode material provided in Example 1 of the present invention;

[0037] Figure 5 The first cycle charge and discharge characteristic curve of the O3 type sodium ion battery layered positive electrode material in the sodium ion battery provided in Example 2 of the present invention. DETAILED DESCRIPTION

[0038] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0039] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0040] The existing technology usually adopts the method of doping with foreign elements to improve the performance. However, although doping can improve the rate performance of the positive electrode material to a certain extent, doping will cause the tap density and compaction density of the material to decrease, thus limiting the application of the material.

[0041] In view of this, the embodiments of the present invention provide an O3 type sodium ion battery layered positive electrode material and a preparation method thereof, a positive electrode sheet and a sodium ion battery that can simultaneously ensure the rate performance and tap density of the material, which are introduced one by one below.

[0042] In an embodiment of the present invention, the layered positive electrode material of the O3 type sodium ion battery comprises: NaNi x Fe y Mn z O2@M, wherein M is a high electron energy alloy powder, and 0≤x≤1, 0≤y≤1 and 0≤z≤1, x+y+z=1.

[0043] On the one hand, by adding alloy powder, the positive electrode material can reduce the solution temperature and time of the material through alloying, so as to reduce the sintering temperature and time, thereby improving the preparation efficiency and reducing the preparation cost while maintaining the material's tap density and compaction density; on the other hand, by doping with transition metals such as Ni, Fe and Mn, the material's rate performance can be effectively improved, thereby improving the material's rate performance while ensuring the material's compaction density and tap density.

[0044] It should be noted that the high electron energy alloy powder is a low melting point alloy and includes Bi2Pb2Hg6, Bi 4.5 Pb 2.3 Sn 0.8 Cd 0.5 In 1.9 、Bi 4.9 Pb 1.8 Sn 1.2 In 2.1 、Bi5Pb 2.7 CdSn 1.3 、Bi 5.2 Pb4Cd 0.8 、Bi 5.3 Pb 3.2 Sn 1.5 、Bi 5.4 Pb 2.6 Cd2、Bi 5.55 Pb 4.45 、Bi 5.6 Sn 0.4 Zn4、Pb 3.5 Zn6In 0.5 、Zn 6.5 In 3.5 At least one of the following. The low melting point alloy contains low melting point elements, which can reduce the crystallization temperature and time of the material, optimize the preparation method and efficiency, and save preparation costs. The use of such a low melting point alloy can maintain a good compaction density and tap density of the material by reducing the sintering temperature and sintering time, so as to ensure the performance of the positive electrode material.

[0045] Exemplarily, the high electron energy alloy powder includes Bi 5.6 Sn 0.4 Zn4, and x=y=z=0.33; or, the high electron energy alloy powder includes Zn 6.5 In 3.5, and x=0.4, y=z=0.3. By selecting the right type of alloy powder and matching the right amount of transition metal elements, the rate performance of the material can be improved, the compaction density and tap density of the material can be ensured, the preparation efficiency of the material can be fully improved, and the preparation cost of the material can be reduced. Of course, in other embodiments of the present invention, the type of high electron energy alloy powder can also be adjusted according to demand, which will not be repeated here.

[0046] An embodiment of the present invention further provides a method for preparing an O3 type sodium ion battery layered positive electrode material, comprising:

[0047] S1: Prepare NaNi x Fe y Mn z The raw materials of O2@M are added with alcohol in proportion and mixed evenly to obtain a mixture;

[0048] S2: The mixture is extremely cooled to form ice crystals;

[0049] S3: crushing ice crystals into powder;

[0050] S4: Sinter the powder to obtain NaNixFeyMnzO2@M.

