A benzoxazine functionalized polyphenylene ether resin prepolymer, thermosetting resin and preparation method thereof
By redistributing commercial high molecular weight polyphenylene ether resin, a benzoxazine-functionalized polyphenylene ether resin prepolymer was synthesized, solving the problems of poor processing performance and insufficient heat resistance in the prior art. This met the requirements for use in high-frequency communication equipment and possessed excellent solvent resistance and thermal properties.
Patent Information
- Application Number
- CN202211203152.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-29
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-09-29
AI Technical Summary
Existing commercial high molecular weight polyphenylene ether resins suffer from poor processing performance, poor solvent resistance, and insufficient heat resistance in ultra-high frequency communication technology. Furthermore, existing modification methods are complex and costly, making it difficult to meet the requirements of high frequency communication equipment.
Low molecular weight polyphenylene ether resin was prepared by redistribution reaction of commercial high molecular weight polyphenylene ether resin, and then reacted with phenolic, amine and aldehyde compounds in a polar/nonpolar mixed solvent to synthesize mono-, di-, and end-capped benzoxazine-functionalized polyphenylene ether resin prepolymers. The reaction was carried out under a nitrogen atmosphere using a one-step or stepwise feeding method, and the benzoxazine-functionalized polyphenylene ether resin prepolymer was obtained after post-treatment.
The preparation process is simplified, the cost is reduced, the glass transition temperature and dielectric properties of polyphenylene ether resin are improved, meeting the requirements of high-frequency communication equipment, and it has excellent solvent resistance and thermal properties.
Smart Images

Figure FHA0000007057320000011 
Figure FHA0000007057320000012 
Figure FHA0000007057320000013
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a benzoxazine functionalized polyphenylene ether resin prepolymer, a thermosetting resin and a preparation method thereof. Background Art
[0002] With the application and promotion of ultra-high frequency communication technology, the research on ultra-high frequency low dielectric polymer resins has attracted widespread attention. As the world's fifth largest engineering plastic, polyphenylene ether resin has the advantages of low dielectric constant (k) and low dielectric loss (f), high tensile strength and bending strength, as well as small thermal expansion coefficient, low water absorption, and good dimensional stability. It has been used in the field of electronic communications. However, commercial high molecular weight polyphenylene ether resins have problems such as high melt viscosity, poor processing performance, poor solvent resistance, and poor heat resistance. They cannot fully meet the application needs of ultra-high frequency communication technology for low dielectric polymer resins. In addition, as a thermoplastic resin, polyphenylene ether resin must be thermally cured when used as a matrix resin for printed circuit boards.
[0003] Since the 1960s, the research focus of polyphenylene ether resin in the field of low dielectric has been to maintain low k and low f characteristics as much as possible, while improving its processability (reducing molecular weight), solvent resistance and heat resistance. The main modification methods include preparing low molecular weight polyphenylene ether resin (generally with a number average molecular weight below 4000) by monomer copolymerization and redistribution; introducing active groups on the terminal hydroxyl group, side methyl group and main chain of polyphenylene ether resin to prepare self-thermosetting polyphenylene ether resin or hyperbranched polyphenylene ether resin; forming binary and ternary composite resin systems with epoxy resin, cyanate resin, bismaleimide resin, polyolefin, etc.; and inorganic / organic composite with inorganic micro- and nanoparticles such as oligomeric silsesquioxane (POSS) and nano-silica. Benzoxazine is a type of nitrogen-containing oxygen heterocyclic structure intermediate synthesized by Mannich condensation reaction using phenolic, aldehyde and primary amine compounds as raw materials, and can be obtained by thermal ring-opening polymerization to obtain benzoxazine resin. Benzoxazine resin has the advantages of good thermal properties, strong adhesion, high mechanical strength, and low dielectric constant (3.4-3.6), which makes it have great development potential in high-frequency communications, aerospace, automotive industry and other fields.
