Glass-ceramics, glass-ceramics products and methods for producing the same
By rationally designing the component ratio and chemical strengthening process of microcrystalline glass, microcrystalline glass products with xiashi crystal phase are formed, which solves the problem of insufficient mechanical properties of existing microcrystalline glass and achieves significant improvements in high strength and impact resistance. , suitable for display and electronic devices.
Patent Information
- Application Number
- CN202211309432.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-25
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-10-25
AI Technical Summary
The existing microcrystalline glass has shortcomings in terms of mechanical properties and is difficult to meet the high requirements of display equipment or electronic equipment, especially in terms of bending, wear and drop resistance.
By reasonably designing the component ratio of microcrystalline glass, it contains components such as SiO2, Al2O3, Li2O and Na2O, forming a crystalline phase, and improving its mechanical properties through chemical strengthening processes to prepare microcrystalline glass products with excellent mechanical properties.
It realizes the high strength, wear resistance and impact resistance of microcrystalline glass products, meets the application needs of display equipment or electronic equipment, and has excellent mechanical properties.
Smart Images

Figure BDA0003907385090000391 
Figure BDA0003907385090000401 
Figure BDA0003907385090000402
Abstract
Description
Technical Field
[0001] The present invention relates to a glass-ceramic, and in particular to a glass-ceramic with excellent mechanical properties, a glass-ceramic product and a manufacturing method thereof. Background Art
[0002] In recent years, with the continuous rise and development of consumer electronic products, glass, as a transparent and high-performance material, has been widely used in such electronic devices. For example, LED and LCD displays and computer monitors, portable electronic products (such as mobile phones, tablets and personal media terminals, etc.), the glass used in them not only needs to withstand the regular "touch" contact from the application for a long time, but also needs to withstand the accidental bending, scratches and impacts that may occur during use, which puts higher requirements on the relevant performance of the glass.
[0003] Glass-ceramics is a material that is formed by heat-treating the glass to precipitate crystals inside the glass. It has better mechanical properties than conventional glass. The microcrystals formed in the glass have obvious advantages over conventional glass in terms of bending resistance, wear resistance, and drop resistance. On the other hand, the mechanical properties of glass-ceramics can be further improved through chemical strengthening. Based on the above advantages, glass-ceramics or glass-ceramics products obtained after treatment are currently used in display devices or electronic devices with high requirements for drop resistance, pressure resistance, and scratch resistance, especially in the front and back covers of portable electronic devices (such as mobile phones, watches, PADs, etc.).
[0004] Therefore, developing a glass-ceramic and glass-ceramic product with excellent mechanical properties and suitable for display devices or electronic devices has become the goal pursued by scientific and technological personnel. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a microcrystalline glass and microcrystalline glass products with excellent mechanical properties.
[0006] The technical solution adopted by the present invention to solve the technical problem is:
[0007] (1) Microcrystalline glass products, whose components, expressed in weight percentage, contain: SiO2: 40-60%; Al2O3: 20-40%; Li2O: 2-15%; Na2O: 3-20%; P2O5+ZrO2: 1-15%.
[0008] (2) The microcrystalline glass product according to (1), wherein the components, expressed in weight percentage, further contain: K2O: 0-8%; and / or ZnO: 0-6%; and / or B2O3: 0-6%; and / or RO: 0-8%; and / or TiO2: 0-5%; and / or Ln2O3: 0-5%; and / or clarifier: 0-2%, wherein RO is one or more of MgO, CaO, SrO, and BaO, and Ln2O3 is one or more of La2O3, Gd2O3, and Y2O3.
[0009] (3) Microcrystalline glass products, whose components, expressed in weight percentage, are composed of SiO2: 40-60%; Al2O3: 20-40%; Li2O: 2-15%; Na2O: 3-20%; P2O5+ZrO2: 1-15%; K2O: 0-8%; ZnO: 0-6%; B2O3: 0-6%; RO: 0-8%; TiO2: 0-5%; Ln2O3: 0-5%; and clarifier: 0-2%, wherein RO is one or more of MgO, CaO, SrO, and BaO, and Ln2O3 is one or more of La2O3, Gd2O3, and Y2O3.
[0010] (4) A microcrystalline glass product, wherein the components thereof include SiO2, Al2O3, Li2O and Na2O, the microcrystalline glass product contains a nepheline crystal phase, and the surface stress of the microcrystalline glass product is above 150 MPa.
[0011] (5) A glass-ceramic product, wherein the main crystal phase contains a nepheline crystal phase, and the Vickers hardness of the glass-ceramic product is 750 kgf / mm 2 above.
[0012] (6) Microcrystalline glass products, whose components, expressed in weight percentage, contain SiO2: 40-60%; Al2O3: 20-40%; Li2O: 2-15%; Na2O: 3-20%, and the microcrystalline glass products contain nepheline crystal phase.
[0013] (7) Glass-ceramic products, the components of which include SiO2, Al2O3, Li2O and Na2O, and the four-point bending strength of the glass-ceramic products with a thickness of less than 1 mm is greater than 700 MPa.
[0014] (8) A microcrystalline glass product, wherein the components thereof include SiO2, Al2O3, Li2O and Na2O, and the haze of the microcrystalline glass product having a thickness of less than 1 mm is less than 0.15%.
[0015] (9) Microcrystalline glass products containing nepheline crystal phase, wherein the microcrystalline glass products having a thickness of less than 1 mm have a light transmittance of more than 88% at a wavelength of 550 nm.
[0016] (10) A microcrystalline glass product comprising a nepheline crystal phase, wherein the depth of the ion exchange layer of the microcrystalline glass product is greater than 50 μm.
[0017] (11) The microcrystalline glass product according to any one of (4) to (10), wherein its components, expressed in weight percentage, contain: SiO2: 40 to 60%; and / or Al2O3: 20 to 40%; and / or Li2O: 2 to 15%; and / or Na2O: 3 to 20%; and / or P2O5+ZrO2: 1 to 15%.
[0018] (12) The microcrystalline glass product according to any one of (4) to (11), wherein the components, expressed in weight percentage, further contain: K2O: 0-8%; and / or ZnO: 0-6%; and / or B2O3: 0-6%; and / or RO: 0-8%; and / or TiO2: 0-5%; and / or Ln2O3: 0-5%; and / or clarifier: 0-2%, wherein RO is one or more of MgO, CaO, SrO, and BaO, and Ln2O3 is one or more of La2O3, Gd2O3, and Y2O3.
[0019] (13) The microcrystalline glass product according to any one of (1) to (12), wherein the components are expressed in weight percentage, wherein: (Al2O3+Na2O) / P2O5 is 3.0 to 30.0, preferably (Al2O3+Na2O) / P2O5 is 4.0 to 20.0, more preferably (Al2O3+Na2O) / P2O5 is 5.0 to 15.0, and further preferably (Al2O3+Na2O) / P2O5 is 6.0 to 10.0.
[0020] (14) The microcrystalline glass product according to any one of (1) to (13), wherein the components are expressed in weight percentage, wherein: SiO2 / Al2O3 is 1.2 to 2.8, preferably SiO2 / Al2O3 is 1.3 to 2.5, more preferably SiO2 / Al2O3 is 1.5 to 2.2, and further preferably SiO2 / Al2O3 is 1.6 to 2.0.
[0021] (15) The microcrystalline glass product according to any one of (1) to (14), wherein the components are expressed in weight percentage, wherein: SiO2 / (Na2O+B2O3) is 2.0 to 15.0, preferably SiO2 / (Na2O+B2O3) is 3.0 to 10.0, more preferably SiO2 / (Na2O+B2O3) is 4.0 to 8.0, and further preferably SiO2 / (Na2O+B2O3) is 5.0 to 7.0.
[0022] (16) The glass-ceramic product according to any one of (1) to (15), wherein the components are expressed in weight percentage, wherein: (Na2O+Li2O) / SiO2 is 0.1 to 0.8, preferably (Na2O+Li2O) / SiO2 is 0.15 to 0.7, more preferably (Na2O+Li2O) / SiO2 is 0.2 to 0.6, and further preferably (Na2O+Li2O) / SiO2 is 0.25 to 0.5.
[0023] (17) The microcrystalline glass product according to any one of (1) to (16), wherein the components are expressed in weight percentage, wherein: (ZrO2+ZnO) / Na2O is less than 2.0, preferably (ZrO2+ZnO) / Na2O is less than 1.5, more preferably (ZrO2+ZnO) / Na2O is 0.01 to 1.0, and further preferably (ZrO2+ZnO) / Na2O is 0.1 to 0.5.
[0024] (18) The glass-ceramic product according to any one of (1) to (17), wherein the components are expressed in weight percentage, wherein: (P2O5+Na2O) / Li2O is 0.5 to 8.0, preferably (P2O5+Na2O) / Li2O is 0.8 to 5.0, more preferably (P2O5+Na2O) / Li2O is 1.0 to 3.0, and further preferably (P2O5+Na2O) / Li2O is 1.5 to 2.5.
[0025] (19) The microcrystalline glass product according to any one of (1) to (18), wherein the components are expressed in weight percentage, wherein: K2O / ZrO2 is greater than 0.1, preferably K2O / ZrO2 is 0.2 to 10.0, more preferably K2O / ZrO2 is 0.3 to 5.0, and further preferably K2O / ZrO2 is 0.4 to 1.5.
[0026] (20) The microcrystalline glass product according to any one of (1) to (19), wherein the components are expressed in weight percentage, wherein: (ZnO+RO+B2O3+TiO2) / P2O5 is less than 1.5, preferably (ZnO+RO+B2O3+TiO2) / P2O5 is less than 1.0, more preferably (ZnO+RO+B2O3+TiO2) / P2O5 is less than 0.5, and further preferably (ZnO+RO+B2O3+TiO2) / P2O5 is less than 0.2, wherein RO is one or more of MgO, CaO, SrO, and BaO.
[0027] (21) The glass-ceramic product according to any one of (1) to (20), wherein the components are expressed in weight percentage, wherein: SiO2: 43-55%, preferably SiO2: 46-53%; and / or Al2O3: 23-36%, preferably Al2O3: 25.5-32%; and / or Li2O: 3-13%, preferably Li2O: 5.5-11%; and / or Na2O: 5-15%, preferably Na2O: 6.5-12%; and / or P2O5+ZrO2: 2-12%, preferably P2O5+ZrO2: 4-10%; and / or K2O: 0-5%, preferably K2O : 0.1-3%; and / or ZnO: 0-3%, preferably ZnO: 0-1%; and / or B2O3: 0-3%, preferably B2O3: 0-1%; and / or RO: 0-5%, preferably RO: 0-2%; and / or TiO2: 0-3%, preferably TiO2: 0-1%; and / or Ln2O3: 0-3%, preferably Ln2O3: 0-1%; and / or clarifier: 0-1%, preferably clarifier: 0-0.5%, wherein RO is one or more of MgO, CaO, SrO and BaO, and Ln2O3 is one or more of La2O3, Gd2O3 and Y2O3.
[0028] (22) The microcrystalline glass product according to any one of (1) to (21), wherein the components are expressed in weight percentage, wherein: ZrO2: 0 to 6%, preferably ZrO2: 0 to 5%, more preferably ZrO2: 0.1 to 3%; and / or P2O5: 0 to 10%, preferably P2O5: 1 to 8%, more preferably P2O5: 2 to 6%.
[0029] (23) The microcrystalline glass product according to any one of (1), (2), (4) to (12), wherein its components, expressed in weight percentage, further contain: Yb2O3+Nb2O5+WO3+Bi2O3+Ta2O5+TeO2+GeO2: 0 to 5%, preferably Yb2O3+Nb2O5+WO3+Bi2O3+Ta2O5+TeO2+GeO2: 0 to 2%, more preferably Yb2O3+Nb2O5+WO3+Bi2O3+Ta2O5+TeO2+GeO2: 0 to 1%.
[0030] (24) The microcrystalline glass product according to any one of (1) to (23), wherein its components do not contain SrO; and / or do not contain BaO; and / or do not contain MgO; and / or do not contain CaO; and / or do not contain ZnO; and / or do not contain PbO; and / or do not contain As2O3; and / or do not contain TiO2; and / or do not contain B2O3; and / or do not contain Y2O3; and / or do not contain La2O3; and / or do not contain Gd2O3.
[0031] (25) According to any one of (1) to (24), the microcrystalline glass product contains a nepheline crystal phase; and / or a lithium silicate crystal phase; and / or a lithium phosphate crystal phase; and / or a petalite crystal phase; and / or a quartz crystal phase.
[0032] (26) According to any one of (1) to (25), the main crystal phase of the microcrystalline glass product is the nepheline crystal phase, or the microcrystalline glass product only contains the nepheline crystal phase.
[0033] (27) According to any one of the microcrystalline glass products described in (1) to (26), in the microcrystalline glass product, the weight percentage of the nepheline crystal phase in the microcrystalline glass product is 10 to 80%, preferably the weight percentage of the nepheline crystal phase in the microcrystalline glass product is 20 to 70%, and more preferably the weight percentage of the nepheline crystal phase in the microcrystalline glass product is 30 to 60%.
[0034] (28) The microcrystalline glass product according to any one of (1) to (27), wherein the ion exchange layer depth of the microcrystalline glass product is greater than 50 μm, preferably greater than 60 μm, more preferably greater than 80 μm, and further preferably greater than 100 μm; and / or the Vickers hardness is 750 kgf / mm 2 Above, preferably 780kgf / mm 2 More preferably 800kgf / mm 2 More preferably, 810 kgf / mm 2 and / or a grain size of 80 nm or less, preferably 60 nm or less, more preferably 50 nm or less, and further preferably 40 nm or less; and / or a surface stress of 150 MPa or more, preferably 170 MPa or more, and more preferably 190 MPa or more.
[0035] (29) According to any one of the microcrystalline glass products described in (1) to (28), the microcrystalline glass product with a thickness of less than 1 mm has a four-point bending strength of 700 MPa or more, preferably 750 MPa or more, and more preferably 800 MPa or more; and / or the drop ball test height is 1100 mm or more, preferably 1300 mm or more, and more preferably 1500 mm or more; and / or the haze is 0.15% or less, preferably 0.12% or less, and more preferably 0.10% or less; and / or the light transmittance at a wavelength of 550 nm is 88% or more, preferably 89% or more, more preferably 90% or more, and further preferably 91% or more; and / or the average optical |B| value at 400 to 800 nm is 1.5 or less, preferably 1.0 or less, and more preferably 0.8 or less.
[0036] (30) According to any one of (7) to (9) and (29), the thickness of the microcrystalline glass product is 0.2 to 1 mm, preferably 0.3 to 0.9 mm, more preferably 0.5 to 0.8 mm, and further preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.7 mm or 0.75 mm.
[0037] (31) The microcrystalline glass product according to any one of (1), (2), (4) to (12), wherein its components, expressed in weight percentage, further contain: NiO: 0 to 4%; and / or Ni2O3: 0 to 4%; and / or CoO: 0 to 2%; and / or Co2O3: 0 to 2%; and / or Fe2O3: 0 to 7%; and / or MnO2: 0 to 4%; and / or Er2O3: 0 to 8%; and / or Nd2O3: 0 to 8%; and / or Cu2O: 0 to 4%; and / or Pr2O3: 0 to 8%; and / or CeO2: 0 to 4%.
[0038] (32) Glass-ceramics, whose components, expressed in percentage by weight, include: SiO2: 40-60%; Al2O3: 20-40%; Li2O: 2-15%; Na2O: 3-20%; P2O5+ZrO2: 1-15%.
[0039] (33) The microcrystalline glass according to (32), whose components, expressed in weight percentage, also contain: K2O: 0-8%; and / or ZnO: 0-6%; and / or B2O3: 0-6%; and / or RO: 0-8%; and / or TiO2: 0-5%; and / or Ln2O3: 0-5%; and / or clarifier: 0-2%, wherein RO is one or more of MgO, CaO, SrO, and BaO, and Ln2O3 is one or more of La2O3, Gd2O3, and Y2O3.
[0040] (34) Glass-ceramics, whose components, expressed in percentage by weight, are SiO2: 40-60%; Al2O3: 20-40%; Li2O: 2-15%; Na2O: 3-20%; P2O5+ZrO2: 1-15%; K2O: 0-8%; ZnO: 0-6%; B2O3: 0-6%; RO: 0-8%; TiO2: 0-5%; Ln2O3: 0-5%; and clarifier: 0-2%, wherein RO is one or more of MgO, CaO, SrO, and BaO, and Ln2O3 is one or more of La2O3, Gd2O3, and Y2O3.
[0041] (35) Glass-ceramics, comprising SiO2, Al2O3, Li2O and Na2O, the glass-ceramics containing a nepheline crystal phase, and the Vickers hardness of the glass-ceramics being 650 kgf / mm 2 above.
[0042] (36) Glass-ceramics, whose main crystal phase contains nepheline crystal phase, and the Vickers hardness of the glass-ceramics is 650 kgf / mm 2 above.
[0043] (37) Glass-ceramics, whose components, expressed in weight percentage, include SiO2: 40-60%; Al2O3: 20-40%; Li2O: 2-15%; Na2O: 3-20%, and the glass-ceramics contains nepheline crystal phase.
[0044] (38) Glass-ceramics, the components of which include SiO2, Al2O3, Li2O and Na2O, and the ball drop height of the main body of the glass-ceramics with a thickness of less than 1 mm is more than 1000 mm.