[0051] In detail, in step S1, NaNi is prepared x Fe y Mn z The raw materials of O2@M include (0.01-1 mol) of nickel-iron-manganese precursor salt, (0.01-1.5 mol) of sodium-containing precursor and (0.01-1 mol) of M metal powder. Alternatively, NaNi x Fe y Mn z The raw materials of O2@M include (0.01-1 mol) of transition metal precursors containing nickel, iron and manganese, (0.5-2.5 mol) of sodium-containing precursors and (0.01-1 mol) of M metal powder. Among them, the sodium-containing precursor includes at least one of sodium carbonate, sodium hydroxide, sodium oxide, sodium peroxide, sodium phosphate, sodium sulfate, sodium dihydrogen phosphate, sodium dihydrogen sulfate and sodium phenol. The transition metal precursors containing nickel, iron and manganese include at least one of nickel oxide, nickel iron oxide, nickel iron manganese oxide, manganese oxide, iron oxide, manganese iron oxide, nickel manganese oxide, nickel hydroxide, iron hydroxide, manganese hydroxide, nickel iron hydroxide, nickel iron manganese hydroxide and nickel manganese hydroxide. M metal powder includes Bi2Pb2Hg6, Bi 4.5 Pb 2.3 Sn 0.8 Cd 0.5 In 1.9 、Bi 4.9 Pb 1.8 Sn 1.2In 2.1 、Bi5Pb 2.7 CdSn 1.3 、Bi 5.2 Pb4Cd 0.8 、Bi 5.3 Pb 3.2 Sn 1.5 、Bi 5.4 Pb 2.6 Cd2、Bi 5.55 Pb 4.45 、Bi 5.6 Sn 0.4 Zn4、Pb 3.5 Zn6In 0.5 、Zn 6.5 In 3.5 That is, in the preparation process, the material can be prepared by using either a precursor salt or various metal precursors, and the material prepared by using the precursor has better performance.

[0052] In step S2, the process of extremely cooling the mixture to form ice crystals is completed in a refrigerator for 0.5-3.2 hours, and the freezing temperature of the refrigerator is below zero degrees Celsius to ensure that ice crystals can be formed. By preparing the material to form ice crystals, the stability of the material structure can be improved, and impurities in the material can be removed, which can provide conditions for the clean phase of the alloying operation, fully guarantee the rate performance of the material, and ensure the tap density and compaction density of the material.

[0053] In step S3, the process of crushing the ice crystals into powder is completed in the crusher for 0.15-1.8 hours. Through the crushing operation, the ice crystals can be crushed into a small particle powder structure to ensure the reliability and stability of the sintering operation, the compaction density and tap density of the prepared material, and the electrochemical performance of the material.

[0054] In step S4, the sintering operation is carried out under the action of mutually intersecting ultrafast laser fields, and the sintering temperature is 425-1125°C, preferably, 580°C-1100°C, or 750°C, etc.; the holding time is 0.5-36h, preferably, 0.15-1.8h. By using laser field heating, the heating temperature can be quickly increased, so that the material can quickly reach the crystallization point, accelerate the material synthesis speed, fully improve the preparation efficiency, and save preparation costs. At the same time, the mutually intersecting laser fields can also activate the internal electronic activity of the material and accelerate the alloying process to ensure the rate performance of the material and ensure the tap density and compaction density of the material.

[0055] The embodiment of the present invention further provides a positive electrode sheet, which is prepared by the above-mentioned sodium ion battery layered positive electrode material. Therefore, it also has the advantages of excellent rate performance, and the tap density and compaction density can be guaranteed.

[0056] In detail, the positive electrode plate includes a positive current collector and a positive active material layer disposed on at least one side of the current collector. The positive active material layer is obtained by coating the positive electrode slurry on the current collector, drying it, and cold pressing it. The positive electrode slurry includes an O3 type sodium ion battery layered positive electrode material, a conductive agent, a binder, and a solvent. Among them, the current collector can be selected as aluminum foil, the conductive agent and the binder each account for less than or equal to 5%, the conductive agent can be selected as carbon black, carbon nanotubes, graphene, etc., the binder can be selected as polyvinylidene chloride (PVDF), and the solvent can be selected as N-methylpyrrolidone (NMP).

[0057] Specifically, when preparing the positive electrode sheet, the prepared raw materials can be weighed first, and the positive electrode material: conductive carbon: PVDF are mixed in a mass ratio of 94:3:3, and then dissolved in a certain amount of NMP. After stirring evenly, it is coated on the current collector, and then dried and cut into pieces to obtain the positive electrode sheet.