[0004] In order to prepare an ultra-high frequency low dielectric thermosetting resin with excellent comprehensive performance of low dielectric, good solvent resistance and high heat resistance, the preparation of benzoxazine-modified polyphenylene ether resin is a new research method based on the respective advantages of polyphenylene ether and benzoxazine resin. In 2018, Chen et al. first introduced benzoxazine functional groups into polyphenylene ether resin (Polymers, 2018, 10 (4): 411-425). They used low molecular weight (number average molecular weight of 1600) polyphenylene ether derivative SA90, i.e. phenol-terminated oligo (2,6-dimethylphenylene oxide) as raw material, nucleophilically substituted with fluoronitrobenzene, and then catalytically hydrogenated to prepare amine-terminated SA90 (APPO). APPO is then used as an amine source, and polyformaldehyde, as well as phenol or bisphenol A, to prepare a telechelic benzoxazine functionalized polyphenylene ether prepolymer or a main chain benzoxazine functionalized polyphenylene ether prepolymer. Finally, through self-curing and epoxy resin curing, a thermosetting resin with a glass transition temperature (218-225°C) and low dielectric properties (k is 2.9, 1GHz) can be obtained. This performance is difficult to meet the use requirements of high-frequency, high-speed, and high-performance communication equipment. In addition, the preparation method has a complicated process and requires multiple chemical reactions such as nitration, amination, and benzoxazine functionalization. The steps are cumbersome and there are many side reactions, which also leads to purification after synthesis being a big problem. And the derivative (SA90) of the polyphenylene ether resin used is expensive. Summary of the invention
[0005] Resin Prepolymer The technical problem to be solved by the present invention is to address the deficiencies of the prior art, and to provide a benzoxazine functionalized polyphenylene ether resin prepolymer, a preparation method, and a thermosetting resin having both low dielectric and high heat resistance obtained by thermal curing.
[0006] In order to achieve the above purpose, the technical solutions adopted are as follows:
[0007] Provided is a benzoxazine functionalized polyphenylene ether resin prepolymer, which is a monofunctional benzoxazine, a difunctional benzoxazine or a terminal main chain benzoxazine functionalized polyphenylene ether resin prepolymer, and the structural formula is shown in formula (a), formula (b) or formula (c) respectively:
[0008]
[0009] Among them: R1- is
[0010] -R 2- for
[0011] -R 3- for
[0012] The n value is 15 to 30, and the m value is 1 to 5.
[0013] Provided is a method for preparing the above-mentioned benzoxazine functionalized polyphenylene ether resin prepolymer:
[0014] Adding reactants into a reaction container in a one-step or multi-step manner, wherein the reactants are a phenol source, an amine source and an aldehyde compound, reacting at 70-120° C. for 5-60 hours under a nitrogen atmosphere, and post-treating to obtain a benzoxazine functionalized polyphenylene ether resin prepolymer, wherein the one-step addition method is to add all the raw materials into the reaction container at the same time, and then add a polar / non-polar mixed solvent to dissolve and react; and the multi-step addition method is to first add an aldehyde compound and an amine compound into the reaction container, and then add a polar / non-polar mixed solvent, and then add a phenol source after sufficient stirring;
[0015] in:
[0016] The phenol source in the preparation of the monofunctional benzoxazine functionalized polyphenylene ether resin prepolymer (formula (a)) is a redistributed polyphenylene ether resin, and the amine source is aniline, furfurylamine, allylamine, or p-vinylaniline;
[0017] The phenol source in the preparation of the bifunctional benzoxazine functionalized polyphenylene ether resin prepolymer (formula (b)) is the redistributed polyphenylene ether resin, and the amine source is 4,4'-diaminodiphenylmethane and hexamethylenediamine;
[0018] In the preparation of the end-capped main chain benzoxazine functionalized polyphenylene ether resin prepolymer (Formula (c)), the phenol source is dihydric phenol and redistributed polyphenylene ether resin, the dihydric phenol is bisphenol A, bisphenol F, bisphenol S, dicyclopentadiene bisphenol A, 4,4'-dihydroxybiphenyl, 4,4'-dihydroxydiphenyl ether, and the amine source is 4,4'-diaminodiphenylmethane and hexamethylenediamine.
[0019] According to the above scheme, the redistributed polyphenylene ether resin is The value range of n is: 15 to 30.
[0020] According to the above scheme, the number average molecular weight of the redistributed polyphenylene ether resin is 2027-3827.
[0021] According to the above scheme, the aldehyde compound is formaldehyde, paraformaldehyde, etc.
[0022] According to the above scheme, the molar ratio of the phenolic hydroxyl group, amino group and aldehyde group of the reactants is 1::1:2.
[0023] According to the above scheme, in the preparation of the end-capped main chain benzoxazine functionalized polyphenylene ether resin prepolymer, the molar ratio of the dihydric phenol compound to the functional group of the phenolic hydroxyl group in the redistributed polyphenylene ether resin is 1:1.