[0045] (39) Glass-ceramics, comprising SiO2, Al2O3, Li2O and Na2O, wherein the haze of the glass-ceramics having a thickness of less than 1 mm is less than 0.15%.
[0046] (40) Microcrystalline glass containing nepheline crystal phase, wherein the light transmittance of microcrystalline glass with a thickness of less than 1 mm at a wavelength of 550 nm is greater than 88%.
[0047] (41) Glass-ceramics, the components of which include SiO2, Al2O3, Li2O and Na2O, wherein the weight percentage of the nepheline crystal phase in the glass-ceramics is 10 to 80%.
[0048] (42) The glass-ceramics according to any one of (35) to (41), wherein its components, expressed in weight percentage, contain: SiO2: 40 to 60%; and / or Al2O3: 20 to 40%; and / or Li2O: 2 to 15%; and / or Na2O: 3 to 20%; and / or P2O5+ZrO2: 1 to 15%.
[0049] (43) The glass-ceramics according to any one of (35) to (42), wherein its components, expressed in weight percentage, further contain: K2O: 0 to 8%; and / or ZnO: 0 to 6%; and / or B2O3: 0 to 6%; and / or RO: 0 to 8%; and / or TiO2: 0 to 5%; and / or Ln2O3: 0 to 5%; and / or clarifier: 0 to 2%, wherein RO is one or more of MgO, CaO, SrO, and BaO, and Ln2O3 is one or more of La2O3, Gd2O3, and Y2O3.
[0050] (44) The glass-ceramics according to any one of (32) to (43), wherein the components are expressed in weight percentage, wherein: (Al2O3+Na2O) / P2O5 is 3.0 to 30.0, preferably (Al2O3+Na2O) / P2O5 is 4.0 to 20.0, more preferably (Al2O3+Na2O) / P2O5 is 5.0 to 15.0, and further preferably (Al2O3+Na2O) / P2O5 is 6.0 to 10.0.
[0051] (45) The glass-ceramics according to any one of (32) to (44), wherein the components are expressed in weight percentage, wherein: SiO2 / Al2O3 is 1.2 to 2.8, preferably SiO2 / Al2O3 is 1.3 to 2.5, more preferably SiO2 / Al2O3 is 1.5 to 2.2, and further preferably SiO2 / Al2O3 is 1.6 to 2.0.
[0052] (46) The glass-ceramics according to any one of (32) to (45), wherein the components are expressed in weight percentage, wherein: SiO2 / (Na2O+B2O3) is 2.0 to 15.0, preferably SiO2 / (Na2O+B2O3) is 3.0 to 10.0, more preferably SiO2 / (Na2O+B2O3) is 4.0 to 8.0, and further preferably SiO2 / (Na2O+B2O3) is 5.0 to 7.0.
[0053] (47) The glass-ceramics according to any one of (32) to (46), wherein the components are expressed in weight percentage, wherein: (Na2O+Li2O) / SiO2 is 0.1 to 0.8, preferably (Na2O+Li2O) / SiO2 is 0.15 to 0.7, more preferably (Na2O+Li2O) / SiO2 is 0.2 to 0.6, and further preferably (Na2O+Li2O) / SiO2 is 0.25 to 0.5.
[0054] (48) The glass-ceramics according to any one of (32) to (47), wherein the components are expressed in weight percentage, wherein: (ZrO2+ZnO) / Na2O is less than 2.0, preferably (ZrO2+ZnO) / Na2O is less than 1.5, more preferably (ZrO2+ZnO) / Na2O is 0.01 to 1.0, and further preferably (ZrO2+ZnO) / Na2O is 0.1 to 0.5.
[0055] (49) The glass-ceramics according to any one of (32) to (48), wherein the components are expressed in weight percentage, wherein: (P2O5+Na2O) / Li2O is 0.5 to 8.0, preferably (P2O5+Na2O) / Li2O is 0.8 to 5.0, more preferably (P2O5+Na2O) / Li2O is 1.0 to 3.0, and further preferably (P2O5+Na2O) / Li2O is 1.5 to 2.5.
[0056] (50) The microcrystalline glass according to any one of (32) to (49), wherein the components are expressed in weight percentage, wherein: K2O / ZrO2 is greater than 0.1, preferably K2O / ZrO2 is 0.2 to 10.0, more preferably K2O / ZrO2 is 0.3 to 5.0, and further preferably K2O / ZrO2 is 0.4 to 1.5.
[0057] (51) The glass-ceramics according to any one of (32) to (50), wherein the components are expressed in weight percentage, wherein: (ZnO+RO+B2O3+TiO2) / P2O5 is less than 1.5, preferably (ZnO+RO+B2O3+TiO2) / P2O5 is less than 1.0, more preferably (ZnO+RO+B2O3+TiO2) / P2O5 is less than 0.5, and further preferably (ZnO+RO+B2O3+TiO2) / P2O5 is less than 0.2, wherein RO is one or more of MgO, CaO, SrO, and BaO.
[0058] (52) The glass-ceramics according to any one of (32) to (51), wherein the components are expressed in weight percentage, wherein: SiO2: 43-55%, preferably SiO2: 46-53%; and / or Al2O3: 23-36%, preferably Al2O3: 25.5-32%; and / or Li2O: 3-13%, preferably Li2O: 5.5-11%; and / or Na2O: 5-15%, preferably Na2O: 6.5-12%; and / or P2O5+ZrO2: 2-12%, preferably P2O5+ZrO2: 4-10%; and / or K2O: 0-5%, preferably K2O : 0.1-3%; and / or ZnO: 0-3%, preferably ZnO: 0-1%; and / or B2O3: 0-3%, preferably B2O3: 0-1%; and / or RO: 0-5%, preferably RO: 0-2%; and / or TiO2: 0-3%, preferably TiO2: 0-1%; and / or Ln2O3: 0-3%, preferably Ln2O3: 0-1%; and / or clarifier: 0-1%, preferably clarifier: 0-0.5%, wherein RO is one or more of MgO, CaO, SrO and BaO, and Ln2O3 is one or more of La2O3, Gd2O3 and Y2O3.
[0059] (53) The glass-ceramics according to any one of (32) to (52), wherein the components are expressed in weight percentage, wherein: ZrO2: 0 to 6%, preferably ZrO2: 0 to 5%, more preferably ZrO2: 0.1 to 3%; and / or P2O5: 0 to 10%, preferably P2O5: 1 to 8%, more preferably P2O5: 2 to 6%.
[0060] (54) The glass-ceramics according to any one of (32), (33), (35) to (43), wherein its components, expressed in weight percentage, further contain: Yb2O3+Nb2O5+WO3+Bi2O3+Ta2O5+TeO2+GeO2: 0 to 5%, preferably Yb2O3+Nb2O5+WO3+Bi2O3+Ta2O5+TeO2+GeO2: 0 to 2%, more preferably Yb2O3+Nb2O5+WO3+Bi2O3+Ta2O5+TeO2+GeO2: 0 to 1%.
[0061] (55) The microcrystalline glass according to any one of (32) to (54), wherein its components do not contain SrO; and / or do not contain BaO; and / or do not contain MgO; and / or do not contain CaO; and / or do not contain ZnO; and / or do not contain PbO; and / or do not contain As2O3; and / or do not contain TiO2; and / or do not contain B2O3; and / or do not contain Y2O3; and / or do not contain La2O3; and / or do not contain Gd2O3.
[0062] (56) According to any one of the microcrystalline glass described in (32) to (55), the microcrystalline glass contains a nepheline crystal phase; and / or a lithium silicate crystal phase; and / or a lithium phosphate crystal phase; and / or a petalite crystal phase; and / or a quartz crystal phase.
[0063] (57) According to any one of the microcrystalline glass described in (32) to (56), the main crystal phase of the microcrystalline glass is the nepheline crystal phase, or the microcrystalline glass only contains the nepheline crystal phase.
[0064] (58) According to any one of the microcrystalline glass described in (32) to (57), in the microcrystalline glass, the weight percentage of the nepheline crystal phase in the microcrystalline glass is 10 to 80%, preferably the weight percentage of the nepheline crystal phase in the microcrystalline glass is 20 to 70%, and more preferably the weight percentage of the nepheline crystal phase in the microcrystalline glass is 30 to 60%.
[0065] (59) The microcrystalline glass according to any one of (32) to (58), wherein the grain size of the microcrystalline glass is less than 80 nm, preferably less than 60 nm, more preferably less than 50 nm, and further preferably less than 40 nm; and / or the Vickers hardness is 650 kgf / mm 2 Above, preferably 680kgf / mm 2 More preferably 700kgf / mm2 above.
[0066] (60) The microcrystalline glass according to any one of (32) to (59), for a microcrystalline glass with a thickness of less than 1 mm, has a body ball drop height of more than 1000 mm, preferably more than 1200 mm, and more preferably more than 1400 mm; and / or a haze of less than 0.15%, preferably less than 0.12%, and more preferably less than 0.10%; and / or a light transmittance of 550 nm wavelength is more than 88%, preferably more than 89%, more preferably more than 90%, and further preferably more than 91%; and / or an average optical |B| value of 400 to 800 nm is less than 1.5, preferably less than 1.0, and more preferably less than 0.8.
[0067] (61) According to any one of (38) to (40) and (60), the thickness of the microcrystalline glass is 0.2 to 1 mm, preferably 0.3 to 0.9 mm, more preferably 0.5 to 0.8 mm, and further preferably 0.55 mm or 0.6 mm or 0.68 mm or 0.7 mm or 0.75 mm.
[0068] (62) The glass-ceramics according to any one of (32), (33), (35) to (43), wherein its components, expressed in weight percentage, further contain: NiO: 0 to 4%; and / or Ni2O3: 0 to 4%; and / or CoO: 0 to 2%; and / or Co2O3: 0 to 2%; and / or Fe2O3: 0 to 7%; and / or MnO2: 0 to 4%; and / or Er2O3: 0 to 8%; and / or Nd2O3: 0 to 8%; and / or Cu2O: 0 to 4%; and / or Pr2O3: 0 to 8%; and / or CeO2: 0 to 4%.
[0069] (63) Matrix glass, whose components, expressed in weight percentage, include: SiO2: 40-60%; Al2O3: 20-40%; Li2O: 2-15%; Na2O: 3-20%; P2O5+ZrO2: 1-15%.
[0070] (64) The matrix glass according to (63), whose components, expressed in weight percentage, also contain: K2O: 0-8%; and / or ZnO: 0-6%; and / or B2O3: 0-6%; and / or RO: 0-8%; and / or TiO2: 0-5%; and / or Ln2O3: 0-5%; and / or clarifier: 0-2%, wherein RO is one or more of MgO, CaO, SrO, and BaO, and Ln2O3 is one or more of La2O3, Gd2O3, and Y2O3.
[0071] (65) Matrix glass, whose components, expressed in weight percentage, are composed of SiO2: 40-60%; Al2O3: 20-40%; Li2O: 2-15%; Na2O: 3-20%; P2O5+ZrO2: 1-15%; K2O: 0-8%; ZnO: 0-6%; B2O3: 0-6%; RO: 0-8%; TiO2: 0-5%; Ln2O3: 0-5%; and clarifier: 0-2%, wherein RO is one or more of MgO, CaO, SrO, and BaO, and Ln2O3 is one or more of La2O3, Gd2O3, and Y2O3.
[0072] (66) The matrix glass according to any one of (63) to (65), wherein the components are expressed in weight percentage, wherein: (Al2O3+Na2O) / P2O5 is 3.0 to 30.0, preferably (Al2O3+Na2O) / P2O5 is 4.0 to 20.0, more preferably (Al2O3+Na2O) / P2O5 is 5.0 to 15.0, and further preferably (Al2O3+Na2O) / P2O5 is 6.0 to 10.0.
[0073] (67) The matrix glass according to any one of (63) to (66), wherein the components are expressed in weight percentage, wherein: SiO2 / Al2O3 is 1.2 to 2.8, preferably SiO2 / Al2O3 is 1.3 to 2.5, more preferably SiO2 / Al2O3 is 1.5 to 2.2, and further preferably SiO2 / Al2O3 is 1.6 to 2.0.
[0074] (68) The matrix glass according to any one of (63) to (67), wherein the components are expressed in weight percentage, wherein: SiO2 / (Na2O+B2O3) is 2.0 to 15.0, preferably SiO2 / (Na2O+B2O3) is 3.0 to 10.0, more preferably SiO2 / (Na2O+B2O3) is 4.0 to 8.0, and further preferably SiO2 / (Na2O+B2O3) is 5.0 to 7.0.
[0075] (69) The matrix glass according to any one of (63) to (68), wherein the components are expressed in weight percentage, wherein: (Na2O+Li2O) / SiO2 is 0.1 to 0.8, preferably (Na2O+Li2O) / SiO2 is 0.15 to 0.7, more preferably (Na2O+Li2O) / SiO2 is 0.2 to 0.6, and further preferably (Na2O+Li2O) / SiO2 is 0.25 to 0.5.
[0076] (70) According to any one of the matrix glass described in (63) to (69), its components are expressed in weight percentage, wherein: (ZrO2+ZnO) / Na2O is less than 2.0, preferably (ZrO2+ZnO) / Na2O is less than 1.5, more preferably (ZrO2+ZnO) / Na2O is 0.01 to 1.0, and further preferably (ZrO2+ZnO) / Na2O is 0.1 to 0.5.
[0077] (71) According to any one of the matrix glass described in (63) to (70), its components are expressed in weight percentage, wherein: (P2O5+Na2O) / Li2O is 0.5 to 8.0, preferably (P2O5+Na2O) / Li2O is 0.8 to 5.0, more preferably (P2O5+Na2O) / Li2O is 1.0 to 3.0, and further preferably (P2O5+Na2O) / Li2O is 1.5 to 2.5.
[0078] (72) According to any one of the matrix glass described in (63) to (71), its components are expressed in weight percentage, wherein: K2O / ZrO2 is greater than 0.1, preferably K2O / ZrO2 is 0.2 to 10.0, more preferably K2O / ZrO2 is 0.3 to 5.0, and further preferably K2O / ZrO2 is 0.4 to 1.5.
[0079] (73) The matrix glass according to any one of (63) to (72), wherein the components are expressed in weight percentage, wherein: (ZnO+RO+B2O3+TiO2) / P2O5 is less than 1.5, preferably (ZnO+RO+B2O3+TiO2) / P2O5 is less than 1.0, more preferably (ZnO+RO+B2O3+TiO2) / P2O5 is less than 0.5, and further preferably (ZnO+RO+B2O3+TiO2) / P2O5 is less than 0.2, wherein RO is one or more of MgO, CaO, SrO, and BaO.
[0080] (74) The matrix glass according to any one of (63) to (73), wherein the components are expressed in weight percentage, wherein: SiO2: 43-55%, preferably SiO2: 46-53%; and / or Al2O3: 23-36%, preferably Al2O3: 25.5-32%; and / or Li2O: 3-13%, preferably Li2O: 5.5-11%; and / or Na2O: 5-15%, preferably Na2O: 6.5-12%; and / or P2O5+ZrO2: 2-12%, preferably P2O5+ZrO2: 4-10%; and / or K2O: 0-5%, preferably K2O : 0.1-3%; and / or ZnO: 0-3%, preferably ZnO: 0-1%; and / or B2O3: 0-3%, preferably B2O3: 0-1%; and / or RO: 0-5%, preferably RO: 0-2%; and / or TiO2: 0-3%, preferably TiO2: 0-1%; and / or Ln2O3: 0-3%, preferably Ln2O3: 0-1%; and / or clarifier: 0-1%, preferably clarifier: 0-0.5%, wherein RO is one or more of MgO, CaO, SrO and BaO, and Ln2O3 is one or more of La2O3, Gd2O3 and Y2O3.
[0081] (75) According to any one of the matrix glass described in (63) to (74), its components are expressed in weight percentage, wherein: ZrO2: 0 to 6%, preferably ZrO2: 0 to 5%, more preferably ZrO2: 0.1 to 3%; and / or P2O5: 0 to 10%, preferably P2O5: 1 to 8%, more preferably P2O5: 2 to 6%.
[0082] (76) The matrix glass according to (63) or (64), whose components, expressed in weight percentage, also contain: Yb2O3+Nb2O5+WO3+Bi2O3+Ta2O5+TeO2+GeO2: 0~5%, preferably Yb2O3+Nb2O5+WO3+Bi2O3+Ta2O5+TeO2+GeO2: 0~2%, more preferably Yb2O3+Nb2O5+WO3+Bi2O3+Ta2O5+TeO2+GeO2: 0~1%.
[0083] (77) The matrix glass according to any one of (63) to (65), wherein its components do not contain SrO; and / or do not contain BaO; and / or do not contain MgO; and / or do not contain CaO; and / or do not contain ZnO; and / or do not contain PbO; and / or do not contain As2O3; and / or do not contain TiO2; and / or do not contain B2O3; and / or do not contain Y2O3; and / or do not contain La2O3; and / or do not contain Gd2O3.
[0084] (78) The matrix glass according to (63) or (64), whose components, expressed in weight percentage, also contain: NiO: 0-4%; and / or Ni2O3: 0-4%; and / or CoO: 0-2%; and / or Co2O3: 0-2%; and / or Fe2O3: 0-7%; and / or MnO2: 0-4%; and / or Er2O3: 0-8%; and / or Nd2O3: 0-8%; and / or Cu2O: 0-4%; and / or Pr2O3: 0-8%; and / or CeO2: 0-4%.