[0058] The embodiment of the present invention further provides a sodium ion battery, which comprises the above-mentioned positive electrode plate. Therefore, the sodium ion battery also has the advantages of excellent rate performance, and the tap density and compaction density can be guaranteed.

[0059] At the same time, the sodium ion battery specifically includes a shell, a positive electrode sheet, a diaphragm, a negative electrode sheet and an electrolyte. Among them, the positive electrode sheet, the diaphragm and the negative electrode sheet are stacked, and a bare cell is formed by lamination or winding. The bare cell is loaded into the shell and injected with electrolyte to obtain a battery. Exemplarily, a winding process can be used to prepare a bare cell. The diaphragm is first wound 5 / 6 turns, and then the positive electrode sheet and the negative electrode sheet are wound in turn, a total of 8 turns are wound, and finally the positive electrode sheet is wound to ensure that the negative electrode sheet is completely wrapped in the positive electrode sheet. The finished winding core is welded with the pole ears and glued, and then it is sealed with aluminum-plastic film, baked in a vacuum oven for 40-120 hours, taken out, and the water content is tested (H2O<200ppm is required), and then the sodium ion battery is obtained after the injection, sealing, aging, formation and volume separation tests according to a certain injection coefficient and ratio.

[0060] Among them, the negative electrode sheet may include a current collector and a negative electrode active material layer, the current collector may be selected as copper foil, and the negative electrode active material layer is obtained by coating the negative electrode active slurry on the current collector, drying and cold pressing. Among them, the negative electrode active slurry includes a negative electrode material, a conductive agent, a binder, a dispersant and a solvent. The amount of the conductive agent and the binder is less than or equal to 10%, and the negative electrode material can be selected as soft carbon, hard carbon or composite carbon, etc. The conductive agent can be selected as conductive carbon black, conductive graphite, vapor-grown carbon fiber, carbon nanotubes, etc. The binder can be selected as styrene-butadiene rubber, the dispersant can be selected as CMC, and the solvent can be selected as N-methylpyrrolidone (NMP). Exemplarily, it can be selected that the mass ratio of negative electrode hard carbon material: conductive carbon: CMC / SBR is 85:10:5. In addition, the electrolyte is obtained by dissolving 1M sodium hexafluorophosphate in a solvent with a volume ratio of EC:DEC=1:1+5%FEC.

[0061] Specifically, when preparing the negative electrode sheet, the raw materials to be prepared can be weighed first, and the negative electrode hard carbon material: conductive carbon: CMC / SBR mass ratio of 85:10:5 are mixed, and then dissolved in a certain amount of NMP, stirred evenly and coated on the current collector, and then dried and cut to obtain the negative electrode sheet.

[0062] The preparation process and performance of the battery are described in detail below in conjunction with specific examples and comparative examples:

[0063] Example 1

[0064] This embodiment provides a sodium ion battery, which is prepared by the following method:

[0065] S1: Preparation of positive electrode sheet, including:

[0066] S11: Preparation of layered positive electrode materials for O3-type sodium ion batteries, specifically including:

[0067] Sa: Precursors sodium carbonate, nickel iron manganese hydroxide and Zn 6.5 In 3.5 The alloy powder was placed in a stirring tank according to a certain stoichiometric ratio (molar ratio of 0.505:1:0.1) and 45 ml of alcohol (ethanol) was added to obtain a mixture;

[0068] Sb: The mixture was placed in a refrigerator to cool for 1.5 h to obtain ice crystals;

[0069] Sc: crush the ice crystals in an ice crystal crusher for 0.5 h to obtain powder;

[0070] Sd: The powder was quickly transferred into a laser field assisted sintering furnace and heated at 615°C for 2.5 hours at a heating rate of 1-10°C / min to obtain NaNi 0.4 Fe 0.3 Mn0.3 O2@Zn 6.5 In 3.5 Positive electrode material.