[0024] According to the above scheme, the polar / non-polar mixed solvent is obtained by mixing a polar solvent and a non-polar solvent in a volume ratio of 1:5 to 5:1. The polar solvent is cyclohexanone, acetone, ethyl acetate, methanol, ether, N,N′-dimethylformamide, dioxane, chloroform, ethanol, tetrahydrofuran, etc., and the non-polar solvent is toluene, butanone, xylene, etc.
[0025] According to the above scheme, the post-treatment is as follows: after the reaction is completed, the reaction solution is poured into a methanol solution to obtain a precipitate, washed multiple times, and then the product is dissolved in a polar / non-polar mixed solvent, precipitated with methanol, and washed multiple times. The above process is repeated multiple times to purify the prepared sample, and finally dried and ground to obtain a light yellow benzoxazine functionalized polyphenylene ether resin prepolymer.
[0026] According to the above scheme, the redistributed polyphenylene ether resin is obtained by redistributing commercial high molecular weight polyphenylene ether.
[0027] According to the above scheme, the preparation method of the redistributed polyphenylene ether resin is as follows: commercial high molecular weight polyphenylene ether, bisphenol A, and peroxide are used as raw materials, dissolved in a polar / non-polar mixed solvent, reacted at 60-125° C. for 4-50 hours, and post-processed to obtain a low molecular weight polyphenylene ether resin after the redistribution reaction, namely, a redistributed polyphenylene ether resin, and the reaction formula is as follows:
[0028]
[0029] According to the above scheme, the peroxide includes benzoic acid peroxide, methyl ethyl ketone peroxide, tert-amyl peroctanoate, dibenzoyl peroxide, benzoyl peroxide, 3,3′,5,5′-tetramethylbiphenylquinone, tri-tert-butylphenoxy free radical, benzoyl peroxide, etc.
[0030] According to the above scheme, the number average molecular weight of the commercial high molecular weight polyphenylene ether resin is 12000-24000, and the n' value is 100-200.
[0031] Preferably, the mass of the peroxide and bisphenol A are 25-30% and 20-25% of the mass of the polyphenylene ether resin, respectively.
[0032] According to the above scheme, the polar / non-polar mixed solvent is obtained by mixing a polar solvent and a non-polar solvent in a volume ratio of 1:5 to 5:1, the polar solvent is cyclohexanone, acetone, ethyl acetate, methanol, ether, N,N′-dimethylformamide, dioxane, chloroform, ethanol, tetrahydrofuran, etc., and the non-polar solvent is toluene, butanone, xylene, etc.
[0033] According to the above scheme, the post-treatment process after the redistribution reaction is to pour the reaction solution into distilled water for precipitation, then dissolve the product in a polar / non-polar mixed solvent, and then precipitate with distilled water, and repeat the precipitation and dissolution process many times until the pH value of the solution is neutral.
[0034] The benzoxazine functionalized polyphenylene ether resin prepolymer is thermally cured to obtain the benzoxazine functionalized polyphenylene ether thermosetting resin.
[0035] A method for preparing the benzoxazine functionalized polyphenylene ether thermosetting resin is provided. The benzoxazine functionalized polyphenylene ether resin prepolymer is dissolved in an organic mixed solvent to prepare a prepolymer solution, and then a curing reaction is performed at 80 to 250° C. for 5 to 24 hours to obtain a thermosetting resin sheet.
[0036] According to the above scheme, the solid content of the prepolymer solution can be 5-50wt%.
[0037] The present invention starts from commercial high molecular weight polyphenylene ether resin, and by redistributing low-cost commercial high molecular weight polyphenylene ether resin, the polyphenylene ether resin can be depolymerized to obtain low molecular weight polyphenylene ether resin with good processability, and at the same time, a phenolic hydroxyl functional group with chemical activity is introduced. The present invention uses the redistributed polyphenylene ether resin obtained by redistributing high molecular weight polyphenylene ether resin as a raw material, and an amine source compound, an aldehyde compound and other phenolic compounds, and only needs one step reaction to synthesize various benzoxazine functionalized polyphenylene ether resin prepolymers with different chemical structures as needed. Further based on the flexible molecular design of benzoxazine, the redistributed low molecular weight polyphenylene ether resin is used as a phenol source, and by selecting amine compounds and phenolic compounds with different chemical structures, a monofunctional benzoxazine, a difunctional benzoxazine and a capped main chain benzoxazine functionalized polyphenylene ether resin prepolymer with different chemical structures can be synthesized according to application needs.
