Foam electromagnetic shielding material with bulletproof function and preparation method thereof
By using specific compositions and process processing in the preparation of electromagnetic shielding materials, the problems of complex and high cost in the existing technology are solved, and the combination of electromagnetic shielding and bulletproof performance is achieved, meeting the market demand for multifunctional materials.
Patent Information
- Application Number
- CN202210829325.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-15
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2042-07-15
AI Technical Summary
In the existing electromagnetic shielding material preparation process, the instrument and equipment are invested heavily, the production cost is high, the preparation process is complex, the foaming is uneven and the protective performance is lacking, making it difficult to meet the multifunctional needs of the market.
The mass ratio of matrix resin, azodiisobutyronitrile, modified absorber, 4,4-diaminodiphenylmethane, melamine and nanoconductive graphite powder is combined to prepare electromagnetic shielding mixing by mechanical stirring and ultrasonic dispersion technology. and heat treatment is carried out after hot pressing to form a foam electromagnetic shielding material with bulletproof function.
The gradient structural design of electromagnetic shielding performance and bulletproof performance is realized, the preparation process is simplified, the production cost is reduced, the material stability and pore density uniformity are improved, and the market demand for multifunctional electromagnetic shielding materials is adapted.
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of preparation of composite materials with electromagnetic protection function, and specifically relates to a foam electromagnetic shielding material with bulletproof function and a preparation method thereof. Background Art
[0002] With the continuous progress of science and technology, information technology has developed rapidly. The popularization of wireless communication systems and electronic equipment has greatly improved people's work efficiency and quality of life, making people show unprecedented dependence on electronic equipment in military, business and daily life. However, electronic equipment will continuously generate electromagnetic radiation during operation, which seriously affects human health; and high-frequency signal bands have extremely strong penetration, which is very easy to cause electromagnetic interference, and more seriously lead to various safety accidents, resulting in huge economic losses and casualties. For example, in the civilian field, strong interference sources will cause communication interruption, navigation failure and other failures of civil aircraft, posing a serious threat to the life safety of crew members and passengers; in the military field, electromagnetic interference will hinder the acquisition of intelligence and the transmission of instructions, especially the electromagnetic signals released by military facilities and equipment, which will expose their own targets in electromagnetic confrontation and be detected by the enemy, seriously threatening national defense security and battlefield situation. With the rapid development of modern military detection and guidance technology and the complexity of electromagnetic radiation situation, "discovery means destruction" has become a consensus among war experts in various countries, and the update and development of electromagnetic shielding materials has been increasingly valued by various countries.
[0003] The United States has been researching electromagnetic shielding materials since the 1950s. Its stealth fighter F-117A performed well in the Gulf War, forcing countries around the world to compete to start researching electromagnetic shielding materials. With the development of science and technology and the progress of the times, electromagnetic shielding materials have been widely used in stealth aircraft, stealth ships, satellites, communication base stations, electrical equipment and other fields. The essence of electromagnetic shielding materials to achieve electromagnetic shielding is energy conversion. It achieves loss by converting electromagnetic energy into other forms of energy. Electromagnetic shielding materials can be divided into coating type, patch type and structural type according to the application form. Structural electromagnetic shielding materials can have the dual functions of load bearing and wave absorption, and are an effective way to achieve the integration of stealth structures such as military facilities and weapons and equipment. Among them, foam electromagnetic shielding materials have excellent electromagnetic shielding effects, and also have many advantages such as strong designability, low density, high strength, good weather resistance, sound absorption, heat insulation, and shock absorption, which have attracted extensive attention and research at home and abroad. However, the current preparation technology for foam electromagnetic shielding materials still has a series of shortcomings such as complex process, high cost and uneven foam pore density. Moreover, it is very difficult to prepare electromagnetic shielding materials with long service life and excellent mechanical properties while ensuring excellent electromagnetic shielding effect, which seriously limits the large-scale application of foam electromagnetic shielding materials in practice.