[0071] S12: NaNi 0.4 Fe 0.3 Mn 0.3 O2@Zn 6.5 In 3.5 The positive electrode material: conductive carbon: PVDF are mixed in a mass ratio of 90:5:5, then dissolved in a certain amount of NMP, stirred evenly and coated on the current collector, and then dried and cut into pieces to obtain the positive electrode sheet.

[0072] S2: Preparation of negative electrode sheet, specifically including:

[0073] The negative electrode hard carbon material: conductive carbon: CMC / SBR are mixed in a mass ratio of 85:10:5, then dissolved in a certain amount of NMP, stirred evenly and coated on the current collector, and then dried and cut into pieces to obtain the negative electrode sheet.

[0074] S3: Preparation of sodium ion batteries, including:

[0075] The positive electrode sheet, the separator and the negative electrode sheet are arranged in sequence and wound to prepare a bare battery cell, and then the bare battery cell is placed in a shell and injected with electrolyte; the battery after injection is left to stand, pre-charged, exhaust gas is evacuated, sealed, and capacity is divided to prepare a sodium ion battery.

[0076] Example 2

[0077] This embodiment provides a sodium ion battery, which is different from the preparation method of the sodium ion battery provided in Example 1 in that:

[0078] Step S11: Preparation of O3 type sodium ion battery layered positive electrode material, specifically comprising:

[0079] Sa: Precursors sodium carbonate, Zn6.5In3.5, nickel nitrate, ferrous oxalate and manganese oxide are contacted in a stoichiometric ratio (molar ratio of 0.505:0.1:0.4:0.3:0.3) to form a mixed powder, the mixed powder is placed in a stirring tank and 45 ml of alcohol (ethanol) is added to obtain a mixture;

[0080] Sb: The mixture was placed in a refrigerator to cool for 1.5 h to obtain ice crystals;

[0081] Sc: crush the ice crystals in an ice crystal crusher for 0.5 h to obtain powder;

[0082] Sd: The powder was quickly transferred into a laser field assisted sintering furnace and heated at 615°C for 2.5 hours at a heating rate of 1-10°C / min. After the sintering, the material was taken out and the remaining proportion (0.05 mol) of sodium carbonate was added. After stirring for 0.5 hours, the powder was transferred into the furnace for secondary sintering at a temperature of about 625°C and a holding time of 1.5 hours to obtain NaNi 0.4 Fe 0.3 Mn 0.3 O2@Zn 6.5 In 3.5 Positive electrode material.

[0083] Example 3

[0084] This embodiment provides a sodium ion battery, which is different from the preparation method of the sodium ion battery provided in Example 1 in that:

[0085] Step S11: Preparation of O3 type sodium ion battery layered positive electrode material, specifically comprising:

[0086] Sa: Precursors sodium carbonate, nickel iron manganese hydroxide, zinc sulfate, and indium oxide are placed in a stirring tank according to a certain stoichiometric ratio (molar ratio of 0.505:1:0.65:0.175) and 45 ml of alcohol (ethanol) is added to obtain a mixture;

[0087] Sb: The mixture was placed in a refrigerator to cool for 1.5 h to obtain ice crystals;

[0088] Sc: crush the ice crystals in an ice crystal crusher for 0.5 h to obtain powder;

[0089] Sd: The powder was quickly transferred into a laser field assisted sintering furnace and heated at 615°C for 2.5 hours at a heating rate of 1-10°C / min to obtain NaNi 0.4 Fe 0.3 Mn 0.3 O2@Zn 6.5 In 3.5 Positive electrode material.

[0090] Example 4

[0091] This embodiment provides a sodium ion battery, which is different from the preparation method of the sodium ion battery provided in Example 1 in that:

[0092] Step S11: Preparation of O3 type sodium ion battery layered positive electrode material, specifically comprising:

[0093] Sa: Precursors sodium carbonate, zinc sulfate, indium oxide, nickel nitrate, ferrous oxalate and manganese oxide are contacted in a stoichiometric ratio (molar ratio of 0.505:0.65:0.175:0.4:0.3:0.3) to obtain a mixed powder, the mixed powder is placed in a stirring tank and 45 ml of alcohol (ethanol) is added to obtain a mixture;