[0038] The benzoxazine functionalized polyphenylene ether resin prepolymer provided by the present invention can not only increase the glass transition temperature of the polyphenylene ether resin, but also maintain its excellent dielectric properties, thereby meeting the use requirements of high-frequency, high-speed, and high-performance communication equipment.
[0039] The present invention significantly improves the glass transition temperature of the benzoxazine functionalized polyphenylene ether resin obtained by introducing benzoxazine groups into the polyphenylene ether molecular structure and curing, which can reach 238-289°C, which is significantly better than the low molecular weight polyphenylene ether resin of the redistribution reaction (the glass transition temperature is only 122°C). This comes from the cross-linking reaction that occurs when the introduced benzoxazine groups are cured and opened. Moreover, in addition to the ring-opening cross-linking of the oxazine ring, the chemical cross-linking or chemical grafting reaction of the introduced double bonds or furan ring structures can also further increase the cross-linking density of the cured resin. In addition, the heat-cured benzoxazine functionalized polyphenylene ether resin can also form abundant intramolecular and intermolecular hydrogen bonds, thereby making the benzoxazine functionalized polyphenylene ether resin have a higher glass transition temperature through chemical cross-linking bonds and hydrogen bonding.
[0040] Moreover, the benzoxazine functionalized polyphenylene ether resin of the present invention has excellent dielectric properties, which is due to the fact that both the benzoxazine resin and the polyphenylene ether resin have good dielectric properties. More importantly, the polymerization cross-linking reaction effectively increases the cross-linking density of the polyphenylene ether resin, thereby effectively suppressing the polarization orientation of the polymer network structure, thereby further improving the dielectric properties of the resin.
[0041] Beneficial effects of the present invention:
[0042] (1) The present invention is based on the redistributed polyphenylene ether resin, and only one step of chemical reaction is required to prepare the prepolymer of the benzoxazine functionalized polyphenylene ether resin, which is low in cost, simple in preparation method, and easy to industrialize. Moreover, the benzoxazine functionalized polyphenylene ether resin prepolymer prepared based on the low molecular weight redistributed polyphenylene ether also has good processability, and the thermosetting resin further obtained therefrom has excellent solvent resistance, thermal properties (glass transition temperature: 238-269°C) and high-frequency dielectric properties (k value: 2.0-2.8), and can be applied to aerospace, microelectronic device packaging and high-frequency communication industries.
[0043] (2) Based on the flexible molecular design of benzoxazine, the present invention uses redistributed low molecular weight polyphenylene ether resin as a phenol source. By selecting amine compounds and phenol compounds with different chemical structures, prepolymers of monofunctional benzoxazines, difunctional benzoxazines and polyphenylene ether resins with end-capped main chain benzoxazine functional groups with different chemical structures can be synthesized according to application needs.
[0044] (3) The benzoxazine functionalized polyphenylene ether thermosetting resin of the present invention has high solvent resistance, and its mass loss rate after immersion in organic solvents such as toluene, xylene, N,N'-dimethylformamide, N,N'-dimethylacetamide and tetrahydrofuran for 72 hours is less than 2%, while the mass loss rate of the low molecular weight polyphenylene ether resin prepared by the redistribution reaction after immersion in organic solvents such as toluene, N,N'-dimethylacetamide and tetrahydrofuran for 72 hours is greater than 2%. This is mainly because the modified resin has a cross-linked network structure and the cross-linking density has been greatly improved.
[0045] (4) Without the need for additional catalysts and harsh reaction conditions, low molecular weight benzoxazine functionalized polyphenylene ether prepolymers can be thermally ring-opened to prepare thermosetting resins. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 Infrared spectra (FTIR) of the redistributed low molecular weight polyphenylene ether resin and the products synthesized in Examples 1-3.