[0004] Chinese patent CN 113248873 A discloses a low-density conductive absorbing epoxy resin foam material and a preparation method thereof. By combining physical foaming and chemical foaming, the problems of heat accumulation and excessive density are solved, while ensuring sufficient foaming; Chinese patent CN 113817210 A discloses a carbon nanocomposite absorbing and heat-insulating epoxy foam material and a preparation method thereof. By using carbon nanomaterials with high specific surface area and stacking graphene sheets and carbon nanotubes, the overall weight of the absorbing material is reduced; Chinese patent 113831131 A provides a carbon foam in-situ grown carbon nano-in-situ grown carbon nanotube composite electromagnetic shielding material. The carbon foam is obtained by carbonizing the melamine foam in a high-temperature tubular furnace, and then modified with a silicon dioxide layer, and carbon nanotubes are grown on the carbon foam skeleton. The obtained electromagnetic shielding material has the advantages of high growth density, good efficiency and good stability. It can be found that the existing process requires large investment in instruments and equipment, has high production costs, and has complex preparation conditions that are difficult to control, which has limited improvement in the electromagnetic shielding effect. Especially with the continuous changes in the battlefield environment, more electromagnetic shielding materials with protective functions are constantly receiving attention, and traditional electromagnetic shielding materials have gradually failed to meet the market's demand for multifunctionality.
[0005] Therefore, in view of the above defects and shortcomings, the present invention provides a foam electromagnetic shielding material with bulletproof function and a preparation method thereof. Summary of the invention
[0006] The purpose of the present invention is to solve the problems in the current preparation process of electromagnetic shielding materials, such as large investment in instruments and equipment, high production cost, complex preparation process, uneven foaming, and lack of protective performance.
[0007] The present invention is realized through the following technical solutions:
[0008] A foam electromagnetic shielding material with bulletproof function and a preparation method thereof, the specific steps are as follows:
[0009] Step 1, according to the mass ratio of base resin, azobisisobutyronitrile, modified absorber, 4,4-diaminodiphenylmethane, melamine and nano-conductive graphite powder of 60:2-5:7-10:2-3:1-2:1-2, respectively weigh the base resin, azobisisobutyronitrile, modified absorber, 4,4-diaminodiphenylmethane, melamine and nano-conductive graphite powder; and according to the mass volume ratio of base resin to dispersion solvent of 1g:50-70ml, measure the dispersion solvent;
[0010] The matrix resin is any one of polystyrene (PS), polypropylene (PP), epoxy resin (EP) or polymethacrylimide (PMI);
[0011] Furthermore, the average particle size distribution of the nano zinc oxide powder and nano silicon dioxide powder is 20 to 50 nm;
[0012] Furthermore, the preparation method of the modified absorber is as follows: the absorber matrix and the silane coupling agent are weighed respectively according to the mass ratio of the absorber matrix to the silane coupling agent of 20:1-2; and the anhydrous ethanol is measured according to the mass volume ratio of the absorber matrix to the anhydrous ethanol of 1g:30-50ml; then the absorber matrix and the silane coupling agent are added to the anhydrous ethanol, heated to 30-40°C, and mechanically stirred at a stirring speed of 200-300r / min, and a modified dispersion is obtained after 20-30min; the modified dispersion is filtered to obtain a modified absorber precursor, and the modified absorber precursor is placed in an oven at 80-100°C, and the modified absorber is obtained after 30-60min;
[0013] The absorber matrix is one or more of silicon carbide fiber, nano zinc oxide powder, nano silicon dioxide powder or polycrystalline iron fiber;
[0014] The average particle size distribution of the nano-conductive graphite powder is 30 to 70 nm;
[0015] The dispersing solvent is any one of anhydrous ethanol, tetrahydrofuran, methyl formate or ethyl acetate;
[0016] Step 2, dissolving the base resin weighed in step 1 into the dispersion solvent, and using mechanical stirring, the stirring speed is 200-300 r / min, 10N30min to obtain a mixed solution A; then transferring the mixed solution A to a 5-15°C environment, and adding the azobisisobutyronitrile and the modified absorber weighed in step 1 to the mixed solution A, continuing mechanical stirring, the stirring speed is 300-500 r / min, and continuously performing ultrasonic dispersion, the ultrasonic power is 500W, the frequency is 50kHz, 30N50min to obtain an absorbing resin dispersion;