[0085] (79) A microcrystalline glass molded body comprising the microcrystalline glass described in any one of (32) to (62).
[0086] (80) A glass cover plate comprising the microcrystalline glass product described in any one of (1) to (31), and / or the microcrystalline glass described in any one of (32) to (62), and / or the matrix glass described in any one of (63) to (78), and / or the microcrystalline glass formed body described in (79).
[0087] (81) A glass component comprising a microcrystalline glass product as described in any one of (1) to (31), and / or a microcrystalline glass as described in any one of (32) to (62), and / or a matrix glass as described in any one of (63) to (78), and / or a microcrystalline glass formed body as described in (79).
[0088] (82) A display device comprising the microcrystalline glass product described in any one of (1) to (31), and / or the microcrystalline glass described in any one of (32) to (62), and / or the matrix glass described in any one of (63) to (78), and / or the microcrystalline glass formed body described in (79), and / or the glass cover plate described in (80), and / or the glass component described in (81).
[0089] (83) An electronic device comprising the microcrystalline glass product described in any one of (1) to (31), and / or the microcrystalline glass described in any one of (32) to (62), and / or the matrix glass described in any one of (63) to (78), and / or the microcrystalline glass formed body described in (79), and / or the glass cover described in (80), and / or the glass component described in (81).
[0090] (84) According to any one of the methods for manufacturing microcrystalline glass products described in (1) to (31), the method comprises the following steps: forming a matrix glass, subjecting the matrix glass to a crystallization process to form a microcrystalline glass, and then subjecting the microcrystalline glass to a chemical strengthening process to form a microcrystalline glass product.
[0091] (85) According to the method for manufacturing microcrystalline glass products described in (84), the crystallization process includes the following steps: heating to a specified crystallization treatment temperature, maintaining the temperature for a certain period of time after reaching the crystallization treatment temperature, and then cooling down, the crystallization treatment temperature is 580-750°C, preferably 600-700°C, and the holding time at the crystallization treatment temperature is 0-8 hours, preferably 1-6 hours.
[0092] (86) According to the method for manufacturing a microcrystalline glass product described in (84), the crystallization process includes the following steps: performing a nucleation process at a first temperature, and then performing a crystal growth process at a second temperature higher than the nucleation process temperature.
[0093] (87) According to the method for manufacturing microcrystalline glass products described in (86), the crystallization process includes the following steps: the first temperature is 500-620°C, and the second temperature is 620-750°C; the holding time at the first temperature is 0-24 hours, preferably 2-15 hours; the holding time at the second temperature is 0-10 hours, preferably 0.5-6 hours.
[0094] (88) According to the method for manufacturing a microcrystalline glass product according to any one of (84) to (87), the chemical strengthening process includes: the microcrystalline glass is immersed in a salt bath of molten Na salt at a temperature of 350 to 470°C for 1 to 36 hours, preferably in the temperature range of 380 to 460°C, and the preferred time range is 2 to 10 hours; and / or the microcrystalline glass is immersed in a salt bath of molten K salt at a temperature of 360 to 450°C for 1 to 36 hours, preferably in the time range of 1 to 10 hours; and / or the microcrystalline glass is immersed in a mixed salt bath of molten K salt and Na salt at a temperature of 360 to 450°C for 1 to 36 hours, preferably in the time range of 2 to 24 hours.
[0095] (89) A method for manufacturing glass-ceramics according to any one of (32) to (62), comprising the steps of forming a matrix glass and then subjecting the matrix glass to a crystallization process to form glass-ceramics.
[0096] (90) According to the method for manufacturing microcrystalline glass described in (89), the crystallization process includes the following steps: heating to a specified crystallization treatment temperature, maintaining the temperature for a certain period of time after reaching the crystallization treatment temperature, and then cooling down, the crystallization treatment temperature is 580 to 750°C, preferably 600 to 700°C, and the holding time at the crystallization treatment temperature is 0 to 8 hours, preferably 1 to 6 hours.
[0097] (91) According to the method for manufacturing microcrystalline glass described in (89), the crystallization process includes the following steps: performing a nucleation process at a first temperature, and then performing a crystal growth process at a second temperature higher than the nucleation process temperature.
[0098] (92) According to the method for manufacturing microcrystalline glass described in (91), the crystallization process includes the following steps: the first temperature is 500-620°C, and the second temperature is 620-750°C; the holding time at the first temperature is 0-24 hours, preferably 2-15 hours; the holding time at the second temperature is 0-10 hours, preferably 0.5-6 hours.
[0099] (93) A method for manufacturing a microcrystalline glass molded body according to (79), the method comprising grinding or polishing the microcrystalline glass to form a microcrystalline glass molded body, or subjecting matrix glass or microcrystalline glass to a heat bending process or a press molding process at a certain temperature to form a microcrystalline glass molded body.
[0100] (94) According to the method for manufacturing a microcrystalline glass molded body described in (79), the method includes the following steps: subjecting the matrix glass to a crystallization heat treatment process, including heating, heat preservation for nucleation, heating, heat preservation for crystallization, and cooling to room temperature to form a pre-crystallized glass; and subjecting the pre-crystallized glass to heat processing and molding to obtain a microcrystalline glass molded body.
[0101] (95) The method for producing a glass-ceramic formed body according to (79), the method comprising the following steps:
[0102] 1) Heating and preheating: Place the matrix glass or pre-crystallized glass or microcrystalline glass in the mold. The mold passes through each heating station in the hot bending machine in turn and stays at each station for a certain period of time to keep warm. The temperature in the preheating zone is 400-800°C, the pressure is 0.01-0.05MPa, and the time is 40-200s;
[0103] 2) Pressurized molding: After preheating, the mold is transferred to the molding station. The hot bending machine applies a certain pressure to the mold. The pressure range is 0.1-0.8Mpa. The molding station temperature range is 650-850℃, and the molding time range is 40-200s.
[0104] 3) Maintaining pressure and cooling: The mold is transferred to the cooling station for cooling step by step. The cooling temperature range is 750-500°C, the pressure is 0.01-0.05Mpa, and the time is 40-200s.
[0105] The beneficial effect of the present invention is that through reasonable component design, the microcrystalline glass or microcrystalline glass products obtained by the present invention have excellent mechanical properties and meet the application requirements in the fields of display devices or electronic devices. DETAILED DESCRIPTION
[0106] The glass-ceramics and glass-ceramics products of the present invention are materials having a crystalline phase (sometimes also referred to as crystal) and a glass phase, which are different from amorphous solids. The crystalline phase of the glass-ceramics and glass-ceramics products can be identified by the peak angles appearing in the X-ray diffraction pattern of X-ray diffraction analysis and / or measured by TEMEDX.
[0107] After repeated experiments and studies, the inventors of the present invention obtained the microcrystalline glass or microcrystalline glass products of the present invention by regulating the content and content ratio of specific components constituting microcrystalline glass and microcrystalline glass products to specific values and precipitating specific crystalline phases.
[0108] Next, the scope of each component (ingredient) of the matrix glass, microcrystalline glass and microcrystalline glass products of the present invention is described. In this specification, unless otherwise specified, the content of each component is expressed in weight percentage (wt%) relative to the total amount of matrix glass, microcrystalline glass or microcrystalline glass product material converted into oxide composition. Here, the "composition converted into oxide" means that when oxides, composite salts and hydroxides used as raw materials for the matrix glass, microcrystalline glass or microcrystalline glass product components of the present invention decompose and transform into oxides when melted, the total weight of the oxide material is taken as 100%. In addition, in this specification, when it is only referred to as glass, it is the matrix glass before crystallization (i.e., crystallization process treatment), the matrix glass after crystallization (i.e., crystallization process treatment) is called microcrystalline glass, and microcrystalline glass products refer to products obtained after chemical strengthening of microcrystalline glass.
[0109] Unless otherwise indicated in specific cases, the numerical ranges listed herein include upper and lower limits, and "above" and "below" include the endpoints, as well as all integers and fractions within the range, without limitation to the specific values listed when defining the range. The term "about" as used herein means that the formula, parameters and other quantities and features are not and need not be exact, and may be approximate and / or larger or lower if necessary, reflecting tolerances, conversion factors and measurement errors, etc. "And / or" as used herein is inclusive, for example, "A; and / or B" means only A, or only B, or both A and B.
[0110] In some embodiments, the crystal phase of the glass-ceramic or glass-ceramic product of the present invention contains a nepheline crystal phase (including eucryptite and / or sodium nepheline), specifically, contains eucryptite, or contains sodium nepheline, or contains eucryptite and sodium nepheline at the same time. The glass-ceramic of the present invention may also contain other crystal phases besides the nepheline crystal phase, such as a lithium silicate crystal phase (one or both of lithium monosilicate and lithium disilicate); and / or a lithium phosphate crystal phase; and / or a petalite crystal phase; and / or a quartz crystal phase.
[0111] In some embodiments of the present invention, the crystal phase in the glass-ceramic or glass-ceramic products contains only nepheline crystal phase (one or both of eucryptite and sodium nepheline).
[0112] In some embodiments, when the microcrystalline glass or microcrystalline glass products contain nepheline crystal phase and other crystal phases, the main crystal phase of the microcrystalline glass or microcrystalline glass products is the nepheline crystal phase, that is, the nepheline crystal phase has a higher weight percentage than other crystal phases.
[0113] In some embodiments, the weight percentage of the nepheline crystal phase in the glass-ceramic or glass-ceramic product is 10-80%, preferably the weight percentage of the nepheline crystal phase in the glass-ceramic or glass-ceramic product is 20-70%, and more preferably the weight percentage of the nepheline crystal phase in the glass-ceramic or glass-ceramic product is 30-60%. In some embodiments, the weight percentage of the nepheline crystal phase in the glass-ceramic or glass-ceramic product is about 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99%, 100%, 101%, 10 1%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80%.
[0114] SiO2 is the basic component of the matrix glass, glass-ceramics and glass-ceramics of the present invention, which can be used to stabilize the network structure of glass and glass-ceramics. It is one of the components that form the nepheline crystal phase after crystallization. If the content of SiO2 is below 40%, the crystals formed in the glass-ceramics will become less and the crystals are easy to become coarse, affecting the haze of the glass-ceramics and glass-ceramics, as well as the performances such as the drop ball test height of the glass-ceramics. Therefore, the lower limit of the SiO2 content is 40%, preferably 43%, and more preferably 46%. If the content of SiO2 exceeds 60%, the glass melting temperature is high, clarification is difficult, and it is not easy to form, which affects the consistency of the glass, and affects the hot bending of glass and glass-ceramics, and is unfavorable to the surface stress and ion exchange layer depth of the glass-ceramics. Therefore, the upper limit of the SiO2 content is 60%, preferably 55%, and more preferably 53%. In some embodiments, the SiO2 may include about 40%, 40.5%, 41%, 41.5%, 42%, 42.5%, 43%, 43.5%, 44%, 44.5%, 45%, 45.5%, 46%, 46.5%, 47%, 47.5%, 48%, 48.5%, 49%, 49.5%, 50%, 50.5%, 51%, 51.5%, 52%, 52.5%, 53%, 53.5%, 54%, 54.5%, 55%, 55.5%, 56%, 56.5%, 57%, 57.5%, 58%, 58.5%, 59%, 59.5%, 60%.
[0115] Al2O3 is a component that forms a glass network structure. It is an important component that helps stabilize glass molding and improve chemical stability. It can also improve the mechanical properties of glass and increase the depth of the ion exchange layer and surface stress of microcrystalline glass products. However, if the Al2O3 content is too high, the glass's solubility and resistance to devitrification will decrease, and the crystals will easily increase during crystallization, reducing the strength of microcrystalline glass and microcrystalline glass products. Therefore, the content of Al2O3 in the present invention is 20-40%, preferably 23-36%, and more preferably 25.5-32%. In some embodiments, the Al2O3 may include about 20%, 20.5%, 21%, 21.5%, 22%, 22.5%, 23%, 23.5%, 24%, 24.5%, 25%, 25.5%, 26%, 26.5%, 27%, 27.5%, 28%, 28.5%, 29%, 29.5%, 30%, 30.5%, 31%, 31.5%, 32%, 32.5%, 33%, 33.5%, 34%, 34.5%, 35%, 35.5%, 36%, 36.5%, 37%, 37.5%, 38%, 38.5%, 39%, 39.5%, 40%.
[0116] In some embodiments, the ratio SiO2 / Al2O3 between the content of SiO2 and the content of Al2O3 is controlled within the range of 1.2 to 2.8, which can improve the four-point bending strength of microcrystalline glass and microcrystalline glass products, and improve the light transmittance of microcrystalline glass and microcrystalline glass products. Therefore, SiO2 / Al2O3 is preferably 1.2 to 2.8, and SiO2 / Al2O3 is more preferably 1.3 to 2.5. Furthermore, controlling SiO2 / Al2O3 within the range of 1.5 to 2.2 can further reduce the |B| value of microcrystalline glass and microcrystalline glass products, and increase the surface stress of microcrystalline glass products. Therefore, it is further preferred that SiO2 / Al2O3 is 1.5 to 2.2, and it is further preferred that SiO2 / Al2O3 is 1.6 to 2.0. In some embodiments, the value of SiO2 / Al2O3 may be 1.2, 1.25, 1.3, 1.35, 1.4, 1.45, 1.5, 1.55, 1.6, 1.65, 1.7, 1.75, 1.8, 1.85, 1.9, 1.95, 2.0, 2.05, 2.1, 2.15, 2.2, 2.25, 2.3, 2.35, 2.4, 2.45, 2.5, 2.55, 2.6, 2.65, 2.7, 2.75, 2.8.
[0117] Li2O can promote the melting of glass, reduce the melting temperature of glass, form eucryptite crystal phase after crystallization, and is also the main component replaced with sodium and potassium ions in the chemical strengthening process. It can increase the surface stress of microcrystalline glass products, help to improve the drop ball test height of microcrystalline glass products, and increase the dielectric constant of microcrystalline glass and microcrystalline glass products. On the other hand, if too much Li2O is contained, it is easy to reduce the chemical stability of glass, and deteriorate the light transmittance of microcrystalline glass and microcrystalline glass products. Therefore, the content of Li2O in the present invention is 2 to 15%, preferably 3 to 13%, and more preferably 5.5 to 11%. In some embodiments, about 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, 10%, 10.5%, 11%, 11.5%, 12%, 12.5%, 13%, 13.5%, 14%, 14.5%, 15% Li2O may be included.
[0118] Na2O can participate in crystallization to form sodium nepheline crystal phase after crystallization, can also participate in chemical strengthening, and can improve the solubility of glass. On the other hand, if the content of Na2O is too high, it is easy to cause the crystal grains to increase or the type of crystal phases to change during the crystallization process. Therefore, the content of Na2O in the present invention is 3 to 20%, preferably 5 to 15%, and more preferably 6.5 to 12%. In some embodiments, the Na2O may include about 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, 10%, 10.5%, 11%, 11.5%, 12%, 12.5%, 13%, 13.5%, 14%, 14.5%, 15%, 15.5%, 16%, 16.5%, 17%, 17.5%, 18%, 18.5%, 19%, 19.5%, 20%.
[0119] In some embodiments, the ratio (Na2O+Li2O) / SiO2 between the total content of Na2O and Li2O Na2O+Li2O and the content of SiO2 is controlled within the range of 0.1 to 0.8, which is beneficial for the microcrystalline glass and microcrystalline glass products to obtain the desired crystalline phase content, while refining the grains and improving the hardness of the microcrystalline glass and microcrystalline glass products. Therefore, it is preferred that (Na2O+Li2O) / SiO2 is 0.1 to 0.8, and it is more preferred that (Na2O+Li2O) / SiO2 is 0.15 to 0.7. Further, controlling (Na2O+Li2O) / SiO2 within the range of 0.2 to 0.6 can further improve the light transmittance of the microcrystalline glass and microcrystalline glass products, and optimize the haze. Therefore, it is further preferred that (Na2O+Li2O) / SiO2 is 0.2 to 0.6, and it is further preferred that (Na2O+Li2O) / SiO2 is 0.25 to 0.5. In some embodiments, the value of (Na2O+Li2O) / SiO2 may be 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8.
[0120] K2O is an optional component that helps improve the low temperature melting property and formability of the glass, but if too much K2O is contained, it is easy to reduce the chemical stability of the glass. Therefore, the content of K2O is 0-8%, preferably 0-5%, and more preferably 0.1-3%. In some embodiments, about 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8% K2O may be included.
[0121] P2O5 can form crystal nuclei in glass, promote uniform crystal growth, and help improve the low-temperature melting property of glass; however, if P2O5 is contained too much, it is easy to reduce the resistance to devitrification and glass phase separation, and the mechanical properties of microcrystalline glass and microcrystalline glass products tend to deteriorate. Therefore, the content of P2O5 in the present invention is 0-10%, preferably 1-8%, and more preferably 2-6%. In some embodiments, about 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, 10% P2O5 may be included.