[0047] in:
[0048] Figure 1 a redistributed low molecular weight polyphenylene ether resin;
[0049] Figure 1 b Example 1, aniline / bisphenol A type benzoxazine functionalized polyphenylene ether resin prepolymer;
[0050] Figure 1 c Example 2, furfurylamine / bisphenol A type benzoxazine functionalized polyphenylene ether resin prepolymer;
[0051] Figure 1 d Example 3, 4,4′-diaminodiphenylmethane / bisphenol A type benzoxazine functionalized polyphenylene ether resin prepolymer. DETAILED DESCRIPTION
[0052] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0053] Redistributed low molecular weight polyphenylene ether resin (number average molecular weight 2027 g / mol)
[0054] 100 g of commercial high molecular weight polyphenylene ether resin (number average molecular weight of 12000 g / mol), 20 g of bisphenol A and 30 g of benzoic acid peroxide were mixed in a toluene / ethanol (5:1 v / v) solvent and reacted at 60°C for 50 h. After the reaction, the mixture was precipitated and washed with distilled water several times to obtain a low molecular weight polyphenylene ether resin (number average molecular weight of 2027 g / mol).
[0055] Example 1
[0056] 100 g of commercial high molecular weight polyphenylene ether resin (number average molecular weight of 12000 g / mol), 25 g of bisphenol A and 25 g of benzoic acid peroxide were mixed in a toluene / ethanol (5:1 v / v) solvent and reacted at 60°C for 50 h. After the reaction, the mixture was precipitated and washed with distilled water several times to obtain a low molecular weight polyphenylene ether resin (number average molecular weight of 2027 g / mol).
[0057] According to the molar ratio of phenolic hydroxyl, amino and aldehyde functional groups of 1:1:2, 0.025mol of the prepared low molecular weight polyphenylene ether resin, 0.025mol of aniline and 0.05mol of paraformaldehyde were added to a four-necked flask equipped with a condenser, magnetic stirring, thermometer and temperature sensor, and 70mL of toluene / ethanol (1:5v / v) mixed solvent was added, and the mixture was slowly heated to 70℃ for 60h. After the reaction, the reaction solution was poured into 200mL of methanol solution (concentration 99wt%) and allowed to stand for 24h to obtain a precipitate, which was washed several times. The precipitation and washing process was repeated several times. Finally, the obtained precipitate was vacuum dried at 60℃ for 12h, and the light yellow powder obtained by grinding the dried product was the prepolymer of aniline / bisphenol A type benzoxazine functionalized polyphenylene ether resin (chemical structure is shown below).
[0058]
[0059] Example 2
[0060] 100 g of commercial high molecular weight polyphenylene ether resin (number average molecular weight of 24000 g / mol), 25 g of bisphenol A and 30 g of benzoic acid peroxide were mixed in a butanone / N,N′-dimethylformamide (1:5 v / v) solvent and reacted at 125°C for 4 h. After the reaction, the mixture was precipitated and washed with distilled water several times to obtain a low molecular weight polyphenylene ether resin (number average molecular weight of 3827 g / mol).
[0061] According to the molar ratio of phenolic hydroxyl, amino and aldehyde functional groups of 1:1:2, 0.025mol of the prepared low molecular weight polyphenylene ether resin, 0.025mol of furfurylamine and 0.05mol of paraformaldehyde were added to a four-necked flask equipped with a condenser, magnetic stirring, thermometer and temperature sensor, and 70mL of toluene / N,N′-dimethylformamide (5:1v / v) mixed solvent was added, and the mixture was slowly heated to 105°C for 5h. After the reaction, the reaction solution was poured into 200mL of methanol solution (concentration 95wt%) and allowed to stand for 24h to obtain a precipitate, which was washed several times. The precipitation and washing process was repeated several times. Finally, the obtained precipitate was vacuum dried at 60°C for 12h, and the light yellow powder obtained by grinding the dried product was the furfurylamine / bisphenol A type benzoxazine functionalized polyphenylene ether resin prepolymer (chemical structure is shown below).
[0062]
[0063] Example 3
[0064] 100 g of commercial high molecular weight polyphenylene ether resin (number average molecular weight of 20000 g / mol), 20 g of bisphenol A and 25 g of 3,3′,5,5′-tetramethylbiphenyl diquinone were mixed in a butanone / dioxane (1:3 v / v) solvent and reacted at 100°C for 24 h. After the reaction, it was precipitated and washed with distilled water several times to obtain a low molecular weight polyphenylene ether resin (number average molecular weight of 2645 g / mol).