[0094] Sb: The mixture was placed in a refrigerator to cool for 1.5 h to obtain ice crystals;

[0095] Sc: crush the ice crystals in an ice crystal crusher for 0.5 h to obtain powder;

[0096] Sd: The powder was quickly transferred into a laser field assisted sintering furnace and heated at 615°C for 2.5 hours at a heating rate of 1-10°C / min. After the sintering, the material was taken out and the remaining proportion (0.05 mol) of sodium carbonate was added. After stirring for 0.5 hours, the powder was transferred into the furnace for secondary sintering at a temperature of about 625°C and a holding time of 1.5 hours to obtain NaNi 0.4 Fe 0.3 Mn 0.3 O2@Zn 6.5 In 3.5 Positive electrode material.

[0097] Example 5

[0098] This embodiment provides a sodium ion battery, which is different from the preparation method of the sodium ion battery provided in Example 1 in that:

[0099] Sa: Precursors sodium carbonate, nickel iron manganese hydroxide and Bi 5.6 Sn 0.4 Zn4 alloy powder was placed in a stirring tank according to a certain stoichiometric ratio (molar ratio of 0.505:1:0.1) and 45 ml of alcohol (ethanol) was added to obtain a mixture;

[0100] Sb: The mixture was placed in a refrigerator to cool for 1.5 h to obtain ice crystals;

[0101] Sc: crush the ice crystals in an ice crystal crusher for 0.5 h to obtain powder;

[0102] Sd: The powder was quickly transferred into a laser field assisted sintering furnace and heated at 615°C for 2.5 hours at a heating rate of 1-10°C / min to obtain NaNi 0.4 Fe 0.3 Mn 0.3 O2@Bi 5.6 Sn 0.4 Zn4 positive electrode material.

[0103] Example 6

[0104] This embodiment provides a sodium ion battery, which is different from the preparation method of the sodium ion battery provided in Example 1 in that:

[0105] Step S11: Preparation of O3 type sodium ion battery layered positive electrode material, specifically comprising:

[0106] Sa: Precursors sodium carbonate, Bi 5.6 Sn 0.4 Zn4, nickel nitrate, ferrous oxalate and manganese oxide are contacted to form a mixed powder, the mixed powder is placed in a stirring tank and 45 ml of alcohol (ethanol) is added to obtain a mixture;

[0107] Sb: The mixture was placed in a refrigerator to cool for 1.5 h to obtain ice crystals;

[0108] Sc: crush the ice crystals in an ice crystal crusher for 0.5 h to obtain powder;

[0109] Sd: The powder was quickly transferred into a laser field assisted sintering furnace and heated at 615°C for 2.5 hours at a heating rate of 1-10°C / min. After the sintering, the material was taken out and the remaining proportion (0.05 mol) of sodium carbonate was added. After stirring for 0.5 hours, the powder was transferred into the furnace for secondary sintering at a temperature of about 625°C and a holding time of 1.5 hours to obtain NaNi 0.4 Fe 0.3 Mn 0.3 O2@Bi 5.6 Sn 0.4 Zn4 positive electrode material.

[0110] Example 7

[0111] This embodiment provides a sodium ion battery, which is different from the preparation method of the sodium ion battery provided in Example 1 in that:

[0112] Step S11: Preparation of O3 type sodium ion battery layered positive electrode material, specifically comprising:

[0113] Sa: Precursors sodium carbonate, nickel iron manganese hydroxide, zinc sulfate, indium oxide, and bismuth oxide are placed in a stirring tank according to a certain stoichiometric ratio (molar ratio of 0.505:1:0.45:0.175:0.2) and 45 ml of alcohol (ethanol) is added to obtain a mixture;

[0114] Sb: The mixture was placed in a refrigerator to cool for 1.5 h to obtain ice crystals;

[0115] Sc: crush the ice crystals in an ice crystal crusher for 0.5 h to obtain powder;

[0116] Sd: The powder was quickly transferred into a laser field assisted sintering furnace and heated at 615°C for 2.5 hours at a heating rate of 1-10°C / min to obtain NaNi 0.4 Fe 0.3 Mn 0.3 O2@Bi 5.6 Sn 0.4 Zn4 positive electrode material.