[0122] In some embodiments, the ratio (Al2O3+Na2O) / P2O5 between the total content of Al2O3 and Na2O Al2O3+Na2O and the content of P2O5 is controlled within the range of 3.0 to 30.0, which is beneficial for the microcrystalline glass and microcrystalline glass products to obtain the desired crystalline phase content, and to increase the Vickers hardness of the microcrystalline glass and microcrystalline glass products, and to increase the height of the drop ball test. Therefore, it is preferred that (Al2O3+Na2O) / P2O5 is 3.0 to 30.0, and it is more preferred that (Al2O3+Na2O) / P2O5 is 4.0 to 20.0. Furthermore, by controlling (Al2O3+Na2O) / P2O5 within the range of 5.0 to 15.0, the four-point bending strength of the microcrystalline glass and microcrystalline glass products can be further optimized, and the depth of the ion exchange layer of the microcrystalline glass products can be increased. Therefore, it is further preferred that (Al2O3+Na2O) / P2O5 is 5.0-15.0, and it is further preferred that (Al2O3+Na2O) / P2O5 is 6.0-10.0. In some embodiments, the value of (Al2O3+Na2O) / P2O5 may be 3.0, 3.5, 4.0, 4.5, 5.0, 5.5, 6.0, 6.5, 7.0, 7.5, 8.0, 8.5, 9.0, 9.5, 10.0, 10.5, 11.0, 11.5, 12.0, 12.5, 13.0, 13.5, 14.0, 14.5, 15.0, 15.5 , 16.0, 16.5, 17.0, 17.5, 18.0, 18.5, 19.0, 19.5, 20.0, 20.5, 21.0, 21.5, 22.0, 22.5, 23.0, 23.5, 24.0, 24.5, 25.0, 25.5, 26.0, 26.5, 27.0, 27.5, 28.0, 28.5, 29.0, 29.5, 30.0.
[0123] In some embodiments, the ratio (P2O5+Na2O) / Li2O between the total content of P2O5 and Na2O (P2O5+Na2O) and the content of Li2O is controlled within the range of 0.5 to 8.0, which is beneficial to increasing the drop ball test height of glass-ceramics and glass-ceramics products and increasing the depth of the ion exchange layer of glass-ceramics products. Therefore, it is preferred that (P2O5+Na2O) / Li2O is 0.5 to 8.0, and it is more preferred that (P2O5+Na2O) / Li2O is 0.8 to 5.0. Furthermore, controlling (P2O5+Na2O) / Li2O within the range of 1.0 to 3.0 can further optimize the hardness and |B| value of glass-ceramics and glass-ceramics products. Therefore, it is further preferred that (P2O5+Na2O) / Li2O is 1.0 to 3.0, and it is further preferred that (P2O5+Na2O) / Li2O is 1.5 to 2.5. In some embodiments, the value of (PO5+Na2O) / Li2O may be 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4.0, 4.5, 5.0, 5.5, 6.0, 6.5, 7.0, 7.5, 8.0.
[0124] ZrO2 has the function of crystallization and precipitation to form crystal nuclei, and at the same time helps to improve the chemical stability of glass. Studies have found that ZrO2 can also improve the stability of glass by significantly reducing the devitrification of glass and lowering the liquidus temperature during the melting process; but if too much ZrO2 is contained, the devitrification resistance of the glass is easily reduced, and the difficulty of controlling the glass crystallization process increases. Therefore, the content of ZrO2 is 0-6%, preferably 0-5%, and more preferably 0.1-3%. In some embodiments, about 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6% ZrO2 may be included.
[0125] In some embodiments, the ratio K2O / ZrO2 between the content of K2O and the content of ZrO2 is controlled to be above 0.1, which is beneficial to refine the grains and reduce the haze and grain size of microcrystalline glass and microcrystalline glass products. Therefore, it is preferred that K2O / ZrO2 is above 0.1, and it is more preferred that K2O / ZrO2 is 0.2 to 10.0. Furthermore, controlling K2O / ZrO2 within the range of 0.3 to 5.0 can further optimize the light transmittance of microcrystalline glass and microcrystalline glass products and prevent the depth of the ion exchange layer of microcrystalline glass products from deteriorating. Therefore, it is further preferred that K2O / ZrO2 is 0.3 to 5.0, and it is further preferred that K2O / ZrO2 is 0.4 to 1.5. In some embodiments, the value of K2O / ZrO2 may be 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, 0.95, 1.0, 1.05, 1.1, 1.15, 1.2, 1.25, 1.3, 1.35, 1.4, 1.45, 1.5, 1.55, 1.6, 1.65, 1.7, 1.75, 1.8, 1 .85, 1.9, 1.95, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4.0, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9, 5.0, 5.5, 6.0, 6.5, 7.0, 7.5, 8.0, 8.5, 9.0, 9.5, 10.0.
[0126] In some embodiments, the total content of P2O5 and ZrO2 (P2O5+ZrO2) is controlled within the range of 1 to 15%, which is beneficial to grain refinement, reducing the grain size of microcrystalline glass and microcrystalline glass products, while reducing the |B| value of microcrystalline glass and microcrystalline glass products, and improving the light transmittance of microcrystalline glass and microcrystalline glass products. Therefore, preferably P2O5+ZrO2 is 1 to 15%, more preferably P2O5+ZrO2 is 2 to 12%, and further preferably P2O5+ZrO2 is 4 to 10%. In some embodiments, P2O5+ZrO2 may be 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, 10%, 10.5%, 11%, 11.5%, 12%, 12.5%, 13%, 13.5%, 14%, 14.5%, 15%.
[0127] ZnO can improve the melting performance of glass, improve the chemical stability of glass, refine grains during crystallization, control the upper limit of ZnO content below 6%, and inhibit the reduction of devitrification resistance. Therefore, the ZnO content is 0-6%, preferably 0-3%, and more preferably 0-1%. In some embodiments, about 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6% ZnO may be included.
[0128] In some embodiments, the ratio of the total content of ZrO2 and ZnO ZrO2+ZnO to the content of Na2O (ZrO2+ZnO) / Na2O is controlled to be below 2.0, which is beneficial to reduce the haze and grain size of microcrystalline glass and microcrystalline glass products, and increase the drop ball test height of microcrystalline glass and microcrystalline glass products. Therefore, it is preferred that (ZrO2+ZnO) / Na2O is below 2.0, more preferably (ZrO2+ZnO) / Na2O is below 1.5, further preferably (ZrO2+ZnO) / Na2O is 0.01 to 1.0, and further preferably (ZrO2+ZnO) / Na2O is 0.1 to 0.5. In some embodiments, the value of (ZrO2+ZnO) / Na2O can be 0, greater than 0, 0.01, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, 0.95, 1.0, 1.05, 1.1, 1.15, 1.2, 1.25, 1.3, 1.35, 1.4, 1.45, 1.5, 1.55, 1.6, 1.65, 1.7, 1.75, 1.8, 1.85, 1.9, 1.95, 2.0.
[0129] B2O3 can improve the network structure of glass and adjust the chemical strengthening properties of microcrystalline glass. If its content is too much, it is not conducive to glass molding, it is easy to crystallize during molding, and the chemical stability is reduced. Therefore, the content of B2O3 is 0-6%, preferably 0-3%, and more preferably 0-1%. In some embodiments, about 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6% B2O3 may be included.
[0130] In some embodiments, the ratio SiO2 / (Na2O+B2O3) between the content of SiO2 and the total content of Na2O and B2O3 Na2O+B2O3 is controlled within the range of 2.0 to 15.0, which is beneficial to increase the depth of the ion exchange layer of the microcrystalline glass product and improve the four-point bending strength of the microcrystalline glass and microcrystalline glass products. Therefore, it is preferred that SiO2 / (Na2O+B2O3) is 2.0 to 15.0, and it is more preferred that SiO2 / (Na2O+B2O3) is 3.0 to 10.0. Further, controlling SiO2 / (Na2O+B2O3) within the range of 4.0 to 8.0 can further optimize the surface stress of the microcrystalline glass product and increase the drop ball test height of the microcrystalline glass and microcrystalline glass products. Therefore, it is further preferred that SiO2 / (Na2O+B2O3) is 4.0 to 8.0, and it is further preferred that SiO2 / (Na2O+B2O3) is 5.0 to 7.0. In some embodiments, the value of SiO2 / (Na2O+B2O3) may be 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, 5.0, 5.5, 6.0, 6.5, 7.0, 7.5, 8.0, 8.5, 9.0, 9.5, 10.0, 10.5, 11.0, 11.5, 12.0, 12.5, 13.0, 13.5, 14.0, 14.5, 15.0.
[0131] Alkaline earth metal oxides RO (RO is one or more of MgO, CaO, SrO, and BaO) help to improve the devitrification resistance of glass and enhance the strength of glass; but when its content is high, the crystallization performance of glass is reduced, which is not conducive to obtaining the desired crystal phase type and grain size of microcrystalline glass. Therefore, the content of RO is 0 to 8%, preferably 0 to 5%, and more preferably 0 to 2%. In some embodiments, about 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8% RO may be included.
[0132] TiO2 is an optional component that helps to lower the melting temperature of glass and improve chemical stability. The present invention contains less than 5% TiO2, which can make the crystallization process of glass easy to control. Preferably, the content of TiO2 is less than 3%, and more preferably less than 1%. In some embodiments, it is further preferred that TiO2 is not contained. In some embodiments, about 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5% TiO2 may be included.
[0133] In some embodiments, the ratio of the total content of ZnO, RO, B2O3, and TiO2, ZnO+RO+B2O3+TiO2, to the content of P2O5 (ZnO+RO+B2O3+TiO2) / P2O5) is controlled to be below 1.5, which is beneficial to reducing the haze of microcrystalline glass and microcrystalline glass products, improving light transmittance, and improving the surface stress of microcrystalline glass products. Therefore, it is preferred that (ZnO+RO+B2O3+TiO2) / P2O5 is below 1.5, more preferably (ZnO+RO+B2O3+TiO2) / P2O5 is below 1.0, further preferably (ZnO+RO+B2O3+TiO2) / P2O5 is below 0.5, and further preferably (ZnO+RO+B2O3+TiO2) / P2O5 is below 0.2. In some embodiments, the value of (ZnO+RO+B2O3+TiO2) / P2O5 can be 0, greater than 0, 0.01, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, 0.95, 1.0, 1.05, 1.1, 1.15, 1.2, 1.25, 1.3, 1.35, 1.4, 1.45, 1.5.
[0134] Ln2O3 (Ln2O3 is one or more of La2O3, Gd2O3, and Y2O3) can reduce the difficulty of melting glass. When the content is too much, it will make it difficult to form crystals when the glass is crystallized, and the drop ball test height of microcrystalline glass and microcrystalline glass products will decrease. Therefore, the upper limit of the Ln2O3 content is 5%, preferably the upper limit is 3%, and more preferably the upper limit is 1%. In some embodiments, about 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5% Ln2O3 may be included.
[0135] In some embodiments, the matrix glass, glass-ceramic or glass-ceramic product may further contain 0-2% of a clarifier to improve the defoaming ability of the matrix glass, glass-ceramic or glass-ceramic product, and such a clarifier includes but is not limited to one or more of Sb2O3, SnO2, SnO, F (fluorine), Cl (chlorine) and Br (bromine), preferably Sb2O3 and SnO2 as clarifiers, more preferably Sb2O3 as clarifiers. When the above clarifiers exist alone or in combination, the upper limit of their content is preferably 1%, and more preferably 0.5%. In some embodiments, the amount of one or more of the above clarifiers is about 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, or 2%.
[0136] Without affecting the performance of the matrix glass, microcrystalline glass or microcrystalline glass products of the present invention, other components not mentioned above, such as Yb2O3, Nb2O5, WO3, Bi2O3, Ta2O5, TeO2, GeO2, etc., may be appropriately contained. However, in order to maintain the excellent performance of the matrix glass, microcrystalline glass or microcrystalline glass products of the present invention, the individual content or total content of Yb2O3, Nb2O5, WO3, Bi2O3, Ta2O5, TeO2, and GeO2 is preferably less than 5%, more preferably less than 2%, further preferably less than 1%, and further preferably not contained.
[0137] PbO and As2O3 are toxic substances, and even a small amount thereof does not meet the requirements of environmental protection. Therefore, in some embodiments of the present invention, it is preferred that PbO and As2O3 are not contained.
[0138] In some embodiments of the present invention, by containing a colorant, a colored matrix glass, a microcrystalline glass or a microcrystalline glass product can be prepared, and the matrix glass, the microcrystalline glass or the microcrystalline glass product can present different colors. Preferably, the colorant contains: NiO: 0-4%; and / or Ni2O3: 0-4%; and / or CoO: 0-2%; and / or Co2O3: 0-2%; and / or Fe2O3: 0-7%; and / or MnO2: 0-4%; and / or Er2O3: 0-8%; and / or Nd2O3: 0-8%; and / or Cu2O: 0-4%; and / or Pr2O5: 0-8%; and / or CeO2: 0-4%. The weight percentage content of the colorant and its function are described in detail as follows:
[0139] The brown or green matrix glass, glass-ceramic or glass-ceramic product prepared by the present invention uses NiO, Ni2O3 or Pr2O5 as a colorant. NiO and Ni2O3 are colorants used to prepare brown or green matrix glass, glass-ceramic or glass-ceramic products. The two components can be used alone or in combination. The content of each component is generally less than 4%, preferably less than 3%. If the content exceeds 4%, the colorant cannot be well dissolved in the matrix glass, glass-ceramic or glass-ceramic product. The lower limit of each content is more than 0.1%. If it is less than 0.1%, the color of the matrix glass, glass-ceramic or glass-ceramic product is not obvious. In some embodiments, about 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4.0% NiO or Ni2O3 may be included. When used in combination, the total amount of NiO and Ni2O3 is generally less than 4%, and the lower limit of the total amount is above 0.1%. In some embodiments, about 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4.0% NiO and Ni2O3 may be included. Pr2O5 is used as a colorant for green matrix glass, microcrystalline glass or microcrystalline glass products. It is used alone, and the content is generally less than 8%, preferably less than 6%. The lower limit of the content is above 0.4%. If it is less than 0.4%, the color of the matrix glass, microcrystalline glass or microcrystalline glass products will not be obvious.In some embodiments, about 0.4%, 0.6%, 0.8%, 1.0%, 1.2%, 1.4%, 1.6%, 1.8%, 2.0%, 2.2%, 2.4%, 2.6%, 2.8%, 3.0%, 3.2%, 3.4%, 3.6%, 3.8%, 4.0%, 4.2%, 4.4%, 4.6%, 4.8%, 5.0%, 5.2%, 5.4%, 5.6%, 5.8%, 6.0%, 6.2%, 6.4%, 6.6%, 6.8%, 7.0%, 7.2%, 7.4%, 7.6%, 7.8%, 8.0% Pr2O5 may be included.
[0140] The blue matrix glass, glass-ceramic or glass-ceramic product prepared by the present invention uses CoO or Co2O3 as a colorant. The two colorant components can be used alone or in combination. The respective contents are generally less than 2%, preferably less than 1.8%. If the content exceeds 2%, the colorant cannot be well dissolved in the matrix glass, glass-ceramic or glass-ceramic product. The respective lower limits of the contents are above 0.05%. If the content is less than 0.05%, the color of the matrix glass, glass-ceramic or glass-ceramic product is not obvious. In some embodiments, about 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0% of CoO or Co2O3 may be included. When used in combination, the total amount of CoO and Co2O3 does not exceed 2%, and the lower limit of the total amount is above 0.05%. In some embodiments, about 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0% of CoO and Co2O3 may be included.
[0141] The yellow matrix glass, glass-ceramics or glass-ceramics products prepared by the present invention use Cu2O or CeO2 as a colorant. The two colorant components are used alone or in combination, and the lower limits of their respective contents are above 0.5%. If the content is below 0.5%, the color of the matrix glass, glass-ceramics or glass-ceramics products is not obvious. The content of Cu2O used alone is below 4%, preferably below 3%. If the content exceeds 4%, the matrix glass is easily crystallized. In some embodiments, about 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4.0% Cu2O may be included. The CeO2 content alone is generally 4% or less, preferably 3% or less. If the content exceeds 4%, the matrix glass, microcrystalline glass or microcrystalline glass product has poor gloss. In some embodiments, about 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4.0% of CeO2 may be included. If two colorants are mixed, the total amount is generally less than 4%, and the lower limit of the total amount is more than 0.5%. In some embodiments, about 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4.0% CeO2 and Cu2O may be included.
[0142] The black or smoke gray matrix glass, glass-ceramics or glass-ceramics products prepared by the present invention use Fe2O3 alone as a colorant; or use a mixture of Fe2O3 and CoO as a colorant; or use a mixture of Fe2O3 and Co2O3 as a colorant; or use a mixture of Fe2O3, CoO and NiO as a colorant; or use a mixture of Fe2O3, Co2O3 and NiO as a colorant. The colorant used to prepare black and smoke gray matrix glass, glass-ceramics or glass-ceramics products mainly uses Fe2O3 for coloring, and the content is less than 7%, preferably less than 5%, and the lower limit of its content is more than 0.2%. In some embodiments, it may contain about 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6% , 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4.0%, 4.5%, 5.0%, 5.5%, 6.0%, 6.5%, 7.0% of Fe2O3. CoO and Co2O3 have absorption in visible light and can deepen the coloring of matrix glass, microcrystalline glass or microcrystalline glass products. Generally, when mixed with Fe2O3, their respective contents are less than 0.6%, and the lower limit is above 0.2%. In some embodiments, CoO and / or Co2O3 may be included in an amount of about 0.2%, 0.3%, 0.4%, 0.5%, or 0.6%. NiO absorbs visible light and can deepen the coloring of the matrix glass, glass-ceramics, or glass-ceramics products. Generally, when mixed, its content is less than 1%, and the lower limit of the total amount is more than 0.2%. In some embodiments, NiO may be included in an amount of about 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, or 1.0%.