[0065] According to the molar ratio of phenolic hydroxyl, amino and aldehyde functional groups of 1:1:2, 0.025mol of the prepared low molecular weight polyphenylene ether resin, 0.0125mol of 4,4′-diaminodiphenylmethane and 0.05mol of polyformaldehyde were added to a four-necked flask equipped with a condenser, magnetic stirring, thermometer and temperature sensor, and 70mL of toluene / N,N′-dimethylformamide (1:1v / v) mixed solvent was added, and the mixture was slowly heated to 120°C for 25h. After the reaction, the reaction solution was poured into 200mL of methanol solution (concentration 90wt%) and allowed to stand for 24h to obtain a precipitate, which was washed several times. The precipitation and washing process was repeated several times. Finally, the obtained precipitate was vacuum dried at 60°C for 12h, and the light yellow powder obtained by grinding the dried product was 4,4′-diaminodiphenylmethane / bisphenol A type benzoxazine functionalized polyphenylene ether resin prepolymer (chemical structure shown below).
[0066]
[0067] Example 4
[0068] 100 g of commercial high molecular weight polyphenylene ether resin (number average molecular weight of 12000 g / mol), 20 g of bisphenol A and 30 g of benzoic acid peroxide were mixed in a toluene / ethanol (5:1 v / v) solvent and reacted at 60°C for 50 h. After the reaction, the mixture was precipitated and washed with distilled water several times to obtain a low molecular weight polyphenylene ether resin (number average molecular weight of 2027 g / mol).
[0069] According to the molar ratio of phenolic hydroxyl, amino and aldehyde functional groups being 1:1:2, and the molar ratio of phenolic hydroxyl functional groups in bisphenol A and redistributed polyphenylene ether resin being 1:1, 0.05 mol of the prepared low molecular weight polyphenylene ether resin, 0.025 mol of bisphenol A, 0.05 mol of 1,6-hexanediamine and 0.2 mol of paraformaldehyde were added into a 250 mL three-necked flask equipped with a condenser, a magnetic stirring device and a thermometer, and then 51 mL of a toluene / ethanol mixed solvent (1:2 v / v) was added. After mixing evenly, the mixture was heated to 90°C and reacted for 48 hours. After the reaction was completed, the reaction solution was poured into 100 mL of a methanol solution (concentration 40 wt%) to obtain a suspension, which was allowed to stand for 24 hours. The supernatant was removed to obtain a precipitate, and the precipitate was vacuum dried at 50°C for 8 hours. Finally, the dried product was ground to obtain a powder, which was a capped main chain benzoxazine functionalized polyphenylene ether resin prepolymer (chemical structure shown below).
[0070]
[0071] Where: R2 is R3 is
[0072] The molecular structural formulas of 1,6-hexanediamine, bisphenol A, and redistributed polyphenylene ether resin used in this embodiment are:
[0073]
[0074] The products synthesized in the comparative example and the example were characterized by infrared spectroscopy (FTIR). The infrared spectroscopy characterization results showed that the present invention successfully synthesized three prepolymers of benzoxazine functionalized polyphenylene ether resin based on the redistributed polyphenylene ether resin.
[0075] Wherein: the redistributed low molecular weight polyphenylene ether resin (number average molecular weight is 2027g / mol) and the product synthesized in the embodiment are shown in Figure 1 .in:
[0076] Figure 1 a: redistributed low molecular weight polyphenylene ether resin (number average molecular weight 2027 g / mol);
[0077] Figure 1 b: aniline / bisphenol A type benzoxazine functionalized polyphenylene ether resin prepolymer synthesized in Example 1;
[0078] Figure 1 c: the furfurylamine / bisphenol A type benzoxazine functionalized polyphenylene ether resin prepolymer of Example 2;
[0079] Figure 1 d: 4,4′-diaminodiphenylmethane / bisphenol A type benzoxazine functionalized polyphenylene ether prepolymer of Example 3).
[0080] like Figure 1 As shown in a, 3460cm-1 is the characteristic absorption peak of the stretching vibration of the hydroxyl group, 1306, 1189, 1020cm-1 are the characteristic absorption peaks of the vibration of phenyl ether, and 857cm-1 is the characteristic absorption peak of the CH bending vibration on the benzene ring. The infrared spectrum of the low molecular weight polyphenylene ether resin is basically consistent with the infrared spectrum of the high molecular weight polyphenylene ether resin, which shows that the redistribution reaction only changes the length of the molecular chain and does not change the chemical structure of the polyphenylene ether. It is worth noting that the prepolymers of the polyphenylene ether resins synthesized in the embodiments of the present invention all contain benzoxazine functional groups, and the characteristic absorption peaks of the oxazine rings are all located at 935cm -1 The COC of the benzoxazine structure (1229 cm -1 ) and CNC(1180cm -1 ) has a characteristic absorption peak of asymmetric stretching vibration at 1498 cm -1 The position corresponds to the characteristic absorption peak of CC stretching vibration in the plane of trisubstituted benzene ring. For the prepolymer of furfurylamine / bisphenol A type benzoxazine functionalized polyphenylene ether resin ( Figure 1 c) It is also possible to observe the -1 The above infrared spectrum results show that the prepolymer of benzoxazine functionalized polyphenylene ether resin is successfully synthesized based on the redistributed polyphenylene ether resin in the present invention.