[0117] Example 8

[0118] This embodiment provides a sodium ion battery, which is different from the preparation method of the sodium ion battery provided in Example 1 in that:

[0119] Step S11: Preparation of O3 type sodium ion battery layered positive electrode material, specifically comprising:

[0120] Sa: Precursors sodium carbonate, zinc sulfate, indium oxide, bismuth oxide, nickel nitrate, ferrous oxalate and manganese oxide are contacted in a stoichiometric ratio (molar ratio of 0.505:0.45:0.175:0.2:0.4:0.3:0.3) to obtain a mixed powder, the mixed powder is placed in a stirring tank and 45 ml of alcohol (ethanol) is added to obtain a mixture;

[0121] Sb: The mixture was placed in a refrigerator to cool for 1.5 h to obtain ice crystals;

[0122] Sc: crush the ice crystals in an ice crystal crusher for 0.5 h to obtain powder;

[0123] Sd: The powder was quickly transferred into a laser field assisted sintering furnace and heated at 615°C for 2.5 hours at a heating rate of 1-10°C / min. After the sintering, the material was taken out and the remaining proportion (0.05 mol) of sodium carbonate was added. After stirring for 0.5 hours, the powder was transferred into the furnace for secondary sintering at a temperature of about 625°C and a holding time of 1.5 hours to obtain NaNi 0.4 Fe 0.3 Mn 0.3 O2@Bi 5.6 Sn 0.4 Zn4 positive electrode material.

[0124] Comparative Example 1

[0125] Comparative Example 1 provides a sodium ion battery, which is different from the preparation method of the sodium ion battery provided in Example 1 in that, in the preparation process of the positive electrode material, a mixed heating method is used to directly mix all the raw materials and then heat them to obtain NaZn 0.1 In 0.1 Ni 0.2 Fe 0.3 Mn 0.3 O2 positive electrode material.

[0126] Comparative Example 2

[0127] Comparative Example 2 provides a sodium ion battery, which differs from the preparation method of the sodium ion battery provided in Example 1 in that no alloy powder is added during the preparation of the positive electrode material, and the positive electrode material prepared is NaNi 0.4 Fe 0.3 Mn 0.3 O2.

[0128] Experimental Example 1

[0129] The sodium ion batteries prepared in Example 1 and Example 2 were tested for capacity. Figure 1 The first cycle charge and discharge characteristic curve of the O3 type sodium ion battery layered positive electrode material in the sodium ion battery provided in Example 1 of the present invention; Figure 2 A scanning electron microscope image of an O3-type sodium ion battery layered positive electrode material provided by an embodiment of the present invention; Figure 3 Transmission electron microscope spectrum of the layered positive electrode material of the O3 type sodium ion battery provided by the embodiment of the present invention; Figure 4 The XRD (X-ray diffraction pattern) spectrum of the O3 type sodium ion battery layered positive electrode material provided in Example 1 of the present invention; Figure 5 The first cycle charge and discharge characteristic curve of the O3 type sodium ion battery layered positive electrode material in the sodium ion battery provided by Example 2 of the present invention. Figures 1 to 4 The initial capacity curve of the battery prepared in Example 1 tested at a current density of 0.1C shows that an initial specific capacity of about 123.4 mA h / g is achieved in the voltage range of 2-4 V. The material is in the form of pellets. Figure 2 It can be clearly observed that the material has excellent electrical conductivity. Figure 3 It can be seen that the material has indeed achieved alloying, and the degree of alloying is very high and very uniform. Figure 4 The diffraction pattern shows that the prepared material is indeed an O3 phase layered oxide, which is consistent with the description in mainstream literature. In addition, the peaks at 32.5° and 42.5° in the figure are impurity peaks introduced by the alloy compound Zn6.5In3.5.

[0130] See also Figure 5 The initial capacity curve of the sodium ion battery prepared in Example 2 tested at a current density of 0.1C shows that an initial specific capacity of about 117 mA h / g is achieved in the voltage range of 2-4 V, and has very excellent conductive properties. However, compared with Example 1, the effect is slightly worse.