[0143] The purple matrix glass, microcrystalline glass or microcrystalline glass products prepared by the present invention use MnO2 as a colorant, and the content is generally less than 4%, preferably less than 3%, and the lower limit of the content is above 0.1%. If it is less than 0.1%, the color of the matrix glass, microcrystalline glass or microcrystalline glass products is not obvious. In some embodiments, about 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4.0% MnO2 may be included.
[0144] The pink matrix glass, glass-ceramics or glass-ceramics products prepared by the present invention use Er2O3 as a colorant, and the content of Er2O3 is generally below 8%, preferably below 6%. Since the coloring efficiency of the rare earth element Er2O3 is low, when the content exceeds 8%, the color of the matrix glass, glass-ceramics or glass-ceramics products cannot be further deepened, but the cost is increased. The lower limit of the content is above 0.4%. If it is less than 0.4%, the color of the matrix glass, glass-ceramics or glass-ceramics products is not obvious. In some embodiments, about 0.4%, 0.6%, 0.8%, 1.0%, 1.2%, 1.4%, 1.6%, 1.8%, 2.0%, 2.2%, 2.4%, 2.6%, 2.8%, 3.0%, 3.2%, 3.4%, 3.6%, 3.8%, 4.0%, 4.2%, 4.4%, 4.6%, 4.8%, 5.0%, 5.2%, 5.4%, 5.6%, 5.8%, 6.0%, 6.2%, 6.4%, 6.6%, 6.8%, 7.0%, 7.2%, 7.4%, 7.6%, 7.8%, 8.0% Er2O3 may be included.
[0145] The purple-red matrix glass, glass-ceramics or glass-ceramics products prepared by the present invention use Nd2O3 as a colorant, and the content of Nd2O3 is generally below 8%, preferably below 6%. Since the rare earth element Nd2O3 has low coloring efficiency, even if the content exceeds 8%, the color of the matrix glass, glass-ceramics or glass-ceramics products cannot be further deepened, but the cost is increased. The lower limit of the content is above 0.4%. If it is less than 0.4%, the color of the matrix glass, glass-ceramics or glass-ceramics products is not obvious. In some embodiments, about 0.4%, 0.6%, 0.8%, 1.0%, 1.2%, 1.4%, 1.6%, 1.8%, 2.0%, 2.2%, 2.4%, 2.6%, 2.8%, 3.0%, 3.2%, 3.4%, 3.6%, 3.8%, 4.0%, 4.2%, 4.4%, 4.6%, 4.8%, 5.0%, 5.2%, 5.4%, 5.6%, 5.8%, 6.0%, 6.2%, 6.4%, 6.6%, 6.8%, 7.0%, 7.2%, 7.4%, 7.6%, 7.8%, 8.0% Nd2O3 may be included.
[0146] The red matrix glass, microcrystalline glass or microcrystalline glass products prepared by the present invention use a mixed colorant of Er2O3, Nd2O3 and MnO2. The Er ions in the glass absorb at 400-500nm, the Mn ions mainly absorb at 500nm, and the Nd ions mainly have strong absorption at 580nm. The mixture of the three substances can be used to prepare red matrix glass, microcrystalline glass or microcrystalline glass products. Since Er2O3 and Nd2O3 are rare earth colored, their coloring ability is relatively weak. The usage amount of Er2O3 is within 6%, the usage amount of Nd2O3 is within 4%, and the coloring of MnO2 is strong, and the usage amount is within 2%. The lower limit of the total amount of the mixed colorant used is above 0.9%.
[0147] The "does not contain" and "0%" recorded in this article mean that the compound, molecule or element is not intentionally added as a raw material to the matrix glass, microcrystalline glass or microcrystalline glass product of the present invention; however, as raw materials and / or equipment for producing matrix glass, microcrystalline glass or microcrystalline glass products, there will be certain impurities or components that are not intentionally added, which will be contained in small amounts or trace amounts in the final matrix glass, microcrystalline glass or microcrystalline glass product, and this situation is also within the scope of protection of the patent of this invention.
[0148] In some embodiments of the present invention, the crystal phase in the glass-ceramics and glass-ceramics products contains a nepheline crystal phase, which provides high strength for the glass-ceramics and glass-ceramics products of the present invention, and the drop ball test height and four-point bending strength of the glass-ceramics and glass-ceramics products become larger. In some embodiments, the glass-ceramics or glass-ceramics products contain a eucryptite crystal phase, in some embodiments, the glass-ceramics or glass-ceramics products contain a sodium nepheline crystal phase, and in some embodiments, the glass-ceramics or glass-ceramics products contain both eucryptite and sodium nepheline crystal phases. The glass-ceramics of the present invention have excellent chemical strengthening properties, and can also be processed into glass-ceramics products through a chemical strengthening process to obtain excellent mechanical strength. Through reasonable component design, the glass-ceramics and glass-ceramics products of the present invention can obtain a suitable grain size, so that the glass-ceramics and glass-ceramics products of the present invention have high strength. The glass-ceramics and glass-ceramics products in the present invention have a suitable content of crystal phases, so that the glass-ceramics and glass-ceramics products of the present invention have excellent mechanical properties.
[0149] The grain size and crystalline phase type in the glass-ceramics or glass-ceramics products of the present invention will affect the haze and light transmittance of the glass-ceramics or glass-ceramics products. In some embodiments, the haze of the glass-ceramics products or glass-ceramics with a thickness of less than 1 mm is less than 0.15%, preferably less than 0.12%, and more preferably less than 0.10%. In some embodiments, the grain size of the glass-ceramics products or glass-ceramics is less than 80 nm, preferably less than 60 nm, and more preferably less than 50 nm.
[0150] In some embodiments, the crystalline content and refractive index of the glass-ceramics or glass-ceramics products of the present invention affect the |B| value of the glass-ceramics or glass-ceramics products. When the glass-ceramics or glass-ceramics products are observed in the visible light range, they appear bluish or yellowish, affecting the optical properties of the product, which is indicated by the |B| value in LAB (chromaticity value of the color of the substance). The glass-ceramics or glass-ceramics products of the present invention present a low |B| value in the visible light range. In some embodiments, the average optical |B| value of the glass-ceramics products or glass-ceramics with a thickness of less than 1 mm at 400 to 800 nm is less than 1.5, preferably less than 1.0, and more preferably less than 0.8.
[0151] In some embodiments, the glass-ceramics or glass-ceramics products of the present invention exhibit high transparency in the visible light range (i.e., the glass-ceramics or glass-ceramics products are transparent). The glass-ceramics or glass-ceramics products exhibit high transmittance in the visible light range. In some preferred embodiments, the light transmittance of the glass-ceramics products or glass-ceramics with a thickness of less than 1 mm at 550 nm is preferably 88% or more, more preferably 89% or more, and even more preferably 90% or more.
[0152] In some embodiments, an antimicrobial component can be added to the matrix glass, glass-ceramic, or glass-ceramic product. The glass-ceramic or glass-ceramic product described herein can be used in applications such as kitchen or dining countertops, where exposure to harmful bacteria is likely. The antimicrobial components contained in the matrix glass, glass-ceramic, or glass-ceramic product include but are not limited to Ag, AgO, Cu, CuO, Cu2O, etc. In some embodiments, the content of the above antimicrobial components alone or in combination is less than 2%, preferably less than 1%.
[0153] The matrix glass, glass-ceramics and glass-ceramics products of the present invention can be produced and manufactured by the following methods:
[0154] Forming matrix glass: Mix the raw materials evenly according to the component ratio, put the uniform mixture into a platinum or quartz crucible, and melt it in an electric furnace or gas furnace at a temperature range of 1250-1650℃ for 5-24 hours according to the melting difficulty of the glass composition. After melting and stirring to make it uniform, it is cooled to an appropriate temperature and cast into a mold, and slowly cooled.
[0155] The matrix glass of the present invention can be formed by a well-known method.
[0156] The matrix glass of the present invention is subjected to crystallization treatment by a crystallization process after forming or after forming processing, and crystals are uniformly separated out inside the glass. The crystallization treatment can be carried out by one stage, or by two stages, and preferably by two stages. The treatment of the nucleation process is carried out at the first temperature, and then the treatment of the crystal growth process is carried out at the second temperature higher than the nucleation process temperature. The crystallization treatment carried out at the first temperature is called the first crystallization treatment, and the crystallization treatment carried out at the second temperature is called the second crystallization treatment.
[0157] In order to obtain the desired physical properties of glass-ceramics, the preferred crystallization process is:
[0158] The above-mentioned crystallization treatment is carried out in one stage, and the nucleation process and the crystal growth process can be carried out continuously. That is, the temperature is raised to a specified crystallization treatment temperature, and after reaching the crystallization treatment temperature, the temperature is maintained for a certain period of time, and then the temperature is lowered. The crystallization treatment temperature is preferably 580 to 750°C, and in order to precipitate the desired crystalline phase, it is more preferably 600 to 700°C. The holding time at the crystallization treatment temperature is preferably 0 to 8 hours, and more preferably 1 to 6 hours.
[0159] When the crystallization treatment is performed in two stages, the first temperature is preferably 500 to 620° C., and the second temperature is preferably 620 to 750° C. The holding time at the first temperature is preferably 0 to 24 hours, more preferably 2 to 15 hours. The holding time at the second temperature is preferably 0 to 10 hours, more preferably 0.5 to 6 hours.
[0160] The above-mentioned holding time of 0 hours means that the temperature starts to drop or rise again within less than 1 minute after reaching the temperature.
[0161] In some embodiments, the matrix glass or glass-ceramics described herein can be manufactured into a formed body by various processes, including but not limited to sheets, and the processes include but are not limited to slit drawing, float process, rolling and other processes for forming sheets known in the art. Alternatively, the matrix glass or glass-ceramics can be formed by float process or rolling process. The formed body of the present invention also includes lenses, prisms, etc.
[0162] The matrix glass or glass-ceramics of the present invention can be used to manufacture a glass molded body or a glass-ceramics molded body in the form of a sheet by grinding or polishing, but the method for manufacturing a glass molded body or a glass-ceramics molded body is not limited to these methods.
[0163] The matrix glass or glass-ceramics of the present invention can be prepared into glass molded bodies or glass-ceramics molded bodies of various shapes by heat bending or pressing at a certain temperature, but is not limited to these methods.
[0164] In some embodiments, a glass forming body or a glass-ceramic forming body can be formed by a heat bending process. The heat bending process is a process in which 2D or 2.5D glass or glass-ceramic is placed in a mold and a 3D curved glass forming body or glass-ceramic forming body is formed by sequentially performing steps including heating preheating, pressurizing, and cooling under pressure in a heat bending machine.
[0165] In some embodiments, the glass-ceramic forming body has a 2.5D or 3D configuration, i.e., the glass-ceramic forming body has a non-planar configuration. As used herein, "non-planar configuration" means that in a 2.5D or 3D shape, at least a portion of the glass-ceramic forming body extends outward or along an angle with a plane defined by the original, laid-out configuration of the 2D matrix glass. A 2.5D or 3D glass-ceramic forming body formed from a matrix glass may have one or more protrusions or curved portions.
[0166] In some embodiments, in combination with the growth of the crystal phase and the transformation of the crystal phase in the microcrystalline glass, the manufacturing method of the microcrystalline glass forming body is a hot bending process method. Specifically, the method includes pre-crystallization and hot working forming. The pre-crystallization described in the present invention is to form pre-crystallized glass by controlling the crystallization process of the matrix glass, and the crystallinity of the pre-crystallized glass does not reach the crystallinity required by the performance index of the target microcrystalline glass forming body. The pre-crystallized glass is then formed into a microcrystalline glass forming body through a hot working forming process.
[0167] In some embodiments, a method for manufacturing a glass-ceramic formed body comprises the following steps:
[0168] 1) subjecting the matrix glass to a crystallization heat treatment process, including heating, heat preservation nucleation, heating, heat preservation crystallization, and cooling to room temperature to form pre-crystallized glass;
[0169] 2) The pre-crystallized glass is heat-processed and formed into a microcrystalline glass formed body.
[0170] The crystallization heat treatment process of the present invention comprises: heating the matrix glass at a certain temperature T h and time t h Under the condition of nucleation, then at a certain temperature T c and time t c The crystallinity of the pre-crystallized glass obtained did not reach the crystallinity required by the performance index of the target microcrystalline glass-ceramic formed body. Using the XRD test data, the total content of the main crystalline phase in the crystallinity of the pre-crystallized glass was calculated by the Rietveld full spectrum fitting refinement method. c1 . The pre-crystallization of the present invention is a complete process in terms of the process, including a nucleation process, one, two or three or more crystallization processes, etc. It is a complete process of heating, heat preservation, heating again, heat preservation..., and then cooling to room temperature according to the process. Different from the primary crystallization, secondary crystallization... mentioned in some documents or patents, the present invention is actually only the first crystallization, the second crystallization... in a complete crystallization process, and the middle is continuous, and there is no process of heating up again after cooling to room temperature.
[0171] The hot working forming of the present invention refers to the hot working process forming the pre-crystallized glass under certain conditions of temperature, time, pressure, etc., and the hot working forming includes more than one hot working process, and the hot working process includes but is not limited to pressing, bending or drawing the pre-crystallized glass under certain conditions of temperature, time, pressure, etc. In the hot working forming process, sometimes a molded body with a complex shape cannot be completed by one hot working, and may need to be completed by multiple hot workings of more than two times.
[0172] In some embodiments, the method for manufacturing the glass-ceramic formed body is a hot bending process. Specifically, in some embodiments, the method for manufacturing the glass-ceramic formed body includes the following steps:
[0173] 1) Preheating: Place the matrix glass or pre-crystallized glass or microcrystalline glass in the mold, and the mold passes through each heating station in the heat bending machine in turn, and stays at each station for a certain period of time to keep warm. The temperature in the preheating zone is 400-800°C, the pressure is 0.01-0.05MPa, and the time is 40-200s. In some embodiments, for a heat bending machine with 5 preheating stations, the initial temperature rise is generally set to about 500°C, and the subsequent stations gradually increase the temperature. The temperature gradient between two adjacent stations gradually decreases from low temperature to high temperature, and the temperature difference between the last preheating station and the first molding station is within 20°C.
[0174] 2) Pressurized molding: After preheating, the mold is transferred to the molding station. The hot bending machine applies a certain pressure to the mold. The pressure range is 0.1-0.8Mpa. The pressure is determined according to factors such as glass thickness and curvature. The molding station temperature range is 650-850℃, and the molding time range is 40-200s.
[0175] 3) Maintain pressure and cool down: transfer the mold to the cooling station and cool down the mold step by step. The cooling temperature range is controlled at 750-500℃, the pressure is 0.01-0.05Mpa, and the time is 40-200s.
[0176] In addition to controlling the appearance quality of ordinary high-aluminum glass, the hot bending process of microcrystalline glass forming bodies also requires controlling the impact of crystal growth and development during the hot bending process on the performance of the microcrystalline glass. For example, 3D curved microcrystalline glass used for display devices or electronic equipment casings requires close attention to light transmittance, haze, |B| value and uniformity after hot bending.
[0177] The change in the crystalline phase before and after hot bending determines the uniformity of the size of the microcrystalline glass formed body, the possibility of mass production and cost control. The matrix glass and microcrystalline glass of the present invention have excellent thermal processing properties. After hot bending, the change in the crystalline phase content is less than 20%, preferably less than 15%, and further preferably less than 10%, which can ensure the uniformity of the haze and |B| value of the microcrystalline glass formed body obtained after hot bending.
[0178] The matrix glass, glass-ceramic, and glass-ceramic articles described herein can have any reasonably useful thickness.
[0179] In addition to improving mechanical properties by precipitating crystals, the microcrystalline glass of the present invention can also obtain more excellent mechanical properties by forming a compressive stress layer, thereby making microcrystalline glass products.
[0180] In some embodiments, the matrix glass or glass-ceramics can be processed into sheets, and / or shaped (such as punching, hot bending, etc.), polished and / or brushed after shaping, and then chemically strengthened through a chemical strengthening process to form a glass-ceramics product. In some embodiments, the glass-ceramics formed body can be chemically strengthened through a chemical strengthening process to form a glass-ceramics product.
[0181] The chemical strengthening described in the present invention is an ion exchange method. During the ion exchange process, smaller metal ions in the matrix glass or glass-ceramic or glass-ceramic formed body are replaced or "exchanged" by larger metal ions of the same valence state near the matrix glass or glass-ceramic or glass-ceramic formed body. The replacement of smaller ions with larger ions forms compressive stress on the surface of the matrix glass or glass-ceramic or glass-ceramic formed body and tensile stress inside.
[0182] In some embodiments, the metal ion is a monovalent alkali metal ion (e.g., Na + , K + , Rb + , Cs + The ion exchange is carried out by immersing the matrix glass or glass-ceramic or glass-ceramic body in a salt bath containing at least one molten salt of a larger metal ion, which is used to replace the smaller metal ions in the matrix glass or glass-ceramic or glass-ceramic body. Alternatively, other monovalent metal ions such as Ag + , Tl + , Cu + The one or more ion exchange processes used to chemically strengthen the matrix glass or glass-ceramic or glass-ceramic forming body may include, but are not limited to, immersing it in a single salt bath, or immersing it in multiple salt baths of the same or different compositions with washing and / or annealing steps between immersions.