[0081] Example 5
[0082] The aniline / bisphenol A type benzoxazine functionalized polyphenylene ether prepolymer prepared in Example 1 was dissolved in a toluene / ethanol (1:5 v / v) mixed solvent to prepare a prepolymer solution with a solid content of 25 wt%, and the prepolymer solution was placed in an oven for thermal curing at 80°C for 24 hours to obtain a benzoxazine functionalized polyphenylene ether thermosetting resin. The glass transition temperature of the prepolymer solution was 238°C, and the dielectric constant was 2.4 at 5 GHz.
[0083] Example 6
[0084] The furfurylamine / bisphenol A benzoxazine functionalized polyphenylene ether prepolymer prepared in Example 2 was dissolved in a mixed solvent of toluene / N,N′-dimethylformamide (5:1 v / v) to prepare a prepolymer solution with a solid content of 25 wt%, and the prepolymer solution was placed in an oven and thermally cured at 250° C. for 5 h to obtain a benzoxazine functionalized polyphenylene ether thermosetting resin. The glass transition temperature was 269° C. and the dielectric constant was 2.0 at 5 GHz.
[0085] Example 7
[0086] The 4,4′-diaminodiphenylmethane / bisphenol A benzoxazine functionalized polyphenylene ether prepolymer prepared in Example 3 was dissolved in a mixed solvent of toluene / N,N′-dimethylformamide (1:1 v / v) to prepare a prepolymer solution with a solid content of 25 wt%, and the prepolymer solution was placed in an oven and thermally cured at 160° C. for 12 h to obtain a benzoxazine functionalized polyphenylene ether thermosetting resin. The glass transition temperature was 247° C., and the dielectric constant was 2.7 at 5 GHz.
[0087] Example 8
[0088] The end-capped main chain benzoxazine functionalized polyphenylene ether prepolymer prepared in Example 4 was dissolved in a toluene / ethanol (1:1 v / v) mixed solvent to prepare a prepolymer solution with a solid content of 25 wt%, which was placed in an oven at 90°C for 24 hours and then cured at 240°C for 6 hours to obtain a benzoxazine functionalized polyphenylene ether thermosetting resin. The glass transition temperature was 289°C and the dielectric constant was 2.1 at 5 GHz.
Claims
1. A benzoxazine functionalized polyphenylene ether resin prepolymer, characterized in that: It is a monofunctional benzoxazine, a difunctional benzoxazine or a polyphenylene ether resin prepolymer with a terminal main chain benzoxazine functional group, and the structural formula is shown in formula (a), formula (b) or formula (c), respectively: Among them: R1- is CH2=CH-CH2-, -R2- is -R3- is -CH2-, -, -O-; The n value is 15 to 30, and the m value is 1 to 5.
2. The method for preparing the benzoxazine functionalized polyphenylene ether resin prepolymer according to claim 1, characterized in that: Adding reactants into a reaction container in a one-step or multi-step manner, wherein the reactants are a phenol source, an amine source and an aldehyde compound, reacting at 70-120° C. for 5-60 hours under a nitrogen atmosphere, and post-treating to obtain a benzoxazine functionalized polyphenylene ether resin prepolymer, wherein the one-step addition method is to add all the raw materials into the reaction container at the same time, and then add a polar / non-polar mixed solvent to dissolve and react; and the multi-step addition method is to first add an aldehyde compound and an amine compound into the reaction container, and then add a polar / non-polar mixed solvent, and then add a phenol source after sufficient stirring; in: The phenol source in the preparation of the monofunctional benzoxazine functionalized polyphenylene ether resin prepolymer (formula (a)) is a redistributed polyphenylene ether resin, and the amine source is aniline, furfurylamine, allylamine, or p-vinylaniline; The phenol source in the preparation of the bifunctional benzoxazine functionalized polyphenylene ether resin prepolymer (formula (b)) is the redistributed polyphenylene ether resin, and the amine source is 4,4'-diaminodiphenylmethane and hexamethylenediamine; In the preparation of the end-capped main chain benzoxazine functionalized polyphenylene ether resin prepolymer (Formula (c)), the phenol source is dihydric phenol and redistributed polyphenylene ether resin, the dihydric phenol is bisphenol A, bisphenol F, bisphenol S, dicyclopentadiene bisphenol A, 4,4'-dihydroxybiphenyl, 4,4'-dihydroxydiphenyl ether, and the amine source is 4,4'-diaminodiphenylmethane and hexamethylenediamine.