[0131] according to Figures 1 to 5It can be seen from the comparison that the positive electrode material provided by the embodiment of the present invention can effectively improve the rate performance of the material, thereby improving the rate performance of the material while ensuring the compaction density and tap density of the material. At the same time, it can be seen from the comparison between Example 1 and Example 2 that the use of nickel-iron-manganese precursor salt to prepare the positive electrode material can improve the rate performance of the positive electrode material compared to the use of transition metal precursors containing nickel, iron and manganese.

[0132] Experimental Example 2

[0133] The sodium ion batteries provided in Examples 1-8 and Comparative Examples 1-2 were subjected to discharge specific capacity test, initial coulomb efficiency test, and rate performance test under the same conditions. Among them, the discharge specific capacity test was carried out at a current density of 0.1C, and the test conditions were charge first and then discharge, constant current charging, and the current was 0.1C corresponding to the calculated current. For the coulomb efficiency test, the test conditions were charge first and then discharge, constant current charging, and the current was 0.1C corresponding to the calculated current. For the rate performance test, the test conditions were charge first and then discharge, constant current charging, and the current was 0.1C corresponding to the calculated current. At the same time, the tap density of the positive electrode material was measured, and the measurement results are shown in Table 1, and in Table 1, method 1 is the preparation method of Example 1, method 2 is the preparation method of Example 2, method 3 is the preparation method of Example 3, method 4 is the preparation method of Example 4, and method 5 is the preparation method of Example 5.

[0134] Table 1. Test results

[0135]

[0136]

[0137] According to the comparison of Examples 1-8 and Comparative Example 1 in Table 1, it can be seen that the alloying synthesis method provided by the embodiment of the present invention can effectively improve the rate performance of the battery, and can ensure the tap density of the material. According to the comparison of Examples 1-8 and Comparative Example 2 in Table 1, it can be seen that the O3 type sodium ion battery layered positive electrode material provided by the embodiment of the present invention can reduce the solution temperature and time of the material by alloying to reduce the sintering temperature and time, thereby maintaining the tap density and compaction density of the material while improving the preparation efficiency and reducing the preparation cost, and can effectively improve the rate performance of the material, thereby ensuring the compaction density and tap density of the material while improving the rate performance of the material. At the same time, according to the comparison of Example 1 and Example 5 in Table 1, as well as Example 2 and Example 6, as well as Example 3 and Example 7, and Example 4 and Example 8 alone, the positive electrode material prepared by using Zn6.5In3.5 alloy powder improves the electrochemical performance of the battery to a higher degree than the positive electrode material prepared by using Bi5.6Sn0.4Zn4 alloy powder.

[0138] In summary, the positive electrode material provided by the embodiment of the present invention can reduce the solution temperature and time of the material by alloying through the addition of alloy powder, so as to reduce the sintering temperature and time, thereby maintaining the tap density and compaction density of the material while improving the preparation efficiency and reducing the preparation cost; at the same time, the positive electrode material provided by the embodiment of the present invention can effectively improve the rate performance of the material by doping with transition metals, thereby improving the rate performance of the material while ensuring the compaction density and tap density of the material. In addition, the preparation method of the positive electrode material provided by the embodiment of the present invention can also further improve the preparation efficiency and improve the rate performance of the material to improve the electrochemical performance of the sodium ion battery.

[0139] In summary, the embodiments of the present invention provide an O3 type sodium ion battery layered positive electrode material and a preparation method thereof, a positive electrode sheet and a sodium ion battery that can simultaneously ensure the rate performance and tap density of the material.