[0183] In some embodiments, the matrix glass or glass-ceramic or glass-ceramic body can be ion exchanged by immersing in a salt bath of molten Na salt (such as NaNO3) at a temperature of about 350 to 470°C for about 1 to 36 hours, preferably in the temperature range of 380 to 460°C, and preferably in the time range of 2 to 10 hours. In this embodiment, Na ions replace part of the Li ions in the matrix glass or glass-ceramic or glass-ceramic body, thereby forming a surface compression layer and exhibiting high mechanical properties. In some embodiments, the matrix glass or glass-ceramic or glass-ceramic body can be ion exchanged by immersing in a salt bath of molten K salt (such as KNO3) at a temperature of about 360 to 450°C for 1 to 36 hours, preferably in the time range of 1 to 10 hours. In some embodiments, the matrix glass or glass-ceramic or glass-ceramic body can be ion exchanged by immersing in a mixed salt bath of molten K salt and Na salt at a temperature of about 360 to 450°C for 1 to 36 hours, preferably in the time range of 2 to 24 hours.
[0184] The performance indicators of the glass-ceramics or glass-ceramics products of the present invention are tested by the following methods:
[0185] [Haze]
[0186] The spectrophotometer Minolta CM-3600A was used to prepare samples with a diameter of less than 1 mm and the test was carried out according to the GB2410-80 standard.
[0187] [Grain size]
[0188] Using a SEM scanning electron microscope, the microcrystalline glass is surface treated in HF acid, gold is sprayed on the surface of the microcrystalline glass, and the surface is scanned under the SEM scanning electron microscope to determine the size of its grains.
[0189] [Light transmittance]
[0190] The light transmittances described in this article are all external transmittances, sometimes referred to as transmittance.
[0191] The samples were processed to a thickness of less than 1 mm and polished in parallel with the opposite surfaces. The light transmittance at 550 nm was measured using a Minolta CM-3600A spectrophotometer.
[0192] [Surface stress] and [Ion exchange layer depth]
[0193] The surface stress was measured using a glass surface stress meter SLP-2000.
[0194] The depth of the ion exchange layer was measured using a glass surface stress meter SLP-2000.
[0195] The calculation was performed under the measurement conditions that the refractive index of the sample was 1.56 and the photoelastic constant was 24.5 [(nm / cm) / Mpa].
[0196] [Drop ball test height]
[0197] A sample of a microcrystalline glass product with a length and width of 150mm×73mm and a thickness of less than 1mm is placed on a glass supporting fixture, and a 132g steel ball is dropped from a specified height. The maximum drop ball test height that the sample can withstand without breaking is the impact. Specifically, the test is implemented starting from a drop ball test height of 400mm. Without breaking, the height is changed in sequence through 400mm, 500mm, 600mm, 700mm and above, with an interval of 100mm each time. For the embodiments with a "drop ball test height", microcrystalline glass products are used as test objects. The test data recorded as 1600mm in the embodiment indicates that the sample has withstood an impact of 1500mm and has not broken. When it was raised to 1600mm for testing, it broke. Therefore, the drop ball test height is 1600mm. The drop ball test height in the present invention is sometimes referred to as the drop ball height.
[0198] [Body falling ball height]
[0199] Place a microcrystalline glass sample with a length and width of 150mm×73mm and a thickness of less than 1mm on a glass supporting fixture, and drop a 32g steel ball from a specified height. The maximum drop ball test height that the sample can withstand without breaking is the main body drop ball height. Specifically, the test starts from a drop ball test height of 400mm. Without breaking, the height is changed in sequence through 400mm, 500mm, 600mm, 700mm and above, with an interval of 100mm each time. For the embodiments with a "main body drop ball height", microcrystalline glass is used as the test object, which is the drop ball test height of microcrystalline glass. The test data recorded as 1300mm in the embodiment indicates that the sample has withstood an impact of 1200mm without breaking, and it broke when it was raised to 1300mm for the test, so the main body drop ball height is 1300mm.
[0200] [Four-point bending strength]
[0201] The microcomputer-controlled electronic universal testing machine CMT6502 was used, the sample specification was a thickness of less than 1 mm, and the test was performed according to ASTM C 158-2002. In the present invention, the four-point bending strength is sometimes referred to as the bending strength.
[0202] [Vickers hardness]
[0203] The load when a diamond square pyramid indenter with an angle of 136° between the opposite faces is pressed into a pyramid-shaped depression on the test surface divided by the surface area (mm) calculated by the length of the depression.2 ) value. The test load was 200 g and the holding time was 20 seconds. In the present invention, Vickers hardness may be simply referred to as hardness.
[0204] [|B|value]
[0205] Use Minolta CM-700d to test the B value. The sample specification is less than 1mm thick. Use the matching calibration long tube and short tube to perform instrument zero calibration and white plate calibration respectively. After calibration, use the long tube to perform air test again to determine the stability and calibration reliability of the instrument (B≤0.05). After the instrument is calibrated, place the product on the zero long tube for testing.
[0206] The |B| value is the absolute value of the B value.
[0207] The microcrystalline glass product of the present invention has the following properties:
[0208] 1) In some embodiments, the four-point bending strength of the glass-ceramic product with a thickness of 1 mm or less is 700 MPa or more, preferably 750 MPa or more, and more preferably 800 MPa or more. The thickness is preferably 0.2 to 1 mm, more preferably 0.3 to 0.9 mm, more preferably 0.5 to 0.8 mm, and even more preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.7 mm, or 0.75 mm.
[0209] 2) In some embodiments, the depth of the ion exchange layer of the microcrystalline glass product is 50 μm or more, preferably 60 μm or more, more preferably 80 μm or more, and further preferably 100 μm or more.
[0210] 3) In some embodiments, the drop ball test height of the glass-ceramic product with a thickness of 1 mm or less is 1100 mm or more, preferably 1300 mm or more, and more preferably 1500 mm or more. The thickness is preferably 0.2 to 1 mm, more preferably 0.3 to 0.9 mm, further preferably 0.5 to 0.8 mm, and further preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.7 mm, or 0.75 mm.
[0211] 4) In some embodiments, the Vickers hardness (H v ) is 750kgf / mm 2 Above, preferably 780kgf / mm 2 More preferably 800kgf / mm 2 More preferably, 810 kgf / mm 2 above.
[0212] 5) In some embodiments, the grain size of the microcrystalline glass product is 80 nm or less, preferably 60 nm or less, more preferably 50 nm or less, and even more preferably 40 nm or less.
[0213] 6) In some embodiments, the surface stress of the microcrystalline glass product is greater than 150 MPa, preferably greater than 170 MPa, and more preferably greater than 190 MPa.
[0214] 7) In some embodiments, the haze of the microcrystalline glass product with a thickness of 1 mm or less is 0.15% or less, preferably 0.12% or less, and more preferably 0.10% or less. The thickness is preferably 0.2 to 1 mm, more preferably 0.3 to 0.9 mm, further preferably 0.5 to 0.8 mm, and further preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.7 mm, or 0.75 mm.
[0215] 8) In some embodiments, the light transmittance of the microcrystalline glass product with a thickness of 1 mm or less at a wavelength of 550 nm is 88% or more, preferably 89% or more, more preferably 90% or more, and further preferably 91% or more. The thickness is preferably 0.2 to 1 mm, more preferably 0.3 to 0.9 mm, further preferably 0.5 to 0.8 mm, and further preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.7 mm, or 0.75 mm.
[0216] 9) In some embodiments, for a glass-ceramic product having a thickness of less than 1 mm, the average optical |B| value at 400-800 nm is less than 1.5, preferably less than 1.0, and more preferably less than 0.8. The thickness is preferably 0.2-1 mm, more preferably 0.3-0.9 mm, further preferably 0.5-0.8 mm, and further preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.7 mm, or 0.75 mm.
[0217] The microcrystalline glass of the present invention has the following properties:
[0218] 1) In some embodiments, the grain size of the glass-ceramics is 80 nm or less, preferably 60 nm or less, more preferably 50 nm or less, and further preferably 40 nm or less.
[0219] 2) In some embodiments, the haze of the microcrystalline glass with a thickness of 1 mm or less is 0.15% or less, preferably 0.12% or less, and more preferably 0.10% or less. The thickness is preferably 0.2 to 1 mm, more preferably 0.3 to 0.9 mm, further preferably 0.5 to 0.8 mm, and further preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.7 mm, or 0.75 mm.
[0220] 3) In some embodiments, the light transmittance of the microcrystalline glass with a thickness of 1 mm or less at a wavelength of 550 nm is 88% or more, preferably 89% or more, more preferably 90% or more, and further preferably 91% or more. The thickness is preferably 0.2 to 1 mm, more preferably 0.3 to 0.9 mm, further preferably 0.5 to 0.8 mm, and further preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.7 mm, or 0.75 mm.
[0221] 4) In some embodiments, the body ball drop height of the microcrystalline glass with a thickness of 1 mm or less is 1000 mm or more, preferably 1200 mm or more, and more preferably 1400 mm or more. The thickness is preferably 0.2 to 1 mm, more preferably 0.3 to 0.9 mm, further preferably 0.5 to 0.8 mm, and further preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.7 mm, or 0.75 mm.
[0222] 5) In some embodiments, for a glass-ceramic having a thickness of less than 1 mm, the average optical |B| value at 400-800 nm is less than 1.5, preferably less than 1.0, and more preferably less than 0.8. The thickness is preferably 0.2-1 mm, more preferably 0.3-0.9 mm, further preferably 0.5-0.8 mm, and further preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.7 mm, or 0.75 mm.
[0223] 6) In some embodiments, the Vickers hardness (H v ) is 650kgf / mm 2 Above, preferably 680kgf / mm 2 More preferably 700kgf / mm 2 above.
[0224] The microcrystalline glass, microcrystalline glass products, matrix glass, glass formed bodies, and microcrystalline glass formed bodies of the present invention can be widely made into glass cover plates or glass components due to the above-mentioned excellent properties; at the same time, the microcrystalline glass, microcrystalline glass products, matrix glass, glass formed bodies, and microcrystalline glass formed bodies of the present invention can be applied to electronic devices or display devices, such as mobile phones, watches, computers, touch screens, etc., for manufacturing protective glass for mobile phones, smart phones, tablet computers, laptops, PDAs, televisions, personal computers, MTA machines, or industrial displays, or for manufacturing touch screens, protective windows, car windows, train windows, aviation machinery windows, touch screen protective glass, or for manufacturing hard disk substrates or solar cell substrates, or for manufacturing white household appliances, such as for manufacturing refrigerator parts or kitchen utensils.
[0225] Example
[0226] In order to further clearly illustrate and describe the technical solution of the present invention, the following non-limiting examples are provided. The examples of the present invention have been tried hard to ensure the accuracy of the numerical values, but some errors and deviations must be taken into account. The composition of the microcrystalline glass or microcrystalline glass product is given in weight % based on the oxide and has been standardized to 100%.
[0227] <Glass-ceramic Example>
[0228] This embodiment adopts the above-mentioned method for manufacturing microcrystalline glass to obtain microcrystalline glass having the composition shown in Tables 1 to 3. In addition, the characteristics of each microcrystalline glass are measured by the test method described in the present invention, and the measurement results are shown in Tables 1 to 3. The thickness of the test sample used for the body drop ball height, haze, light transmittance, |B| value, etc. in the following embodiments is 0.7 mm.
[0229] Table 1.
[0230]
[0231]
[0232] Table 2.
[0233]
[0234]
[0235] Table 3.
[0236]
[0237]
[0238] <Glass-ceramic product example>
[0239] This embodiment adopts the manufacturing method of the above-mentioned microcrystalline glass products to obtain microcrystalline glass products with the compositions shown in Tables 4 to 6. In addition, the characteristics of each microcrystalline glass product are measured by the test method described in the present invention, and the measurement results are shown in Tables 4 to 6. The thickness of the test sample used for the four-point bending strength, drop ball test height, haze, light transmittance, |B| value, etc. in the following embodiments is 0.7 mm.
[0240] Table 4.
[0241]
[0242]
[0243] Table 5.
[0244]
[0245]
[0246] Table 6.
[0247]
[0248]
Claims
1. A glass-ceramic product, characterized in that: Its components, expressed in weight percentage, include: SiO2: 40-60%; Al2O3: 20-40%; Li2O: 2-15%; Na2O: 3-20%; P2O5+ZrO2: 1-15%, (ZnO+RO+B2O3+TiO2) / P2O5 is less than 1.5, (P2O5+Na2O) / Li2O is 0.5-2.5, and the RO is one or more of MgO, CaO, SrO, and BaO.
2. The glass-ceramic product according to claim 1, characterized in that: Its components, expressed in weight percentage, also contain: K2O: 0-8%; and / or ZnO: 0-6%; and / or B2O3: 0-6%; and / or RO: 0-8%; and / or TiO2: 0-5%; and / or Ln2O3: 0-5%; and / or clarifier: 0-2%, wherein RO is one or more of MgO, CaO, SrO, and BaO, and Ln2O3 is one or more of La2O3, Gd2O3, and Y2O3.
3. A glass-ceramic product, characterized in that: Its components, expressed by weight percentage, are SiO2: 40-60%; Al2O3: 20-40%; Li2O: 2-15%; Na2O: 3-20%; P2O5+ZrO2: 1-15%; K2O: 0-8%; ZnO: 0~6%; B2O3: 0~6%; RO: 0~8%; TiO2: 0~5%; Ln2O3: 0~5%; Clarifier: composition of 0-2%, (ZnO+RO+B2O3+TiO2) / P2O5 is less than 1.5, (P2O5+Na2O) / Li2O is 0.5-2.5, RO is one or more of MgO, CaO, SrO, BaO, Ln2O3 is one or more of La2O3, Gd2O3, Y2O3.
4. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: Its components are expressed in weight percentage, wherein: (Al2O3+Na2O) / P2O5 is 3.0-30.
0.
5. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: Its components are expressed in weight percentage, wherein: (Al2O3+Na2O) / P2O5 is 4.0-20.
0.
6. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: Its components are expressed in weight percentage, wherein: (Al2O3+Na2O) / P2O5 is 5.0-15.
0.
7. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: Its components are expressed in weight percentage, wherein: (Al2O3+Na2O) / P2O5 is 6.0-10.
0.
8. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: Its components are expressed in weight percentage, wherein SiO2 / Al2O3 is 1.2 to 2.
8.
9. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: Its components are expressed in weight percentage, wherein SiO2 / Al2O3 is 1.3 to 2.
5.
10. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: Its components are expressed in weight percentage, wherein SiO2 / Al2O3 is 1.5 to 2.
2.
11. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: Its components are expressed in weight percentage, wherein SiO2 / Al2O3 is 1.6 to 2.
0.
12. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: Its components are expressed in weight percentage, wherein SiO2 / (Na2O+B2O3) is 2.0-15.
0.
13. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: Its components are expressed in weight percentage, wherein SiO2 / (Na2O+B2O3) is 3.0-10.
0.
14. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: Its components are expressed in weight percentage, wherein SiO2 / (Na2O+B2O3) is 4.0 to 8.
0.
15. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: Its components are expressed in weight percentage, wherein SiO2 / (Na2O+B2O3) is 5.0-7.
0.
16. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: Its components are expressed in weight percentage, wherein: (Na2O+Li2O) / SiO2 is 0.1 to 0.
8.
17. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: Its components are expressed in weight percentage, wherein: (Na2O+Li2O) / SiO2 is 0.15-0.
7.
18. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: Its components are expressed in weight percentage, wherein: (Na2O+Li2O) / SiO2 is 0.2-0.
6.
19. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: Its components are expressed in weight percentage, wherein: (Na2O+Li2O) / SiO2 is 0.25-0.
5.
20. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: Its components are expressed in weight percentage, wherein: (ZrO2+ZnO) / Na2O is less than 2.
0.
21. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: Its components are expressed in weight percentage, wherein: (ZrO2+ZnO) / Na2O is less than 1.
5.
22. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: Its components are expressed in weight percentage, wherein: (ZrO2+ZnO) / Na2O is 0.01-1.
0.
23. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: Its components are expressed in weight percentage, wherein: (ZrO2+ZnO) / Na2O is 0.1-0.
5.
24. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: Its components are expressed in weight percentage, wherein: (P2O5+Na2O) / Li2O is 0.8-2.
5.
25. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: Its components are expressed in weight percentage, wherein: (P2O5+Na2O) / Li2O is 1.0 to 2.
5.
26. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: Its components are expressed in weight percentage, wherein: (P2O5+Na2O) / Li2O is 1.5 to 2.
5.
27. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: Its components are expressed in weight percentage, wherein K2O / ZrO2 is greater than 0.
1.
28. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: The components are expressed in weight percentage, wherein K2O / ZrO2 is 0.2-10.
0.
29. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: The components are expressed in weight percentage, wherein K2O / ZrO2 is 0.3-5.
0.
30. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: Its components are expressed in weight percentage, wherein K2O / ZrO2 is 0.4-1.
5.
31. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: Its components are expressed in weight percentage, wherein: (ZnO+RO+B2O3+TiO2) / P2O5 is less than 1.0, and the RO is one or more of MgO, CaO, SrO, and BaO.
32. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: Its components are expressed in weight percentage, wherein: (ZnO+RO+B2O3+TiO2) / P2O5 is less than 0.5, and the RO is one or more of MgO, CaO, SrO, and BaO.
33. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: Its components are expressed in weight percentage, wherein: (ZnO+RO+B2O3+TiO2) / P2O5 is less than 0.2, and the RO is one or more of MgO, CaO, SrO, and BaO.
34. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: Its components are expressed in weight percentage, wherein: SiO2: 43-55%; and / or Al2O3: 23-36%; and / or Li2O: 3-13%; and / or Na2O: 5-15%; and / or P2O5+ZrO2: 2-12%; and / or K2O: 0-5%; and / or ZnO: 0-3%; and / or B2O3: 0-3%; and / or RO: 0-5%; and / or TiO2: 0-3%; and / or Ln2O3: 0-3%; and / or clarifier: 0-1%, wherein RO is one or more of MgO, CaO, SrO and BaO, and Ln2O3 is one or more of La2O3, Gd2O3 and Y2O3.
35. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: Its components are expressed in weight percentage, wherein: SiO2: 46-53%; and / or Al2O3: 25.5-32%; and / or Li2O: 5.5-11%; and / or Na2O: 6.5-12%; and / or P2O5+ZrO2: 4-10%; and / or K2O: 0.1-3%; and / or ZnO: 0-1%; and / or B2O3: 0-1%; and / or RO: 0-2%; and / or TiO2: 0-1%; and / or Ln2O3: 0-1%; and / or clarifier: 0-0.5%, wherein RO is one or more of MgO, CaO, SrO and BaO, and Ln2O3 is one or more of La2O3, Gd2O3 and Y2O3.
36. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: The components are expressed by weight percentage, wherein: ZrO2: 0-6%; and / or P2O5: 0-10%.
37. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: The components are expressed by weight percentage, wherein: ZrO2: 0-5%; and / or P2O5: 1-8%.
38. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: The components are expressed by weight percentage, wherein: ZrO2: 0.1-3%; and / or P2O5: 2-6%.
39. The glass-ceramic product according to claim 1 or 2, characterized in that: Its components, expressed in weight percentage, also contain: Yb2O3+Nb2O5+WO3+Bi2O3+Ta2O5+TeO2+GeO2: 0-5%.
40. The glass-ceramic product according to claim 1 or 2, characterized in that: Its components, expressed in weight percentage, also contain: Yb2O3+Nb2O5+WO3+Bi2O3+Ta2O5+TeO2+GeO2: 0-2%.
41. The glass-ceramic product according to claim 1 or 2, characterized in that: Its components, expressed in weight percentage, also include: Yb2O3+Nb2O5+WO3+Bi2O3+Ta2O5+TeO2+GeO2: 0~1%.
42. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: The microcrystalline glass product contains nepheline crystal phase; and / or lithium silicate crystal phase; and / or lithium phosphate crystal phase; and / or petalite crystal phase; and / or quartz crystal phase.
43. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: The main crystal phase of the microcrystalline glass product is the nepheline crystal phase, or the microcrystalline glass product only contains the nepheline crystal phase.
44. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: In the microcrystalline glass product, the weight percentage of the nepheline crystal phase in the microcrystalline glass product is 10 to 80%.
45. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: In the microcrystalline glass product, the weight percentage of the nepheline crystal phase in the microcrystalline glass product is 20 to 70%.
46. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: In the microcrystalline glass product, the weight percentage of the nepheline crystal phase in the microcrystalline glass product is 30-60%.
47. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: The ion exchange layer depth of the microcrystalline glass product is greater than 50 μm; and / or the Vickers hardness is 750 kgf / mm 2 and / or the grain size is 80 nm or less; and / or the surface stress is 150 MPa or more.
48. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: The ion exchange layer depth of the microcrystalline glass product is greater than 60 μm; and / or the Vickers hardness is 780 kgf / mm 2 and / or the grain size is 60 nm or less; and / or the surface stress is 170 MPa or more.
49. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: The ion exchange layer depth of the microcrystalline glass product is greater than 80 μm; and / or the Vickers hardness is 800 kgf / mm 2 and / or the grain size is 50 nm or less; and / or the surface stress is 190 MPa or more.
50. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: The ion exchange layer depth of the microcrystalline glass product is greater than 100 μm; and / or the Vickers hardness is 810 kgf / mm 2 and / or the grain size is less than 40 nm.
51. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: Microcrystalline glass products with a thickness of less than 1 mm have a four-point bending strength of more than 700 MPa; and / or a drop ball test height of more than 1100 mm; and / or a haze of less than 0.15%; and / or a light transmittance of 550 nm wavelength of more than 88%; and / or an average light |B| value of 400-800 nm is less than 1.
5.
52. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: Microcrystalline glass products with a thickness of less than 1 mm have a four-point bending strength of more than 750 MPa; and / or a drop ball test height of more than 1300 mm; and / or a haze of less than 0.12%; and / or a light transmittance of 550 nm wavelength of more than 89%; and / or an average light |B| value of 400-800 nm is less than 1.
0.
53. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: Microcrystalline glass products with a thickness of less than 1 mm have a four-point bending strength of more than 800 MPa; and / or a drop ball test height of more than 1500 mm; and / or a haze of less than 0.10%; and / or a light transmittance of 550 nm wavelength of more than 90%; and / or an average light |B| value of 400-800 nm is less than 0.
8.
54. The glass-ceramic product according to any one of claims 1 to 3, characterized in that: For glass-ceramic products with a thickness of less than 1 mm, the light transmittance at a wavelength of 550 nm is over 91%.
55. The glass-ceramic product according to claim 51, characterized in that The thickness of the microcrystalline glass product is 0.2 to 1 mm.
56. The glass-ceramic product according to claim 51, characterized in that The thickness of the microcrystalline glass product is 0.3-0.9 mm.
57. The glass-ceramic product according to claim 51, characterized in that The thickness of the microcrystalline glass product is 0.5 to 0.8 mm.
58. The glass-ceramic product according to claim 51, characterized in that The thickness of the microcrystalline glass product is 0.55 mm, 0.6 mm, 0.68 mm, 0.7 mm or 0.75 mm.
59. The glass-ceramic product according to claim 1 or 2, characterized in that: Its components, expressed in weight percentage, also contain: NiO: 0-4%; and / or Ni2O3: 0-4%; and / or CoO: 0-2%; and / or Co2O3: 0-2%; and / or Fe2O3: 0-7%; and / or MnO2: 0-4%; and / or Er2O3: 0-8%; and / or Nd2O3: 0-8%; and / or Cu2O: 0-4%; and / or Pr2O3: 0-8%; and / or CeO2: 0-4%.
60. Glass-ceramics, characterized in that: Its components, expressed in weight percentage, include: SiO2: 40-60%; Al2O3: 20-40%; Li2O: 2-15%; Na2O: 3-20%; P2O5+ZrO2: 1-15%, (ZnO+RO+B2O3+TiO2) / P2O5 is less than 1.5, (P2O5+Na2O) / Li2O is 0.5-2.5, and the RO is one or more of MgO, CaO, SrO, and BaO.
61. The glass-ceramic according to claim 60, characterized in that: Its components, expressed in weight percentage, also contain: K2O: 0-8%; and / or ZnO: 0-6%; and / or B2O3: 0-6%; and / or RO: 0-8%; and / or TiO2: 0-5%; and / or Ln2O3: 0-5%; and / or clarifier: 0-2%, wherein RO is one or more of MgO, CaO, SrO, and BaO, and Ln2O3 is one or more of La2O3, Gd2O3, and Y2O3.
62. Glass-ceramics, characterized in that: Its components, expressed by weight percentage, are SiO2: 40-60%; Al2O3: 20-40%; Li2O: 2-15%; Na2O: 3-20%; P2O5+ZrO2: 1-15%; K2O: 0-8%; ZnO: 0~6%; B2O3: 0~6%; RO: 0~8%; TiO2: 0~5%; Ln2O3: 0~5%; Clarifier: composition of 0-2%, (ZnO+RO+B2O3+TiO2) / P2O5 is less than 1.5, (P2O5+Na2O) / Li2O is 0.5-2.5, RO is one or more of MgO, CaO, SrO, BaO, Ln2O3 is one or more of La2O3, Gd2O3, Y2O3.
63. The glass-ceramics according to any one of claims 60 to 62, characterized in that: Its components are expressed in weight percentage, wherein: (Al2O3+Na2O) / P2O5 is 3.0-30.
0.
64. The glass-ceramics according to any one of claims 60 to 62, characterized in that: Its components are expressed in weight percentage, wherein: (Al2O3+Na2O) / P2O5 is 4.0-20.
0.
65. The glass-ceramics according to any one of claims 60 to 62, characterized in that: Its components are expressed in weight percentage, wherein: (Al2O3+Na2O) / P2O5 is 5.0-15.
0.
66. The glass-ceramics according to any one of claims 60 to 62, characterized in that: Its components are expressed in weight percentage, wherein: (Al2O3+Na2O) / P2O5 is 6.0-10.
0.
67. The glass-ceramics according to any one of claims 60 to 62, characterized in that: Its components are expressed in weight percentage, wherein SiO2 / Al2O3 is 1.2 to 2.
8.
68. The glass-ceramics according to any one of claims 60 to 62, characterized in that: Its components are expressed in weight percentage, wherein SiO2 / Al2O3 is 1.3 to 2.
5.
69. The glass-ceramics according to any one of claims 60 to 62, characterized in that: Its components are expressed in weight percentage, wherein SiO2 / Al2O3 is 1.5 to 2.
2.
70. The glass-ceramics according to any one of claims 60 to 62, characterized in that: Its components are expressed in weight percentage, wherein SiO2 / Al2O3 is 1.6 to 2.
0.
71. The glass-ceramics according to any one of claims 60 to 62, characterized in that: Its components are expressed in weight percentage, wherein SiO2 / (Na2O+B2O3) is 2.0-15.
0.
72. The glass-ceramics according to any one of claims 60 to 62, characterized in that: Its components are expressed in weight percentage, wherein SiO2 / (Na2O+B2O3) is 3.0-10.
0.
73. The glass-ceramics according to any one of claims 60 to 62, characterized in that: Its components are expressed in weight percentage, wherein SiO2 / (Na2O+B2O3) is 4.0 to 8.
0.
74. The glass-ceramics according to any one of claims 60 to 62, characterized in that: Its components are expressed in weight percentage, wherein SiO2 / (Na2O+B2O3) is 5.0-7.
0.
75. The glass-ceramics according to any one of claims 60 to 62, characterized in that: Its components are expressed in weight percentage, wherein: (Na2O+Li2O) / SiO2 is 0.1 to 0.
8.
76. The glass-ceramics according to any one of claims 60 to 62, characterized in that: Its components are expressed in weight percentage, wherein: (Na2O+Li2O) / SiO2 is 0.15-0.
7.
77. The glass-ceramics according to any one of claims 60 to 62, characterized in that: Its components are expressed in weight percentage, wherein: (Na2O+Li2O) / SiO2 is 0.2-0.
6.
78. The glass-ceramics according to any one of claims 60 to 62, characterized in that: Its components are expressed in weight percentage, wherein: (Na2O+Li2O) / SiO2 is 0.25-0.
5.
79. The glass-ceramics according to any one of claims 60 to 62, characterized in that: Its components are expressed in weight percentage, wherein: (ZrO2+ZnO) / Na2O is less than 2.
0.
80. The glass-ceramics according to any one of claims 60 to 62, characterized in that: Its components are expressed in weight percentage, wherein: (ZrO2+ZnO) / Na2O is less than 1.
5.
81. The glass-ceramics according to any one of claims 60 to 62, characterized in that: Its components are expressed in weight percentage, wherein: (ZrO2+ZnO) / Na2O is 0.01-1.
0.
82. The glass-ceramics according to any one of claims 60 to 62, characterized in that: Its components are expressed in weight percentage, wherein: (ZrO2+ZnO) / Na2O is 0.1-0.
5.
83. The glass-ceramics according to any one of claims 60 to 62, characterized in that: Its components are expressed in weight percentage, wherein: (P2O5+Na2O) / Li2O is 0.8-2.
5.
84. The glass-ceramics according to any one of claims 60 to 62, characterized in that: Its components are expressed in weight percentage, wherein: (P2O5+Na2O) / Li2O is 1.0 to 2.
5.
85. The glass-ceramics according to any one of claims 60 to 62, characterized in that: Its components are expressed in weight percentage, wherein: (P2O5+Na2O) / Li2O is 1.5 to 2.
5.
86. The glass-ceramics according to any one of claims 60 to 62, characterized in that: Its components are expressed in weight percentage, wherein K2O / ZrO2 is greater than 0.
1.
87. The glass-ceramics according to any one of claims 60 to 62, characterized in that: The components are expressed in weight percentage, wherein K2O / ZrO2 is 0.2-10.
0.
88. The glass-ceramics according to any one of claims 60 to 62, characterized in that: The components are expressed in weight percentage, wherein K2O / ZrO2 is 0.3-5.
0.
89. The glass-ceramics according to any one of claims 60 to 62, characterized in that: Its components are expressed in weight percentage, wherein K2O / ZrO2 is 0.4-1.
5.
90. The glass-ceramics according to any one of claims 60 to 62, characterized in that: Its components are expressed in weight percentage, wherein: (ZnO+RO+B2O3+TiO2) / P2O5 is less than 1.0, and the RO is one or more of MgO, CaO, SrO, and BaO.
91. The glass-ceramics according to any one of claims 60 to 62, characterized in that: Its components are expressed in weight percentage, wherein: (ZnO+RO+B2O3+TiO2) / P2O5 is less than 0.5, and the RO is one or more of MgO, CaO, SrO, and BaO.
92. The glass-ceramics according to any one of claims 60 to 62, characterized in that: Its components are expressed in weight percentage, wherein: (ZnO+RO+B2O3+TiO2) / P2O5 is less than 0.2, and the RO is one or more of MgO, CaO, SrO, and BaO.
93. The glass-ceramics according to any one of claims 60 to 62, characterized in that: Its components are expressed in weight percentage, wherein: SiO2: 43-55%; and / or Al2O3: 23-36%; and / or Li2O: 3-13%; and / or Na2O: 5-15%; and / or P2O5+ZrO2: 2-12%; and / or K2O: 0-5%; and / or ZnO: 0-3%; and / or B2O3: 0-3%; and / or RO: 0-5%; and / or TiO2: 0-3%; and / or Ln2O3: 0-3%; and / or clarifier: 0-1%, wherein RO is one or more of MgO, CaO, SrO and BaO, and Ln2O3 is one or more of La2O3, Gd2O3 and Y2O3.
94. The glass-ceramics according to any one of claims 60 to 62, characterized in that: Its components are expressed in weight percentage, wherein: SiO2: 46-53%; and / or Al2O3: 25.5-32%; and / or Li2O: 5.5-11%; and / or Na2O: 6.5-12%; and / or P2O5+ZrO2: 4-10%; and / or K2O: 0.1-3%; and / or ZnO: 0-1%; and / or B2O3: 0-1%; and / or RO: 0-2%; and / or TiO2: 0-1%; and / or Ln2O3: 0-1%; and / or clarifier: 0-0.5%, wherein RO is one or more of MgO, CaO, SrO and BaO, and Ln2O3 is one or more of La2O3, Gd2O3 and Y2O3.
95. The glass-ceramics according to any one of claims 60 to 62, characterized in that: The components are expressed by weight percentage, wherein: ZrO2: 0-6%; and / or P2O5: 0-10%.
96. The glass-ceramics according to any one of claims 60 to 62, characterized in that: The components are expressed by weight percentage, wherein: ZrO2: 0-5%; and / or P2O5: 1-8%.
97. The glass-ceramics according to any one of claims 60 to 62, characterized in that: The components are expressed by weight percentage, wherein: ZrO2: 0.1-3%; and / or P2O5: 2-6%.
98. The glass-ceramics according to claim 60 or 61, characterized in that: Its components, expressed in weight percentage, also contain: Yb2O3+Nb2O5+WO3+Bi2O3+Ta2O5+TeO2+GeO2: 0-5%.
99. The glass-ceramics according to claim 60 or 61, characterized in that: Its components, expressed in weight percentage, also contain: Yb2O3+Nb2O5+WO3+Bi2O3+Ta2O5+TeO2+GeO2: 0-2%.
100. The glass-ceramic according to claim 60 or 61, characterized in that: Its components, expressed in weight percentage, also include: Yb2O3+Nb2O5+WO3+Bi2O3+Ta2O5+TeO2+GeO2: 0~1%.
101. The glass-ceramics according to any one of claims 60 to 62, characterized in that: The microcrystalline glass contains nepheline crystal phase; and / or lithium silicate crystal phase; and / or lithium phosphate crystal phase; and / or petalite crystal phase; and / or quartz crystal phase.
102. The glass-ceramics according to any one of claims 60 to 62, characterized in that: The main crystal phase of the microcrystalline glass is the nepheline crystal phase, or the microcrystalline glass only contains the nepheline crystal phase.
103. The glass-ceramics according to any one of claims 60 to 62, characterized in that: In the microcrystalline glass, the weight percentage of the nepheline crystal phase in the microcrystalline glass is 10 to 80%.