3. The method for preparing a benzoxazine functionalized polyphenylene ether resin prepolymer according to claim 2, characterized in that: The redistributed polyphenylene ether resin is The value of n is 15 to 30.
4. The method for preparing a benzoxazine functionalized polyphenylene ether resin prepolymer according to claim 2, characterized in that: The number average molecular weight of the redistributed polyphenylene ether resin is 2027-3827.
5. The method for preparing a benzoxazine functionalized polyphenylene ether resin prepolymer according to claim 2, characterized in that: The aldehyde compound is formaldehyde or polyformaldehyde; the molar ratio of the phenolic hydroxyl group, amino group and aldehyde group functional groups of the reactants is 1:1:2; the molar ratio of the dihydric phenol compound and the phenolic hydroxyl group functional group in the redistributed polyphenylene ether resin in the preparation of the end-capped main chain benzoxazine functionalized polyphenylene ether resin prepolymer is 1:
1.
6. The method for preparing a benzoxazine functionalized polyphenylene ether resin prepolymer according to claim 2, characterized in that: The polar / non-polar mixed solvent is obtained by mixing a polar solvent and a non-polar solvent in a volume ratio of 1:5 to 5:
1. The polar solvent is cyclohexanone, acetone, ethyl acetate, methanol, ether, N,N′-dimethylformamide, dioxane, chloroform, ethanol, tetrahydrofuran, and the non-polar solvent is toluene and xylene.
7. The method for preparing a benzoxazine functionalized polyphenylene ether resin prepolymer according to claim 2, characterized in that: The post-treatment is as follows: after the reaction is completed, the reaction solution is poured into a methanol solution to obtain a precipitate, washed multiple times, and then the product is dissolved in a polar / non-polar mixed solvent, precipitated with methanol, washed multiple times, and the above process is repeated multiple times to purify the prepared product, and finally dried and ground to obtain a light yellow benzoxazine functionalized polyphenylene ether resin prepolymer.
8. The method for preparing a benzoxazine functionalized polyphenylene ether resin prepolymer according to claim 2, characterized in that: The redistributed polyphenylene ether resin is obtained by redistributing commercial high molecular weight polyphenylene ether.
9. The method for preparing a benzoxazine functionalized polyphenylene ether resin prepolymer according to claim 8, characterized in that: The redistribution reaction is as follows: commercial high molecular weight polyphenylene ether, bisphenol A, peroxide or 3,3′,5,5′-tetramethylbiphenyl diquinone or tri-tert-butylphenoxy free radical are used as raw materials, dissolved in a polar / non-polar mixed solvent, reacted at 60 to 125° C. for 4 to 50 hours, and post-processed to obtain a low molecular weight polyphenylene ether resin after the redistribution reaction, namely, a redistributed polyphenylene ether resin. The reaction formula is as follows:
10. The method for preparing a benzoxazine functionalized polyphenylene ether resin prepolymer according to claim 9, characterized in that: The peroxides include benzoic acid peroxide, methyl ethyl ketone peroxide, tert-amyl peroctoate, dibenzoyl peroxide and benzoyl peroxide; the number average molecular weight of the commercial high molecular weight polyphenylene ether resin is 12000-24000, and the n' value is 100-200; the masses of the peroxide and bisphenol A are 25-30% and 20-25% of the mass of the polyphenylene ether resin respectively.
11. A benzoxazine functionalized polyphenylene ether thermosetting resin obtained by thermally curing the benzoxazine functionalized polyphenylene ether resin prepolymer according to claim 1.
12. The method for preparing the benzoxazine functionalized polyphenylene ether thermosetting resin according to claim 11, characterized in that: The benzoxazine functionalized polyphenylene ether resin prepolymer is dissolved in an organic mixed solvent to prepare a prepolymer solution, and then a curing reaction is carried out at 80 to 250° C. for 5 to 24 hours to obtain a heat-cured resin sheet.