[0140] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. An O3 type sodium ion battery layered positive electrode material, characterized in that: include: NeNi x Fe y Mn z O2@M, where M is a high electron energy alloy powder, and 0≤x≤1, 0≤y≤1 and 0≤z≤1, x+y+z=1; The high electron energy alloy powder is a low melting point alloy and includes Bi2Pb2Hg6, Bi 4.5 Pb 2.3 Sn 0.8 Cd 0.5 In 1.9 、Bi 4.9 Pb 1.8 Sn 1.2 In 2.1 、Bi5Pb 2.7 CdSn 1.3 、Bi 5.2 Pb4Cd 0.8 、Bi 5.3 Pb 3.2 Sn 1.5 、Bi 5.4 Pb 2.6 Cd2、Bi 5.55 Pb 4.45 、Bi 5.6 Sn 0.4 Zn4、Pb 3.5 Zn6In 0.5 、Zn 6.5 In 3.5 At least one of .

2. The O3 type sodium ion battery layered positive electrode material according to claim 1, characterized in that: The high electron energy alloy powder includes Zn 6.5 In 3.5 , and x=0.4, y=z=0.

3.

3. A method for preparing an O3 type sodium ion battery layered positive electrode material according to any one of claims 1 to 2, characterized in that: include: The NaNi x Fe y Mn z The raw materials of O2@M are added with alcohol in proportion and mixed evenly to obtain a mixture; Extremely cooling the mixture to form ice crystals; crushing the ice crystals to form a powder; The powder is sintered to obtain the NaNi x Fe y Mn z O2@M.

4. The method for preparing the layered positive electrode material for an O3 type sodium ion battery according to claim 3, characterized in that: Preparation of the NaNi x Fe y Mn z The raw materials of O2@M include 0.01-1 mol of nickel-iron-manganese precursor salt, 0.01-1.5 mol of sodium-containing precursor and 0.01-1 mol of M metal powder; Alternatively, the NaNi x Fe y Mn z The raw materials of O2@M include 0.01-1 mol of transition metal precursor containing nickel, iron and manganese, 0.5-2.5 mol of sodium-containing precursor and 0.01-1 mol of M metal powder.

5. The method for preparing the layered positive electrode material for an O3 type sodium ion battery according to claim 4, characterized in that: When preparing the NaNi x Fe y Mn z When the raw materials of O2@M include nickel-iron-manganese precursor salt, a sodium-containing precursor and M metal powder, the sodium-containing precursor includes at least one of sodium carbonate, sodium hydroxide, sodium oxide, sodium peroxide, sodium phosphate, sodium sulfate, sodium dihydrogen phosphate, sodium dihydrogen sulfate and sodium phenol.

6. The method for preparing the layered positive electrode material for an O3 type sodium ion battery according to claim 4, characterized in that: When preparing the NaNi x Fe y Mn z When the raw materials of O2@M include a transition metal precursor containing nickel, iron and manganese, a sodium-containing precursor and M metal powder, the sodium-containing precursor includes at least one of sodium carbonate, sodium hydroxide, sodium oxide, sodium peroxide, sodium phosphate, sodium sulfate, sodium dihydrogen phosphate, sodium dihydrogen sulfate and sodium phenol; the transition metal precursor containing nickel, iron and manganese includes at least one of nickel oxide, nickel-iron oxide, nickel-iron-manganese oxide, manganese oxide, iron oxide, manganese-iron oxide, nickel-manganese oxide, nickel hydroxide, iron hydroxide, manganese hydroxide, nickel-iron hydroxide, nickel-iron-manganese hydroxide and nickel-manganese hydroxide.

7. The method for preparing the layered positive electrode material for an O3 type sodium ion battery according to claim 3, characterized in that: The process of extremely cooling the mixture to form the ice crystals is completed by freezing in a refrigerator for 0.5-3.2 hours; And / or, the process of crushing the ice crystals to form the powder is completed in a crusher for 0.15-1.8 hours; And / or, the sintering operation is carried out under the action of mutually intersecting ultrafast laser fields, the sintering temperature is 425-1125° C., and the holding time is 0.5-36 hours.

8. A positive electrode sheet, characterized in that: The invention relates to an O3 type sodium ion battery layered positive electrode material comprising any one of claims 1 to 2; or an O3 type sodium ion battery layered positive electrode material prepared by the method for preparing the O3 type sodium ion battery layered positive electrode material according to any one of claims 3 to 7.

9. A sodium ion battery, characterized in that: Including the positive electrode sheet as described in claim 8.