104. The glass-ceramics according to any one of claims 60 to 62, characterized in that: In the microcrystalline glass, the weight percentage of the nepheline crystal phase in the microcrystalline glass is 20 to 70%.
105. The glass-ceramics according to any one of claims 60 to 62, characterized in that: In the microcrystalline glass, the weight percentage of the nepheline crystal phase in the microcrystalline glass is 30-60%.
106. The glass-ceramics according to any one of claims 60 to 62, characterized in that: The crystal size of the microcrystalline glass is less than 80nm; and / or the Vickers hardness is 650kgf / mm 2 above.
107. The glass-ceramics according to any one of claims 60 to 62, characterized in that: The crystal size of the microcrystalline glass is less than 60nm; and / or the Vickers hardness is 680kgf / mm 2 above.
108. The glass-ceramics according to any one of claims 60 to 62, characterized in that: The crystal size of the microcrystalline glass is less than 50nm; and / or the Vickers hardness is 700kgf / mm 2 above.
109. The glass-ceramics according to any one of claims 60 to 62, characterized in that: The crystal grain size of the microcrystalline glass is less than 40 nm.
110. The glass-ceramics according to any one of claims 60 to 62, characterized in that: The microcrystalline glass with a thickness of less than 1mm has a body ball drop height of more than 1000mm; and / or a haze of less than 0.15%; and / or a light transmittance of 550nm wavelength of more than 88%; and / or an average light |B| value of 400-800nm is less than 1.
5.
111. The glass-ceramics according to any one of claims 60 to 62, characterized in that: The microcrystalline glass with a thickness of less than 1mm has a body ball drop height of more than 1200mm; and / or a haze of less than 0.12%; and / or a light transmittance of 550nm wavelength of more than 89%; and / or an average light |B| value of 400-800nm is less than 1.
0.
112. The glass-ceramics according to any one of claims 60 to 62, characterized in that: The microcrystalline glass with a thickness of less than 1mm has a body ball drop height of more than 1400mm; and / or a haze of less than 0.10%; and / or a light transmittance of 550nm wavelength of more than 90%; and / or an average light |B| value of 400-800nm is less than 0.
8.
113. The glass-ceramics according to any one of claims 60 to 62, characterized in that: The transmittance of glass-ceramics with a thickness of less than 1 mm at a wavelength of 550 nm is over 91%.
114. The glass-ceramic according to claim 110, characterized in that: The thickness of the microcrystalline glass is 0.2-1 mm.
115. The glass-ceramic according to claim 110, characterized in that: The thickness of the microcrystalline glass is 0.3-0.9 mm.
116. The glass-ceramic according to claim 110, characterized in that: The thickness of the microcrystalline glass is 0.5-0.8 mm.
117. The glass-ceramic according to claim 110, characterized in that: The thickness of the microcrystalline glass is 0.55 mm, 0.6 mm, 0.68 mm, 0.7 mm or 0.75 mm.
118. The glass-ceramic according to claim 60 or 61, characterized in that: Its components, expressed in weight percentage, also contain: NiO: 0-4%; and / or Ni2O3: 0-4%; and / or CoO: 0-2%; and / or Co2O3: 0-2%; and / or Fe2O3: 0-7%; and / or MnO2: 0-4%; and / or Er2O3: 0-8%; and / or Nd2O3: 0-8%; and / or Cu2O: 0-4%; and / or Pr2O3: 0-8%; and / or CeO2: 0-4%.
119. Matrix glass, characterized in that Its components, expressed in weight percentage, include: SiO2: 40-60%; Al2O3: 20-40%; Li2O: 2-15%; Na2O: 3-20%; P2O5+ZrO2: 1-15%, (ZnO+RO+B2O3+TiO2) / P2O5 is less than 1.5, (P2O5+Na2O) / Li2O is 0.5-2.5, and the RO is one or more of MgO, CaO, SrO, and BaO.
120. The matrix glass according to claim 119, characterized in that Its components, expressed in weight percentage, also contain: K2O: 0-8%; and / or ZnO: 0-6%; and / or B2O3: 0-6%; and / or RO: 0-8%; and / or TiO2: 0-5%; and / or Ln2O3: 0-5%; and / or clarifier: 0-2%, wherein RO is one or more of MgO, CaO, SrO, and BaO, and Ln2O3 is one or more of La2O3, Gd2O3, and Y2O3.
121. The matrix glass according to claim 119 or 120, characterized in that Its components are expressed in weight percentage, wherein: (Al2O3+Na2O) / P2O5 is 3.0-30.0; and / or SiO2 / Al2O3 is 1.2-2.8; and / or SiO2 / (Na2O+B2O3) is 2.0-15.0; and / or (Na2O+Li2O) / SiO2 is 0.1-0.8; and / or (ZrO2+ZnO) / Na2O is less than 2.0; and / or K2O / ZrO2 is more than 0.1; and / or (ZnO+RO+B2O3+TiO2) / P2O5 is less than 1.0, wherein RO is one or more of MgO, CaO, SrO, and BaO.
122. The matrix glass according to claim 119 or 120, characterized in that Its components are expressed in weight percentage, wherein: (Al2O3+Na2O) / P2O5 is 4.0-20.0; and / or SiO2 / Al2O3 is 1.3-2.5; and / or SiO2 / (Na2O+B2O3) is 3.0-10.0; and / or (Na2O+Li2O) / SiO2 is 0.15-0.7; and / or (ZrO2+ZnO) / Na2O is less than 1.5; and / or (P2O5+Na2O) / Li2O is 0.8-2.5; and / or K2O / ZrO2 is 0.2-10.0; and / or (ZnO+RO+B2O3+TiO2) / P2O5 is less than 0.5, wherein RO is one or more of MgO, CaO, SrO, and BaO.
123. The matrix glass according to claim 119 or 120, characterized in that Its components are expressed in weight percentage, wherein: (Al2O3+Na2O) / P2O5 is 5.0-15.0; and / or SiO2 / Al2O3 is 1.5-2.2; and / or SiO2 / (Na2O+B2O3) is 4.0-8.0; and / or (Na2O+Li2O) / SiO2 is 0.2-0.6; and / or (ZrO2+ZnO) / Na2O is 0.01-1.0; and / or (P2O5+Na2O) / Li2O is 1.0-2.5; and / or K2O / ZrO2 is 0.3-5.0; and / or (ZnO+RO+B2O3+TiO2) / P2O5 is less than 0.2, and the RO is one or more of MgO, CaO, SrO, and BaO.
124. The matrix glass according to claim 119 or 120, characterized in that Its components are expressed in weight percentage, wherein: (Al2O3+Na2O) / P2O5 is 6.0-10.0; and / or SiO2 / Al2O3 is 1.6-2.0; and / or SiO2 / (Na2O+B2O3) is 5.0-7.0; and / or (Na2O+Li2O) / SiO2 is 0.25-0.5; and / or (ZrO2+ZnO) / Na2O is 0.1-0.5; and / or (P2O5+Na2O) / Li2O is 1.5-2.5; and / or K2O / ZrO2 is 0.4-1.
5.
125. The matrix glass according to claim 119 or 120, characterized in that Its components are expressed in weight percentage, wherein: SiO2: 43-55%; and / or Al2O3: 23-36%; and / or Li2O: 3-13%; and / or Na2O: 5-15%; and / or P2O5+ZrO2: 2-12%; and / or K2O: 0-5%; and / or ZnO: 0-3%; and / or B2O3: 0-3%; and / or RO: 0-5%; and / or TiO2: 0-3%; and / or Ln2O3: 0-3%; and / or clarifier: 0-1%, wherein RO is one or more of MgO, CaO, SrO and BaO, and Ln2O3 is one or more of La2O3, Gd2O3 and Y2O3.
126. The matrix glass according to claim 119 or 120, characterized in that Its components are expressed in weight percentage, wherein: SiO2: 46-53%; and / or Al2O3: 25.5-32%; and / or Li2O: 5.5-11%; and / or Na2O: 6.5-12%; and / or P2O5+ZrO2: 4-10%; and / or K2O: 0.1-3%; and / or ZnO: 0-1%; and / or B2O3: 0-1%; and / or RO: 0-2%; and / or TiO2: 0-1%; and / or Ln2O3: 0-1%; and / or clarifier: 0-0.5%, wherein RO is one or more of MgO, CaO, SrO and BaO, and Ln2O3 is one or more of La2O3, Gd2O3 and Y2O3.
127. The matrix glass according to claim 119 or 120, characterized in that The components are expressed by weight percentage, wherein: ZrO2: 0-6%; and / or P2O5: 0-10%.
128. The matrix glass according to claim 119 or 120, characterized in that The components are expressed by weight percentage, wherein: ZrO2: 0-5%; and / or P2O5: 1-8%.
129. The matrix glass according to claim 119 or 120, characterized in that The components are expressed by weight percentage, wherein: ZrO2: 0.1-3%; and / or P2O5: 2-6%.
130. The matrix glass according to claim 119 or 120, characterized in that Its components, expressed in weight percentage, also contain: Yb2O3+Nb2O5+WO3+Bi2O3+Ta2O5+TeO2+GeO2: 0-5%.
131. The matrix glass according to claim 119 or 120, characterized in that Its components, expressed in weight percentage, also contain: Yb2O3+Nb2O5+WO3+Bi2O3+Ta2O5+TeO2+GeO2: 0-2%.
132. The matrix glass according to claim 119 or 120, characterized in that Its components, expressed in weight percentage, also include: Yb2O3+Nb2O5+WO3+Bi2O3+Ta2O5+TeO2+GeO2: 0~1%.
133. The matrix glass according to claim 119 or 120, characterized in that Its components, expressed in weight percentage, also contain: NiO: 0-4%; and / or Ni2O3: 0-4%; and / or CoO: 0-2%; and / or Co2O3: 0-2%; and / or Fe2O3: 0-7%; and / or MnO2: 0-4%; and / or Er2O3: 0-8%; and / or Nd2O3: 0-8%; and / or Cu2O: 0-4%; and / or Pr2O3: 0-8%; and / or CeO2: 0-4%.
134. A glass-ceramic formed body, characterized in that: Containing the glass-ceramics described in any one of claims 60 to 118.
135. A glass cover plate, characterized in that: A microcrystalline glass product containing any one of claims 1 to 59, and / or the microcrystalline glass according to any one of claims 60 to 118, and / or the matrix glass according to any one of claims 119 to 133, and / or the microcrystalline glass formed body according to claim 134.
136. A glass component, characterized in that: A microcrystalline glass product containing any one of claims 1 to 59, and / or the microcrystalline glass according to any one of claims 60 to 118, and / or the matrix glass according to any one of claims 119 to 133, and / or the microcrystalline glass formed body according to claim 134.
137. A display device, characterized in that A glass-ceramic product containing any one of claims 1 to 59, and / or the glass-ceramic product according to any one of claims 60 to 118, and / or the matrix glass according to any one of claims 119 to 133, and / or the glass-ceramic formed body according to claim 134, and / or the glass cover plate according to claim 135, and / or the glass component according to claim 136.
138. An electronic device, characterized in that A glass-ceramic product containing any one of claims 1 to 59, and / or the glass-ceramic product according to any one of claims 60 to 118, and / or the matrix glass according to any one of claims 119 to 133, and / or the glass-ceramic formed body according to claim 134, and / or the glass cover plate according to claim 135, and / or the glass component according to claim 136.
139. The method for manufacturing a glass-ceramic product according to any one of claims 1 to 59, characterized in that: The method comprises the following steps: forming a matrix glass, subjecting the matrix glass to a crystallization process to form a microcrystalline glass, and then subjecting the microcrystalline glass to a chemical strengthening process to form a microcrystalline glass product.
140. The method for manufacturing a glass-ceramic product according to claim 139, characterized in that: The crystallization process includes the following steps: heating to a specified crystallization treatment temperature, maintaining the temperature for a certain period of time after reaching the crystallization treatment temperature, and then cooling down. The crystallization treatment temperature is 580-750°C, and the maintenance time at the crystallization treatment temperature is 0-8 hours.
141. The method for manufacturing a glass-ceramic product according to claim 139, wherein: The crystallization process includes the following steps: heating to a specified crystallization treatment temperature, maintaining the temperature for a certain period of time after reaching the crystallization treatment temperature, and then cooling down. The crystallization treatment temperature is 600-700°C, and the maintenance time at the crystallization treatment temperature is 1-6 hours.
142. The method for manufacturing a glass-ceramic product according to claim 139, characterized in that: The crystallization process includes the following steps: performing a nucleation process at a first temperature, and then performing a crystal growth process at a second temperature higher than the nucleation process temperature.
143. The method for manufacturing a glass-ceramic product according to claim 142, characterized in that: The crystallization process comprises the following steps: the first temperature is 500-620° C., the second temperature is 620-750° C.; the holding time at the first temperature is 0-24 hours; and the holding time at the second temperature is 0-10 hours.
144. The method for manufacturing a glass-ceramic product according to claim 142, characterized in that: The crystallization process comprises the following steps: the first temperature is 500-620° C., the second temperature is 620-750° C.; the holding time at the first temperature is 2-15 hours; and the holding time at the second temperature is 0.5-6 hours.
145. The method for manufacturing a glass-ceramic product according to claim 139, characterized in that: The chemical strengthening process includes: immersing the microcrystalline glass in a salt bath of molten Na salt at a temperature of 350-470°C for 1-36 hours; and / or immersing the microcrystalline glass in a salt bath of molten K salt at a temperature of 360-450°C for 1-36 hours; and / or immersing the microcrystalline glass in a mixed salt bath of molten K salt and Na salt at a temperature of 360-450°C for 1-36 hours.
146. The method for manufacturing a glass-ceramic product according to claim 139, wherein: The chemical strengthening process includes: immersing the microcrystalline glass in a salt bath of molten Na salt at a temperature of 380 to 460°C for 2 to 10 hours; and / or immersing the microcrystalline glass in a salt bath of molten K salt at a temperature of 360 to 450°C for 1 to 10 hours; and / or immersing the microcrystalline glass in a mixed salt bath of molten K salt and Na salt at a temperature of 360 to 450°C for 2 to 24 hours.
147. The method for producing glass-ceramics according to any one of claims 60 to 118, characterized in that: The method comprises the following steps: forming a matrix glass, and then forming a microcrystalline glass through a crystallization process.
148. The method for manufacturing glass-ceramics according to claim 147, characterized in that: The crystallization process includes the following steps: heating to a specified crystallization treatment temperature, maintaining the temperature for a certain period of time after reaching the crystallization treatment temperature, and then cooling down. The crystallization treatment temperature is 580-750°C, and the maintenance time at the crystallization treatment temperature is 0-8 hours.
149. The method for manufacturing glass-ceramics according to claim 147, characterized in that: The crystallization process includes the following steps: heating to a specified crystallization treatment temperature, maintaining the temperature for a certain period of time after reaching the crystallization treatment temperature, and then cooling down. The crystallization treatment temperature is 600-700°C, and the maintenance time at the crystallization treatment temperature is 1-6 hours.
150. The method for manufacturing glass-ceramics according to claim 147, characterized in that: The crystallization process includes the following steps: performing a nucleation process at a first temperature, and then performing a crystal growth process at a second temperature higher than the nucleation process temperature.
151. The method for manufacturing glass-ceramics according to claim 150, characterized in that: The crystallization process comprises the following steps: the first temperature is 500-620° C., the second temperature is 620-750° C.; the holding time at the first temperature is 0-24 hours; and the holding time at the second temperature is 0-10 hours.
152. The method for manufacturing glass-ceramics according to claim 150, characterized in that: The crystallization process comprises the following steps: the first temperature is 500-620° C., the second temperature is 620-750° C.; the holding time at the first temperature is 2-15 hours; and the holding time at the second temperature is 0.5-6 hours.
153. The method for manufacturing a glass-ceramic molded body according to claim 134, characterized in that: The method comprises grinding or polishing the microcrystalline glass to form a microcrystalline glass formed body, or subjecting the matrix glass or the microcrystalline glass to a heat bending process or a pressing process at a certain temperature to form a microcrystalline glass formed body.
154. The method for manufacturing a glass-ceramic molded body according to claim 134, characterized in that: The method comprises the following steps: subjecting the matrix glass to a crystallization heat treatment process, including heating, heat preservation nucleation, heating, heat preservation crystallization, and cooling to room temperature to form pre-crystallized glass; and subjecting the pre-crystallized glass to thermal processing and molding to obtain a microcrystalline glass formed body.
155. The method for manufacturing a glass-ceramic molded body according to claim 134, characterized in that: The method comprises the following steps: 1) Heating and preheating: Place the matrix glass or pre-crystallized glass or microcrystalline glass in the mold. The mold passes through each heating station in the hot bending machine in turn and stays at each station for a certain period of time to keep warm. The temperature in the preheating zone is 400-800°C, the pressure is 0.01-0.05MPa, and the time is 40-200s; 2) Pressurized molding: After preheating, the mold is transferred to the molding station. The hot bending machine applies a certain pressure to the mold. The pressure range is 0.1-0.8Mpa. The molding station temperature range is 650-850℃, and the molding time range is 40-200s. 3) Maintaining pressure and cooling: The mold is transferred to the cooling station for cooling step by step. The cooling temperature range is 750-500°C, the pressure is 0.01-0.05Mpa, and the time is 40-200s.