[0017] Step 3: Maintain the temperature environment of step 2 and continuously introduce high-purity carbon dioxide (CO 2 ) gas flow rate of 30 to 50 ml / min; then add the 4,4-diaminodiphenylmethane, melamine and nano-conductive graphite powder weighed in step 1 to the absorbing resin dispersion obtained in step 2, use mechanical stirring at a stirring speed of 500 to 800 r / min, and obtain an electromagnetic shielding mixed solution after 90 to 120 minutes;
[0018] The purity of the high-purity carbon dioxide gas stream is ≥99.99%;
[0019] Step 4: Cut the aramid non-woven fabric into 48mm x 98mm cloth pieces, and apply modified ethylene-vinyl alcohol resin (EOVH) on the upward side of the cloth piece, and then quickly stack the coated aramid non-woven fabric pieces in 10 to 20 layers with the coated surface facing upward to obtain a bulletproof aramid chip, which is then placed in a 50mm x 100mm x 30mm hot pressing mold for standby use;
[0020] The preparation method of the modified ethylene-vinyl alcohol resin is as follows: ethylene-vinyl alcohol resin and flaky graphene are weighed respectively according to a mass ratio of ethylene-vinyl alcohol resin to flaky graphene of 30:1-2; and anhydrous ethanol is measured according to a mass volume ratio of ethylene-vinyl alcohol resin to anhydrous ethanol of 1g:30-50ml; then, the ethylene-vinyl alcohol resin and the flaky graphene are added to the anhydrous ethanol, mechanically stirred at a stirring speed of 100-300r / min, and ultrasonic dispersion is continuously performed at a power of 200W and a frequency of 50kHz, mechanical stirring is stopped after 20-40min, and ultrasonic dispersion is continued for 30-50min, so as to obtain the modified ethylene-vinyl alcohol resin;
[0021] Step 5. Pour the electromagnetic shielding mixed liquid obtained in step 3 into the mold containing the bulletproof aramid chip in step 4; then place the mold in a hot press at 70-90°C for hot pressing with a pressure of 6-8MPa, and obtain a foam electromagnetic shielding material precursor with bulletproof function after 5N8h; then place the foam electromagnetic shielding material precursor with bulletproof function in a tubular furnace at 300-400°C for heat treatment, and obtain a foam electromagnetic shielding material with bulletproof function after 50-90min.
[0022] The tubular furnace uses high-purity argon gas for atmosphere protection, and the purity of the high-purity argon gas is ≥99.99%.
[0023] Beneficial Effects
[0024] 1. A foam electromagnetic shielding material with bulletproof function and a preparation method thereof, which has a gradient structure design of electromagnetic shielding performance and bulletproof performance from the outside to the inside, so that the prepared composite material has both electromagnetic shielding performance and bulletproof performance, which meets the demand of domestic and foreign markets for the protective performance of electromagnetic shielding materials;
[0025] 2. A foam electromagnetic shielding material with bulletproof function and a preparation method thereof, which makes the pore density more uniform, the foaming more complete, and the dispersion of the absorbent more uniform by combining physical and chemical foaming methods; at the same time, the modified treatment of the absorbent makes the interface performance between the absorbent and the resin matrix better, and the stability of the prepared foam electromagnetic shielding material is significantly improved;
[0026] 3. A foam electromagnetic shielding material with bulletproof function and its preparation method. The raw materials for preparation are abundant, no complicated production instruments and equipment are required, and the production cost is low. At the same time, the operation process is simple, the steps are concise, and no three wastes are generated during the preparation process, which meets the requirements of green and environmentally friendly sustainable development. DETAILED DESCRIPTION
[0027] The following embodiments are further explanations of the present invention, which are partial embodiments of the present invention, but not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without any creative work belong to the scope of protection of the present invention.
[0028] Example 1
[0029] 10g of nano zinc oxide powder, 3g of nano silicon dioxide powder, 3g of polycrystalline iron fiber and 1.2g of silane coupling agent were added to 600ml of anhydrous ethanol, heated to 32°C, and mechanically stirred at a stirring speed of 260r / min to obtain a modified dispersion after 24min; the modified dispersion was filtered to obtain a modified absorbent precursor, and the modified absorbent precursor was placed in an oven at 80°C to obtain 16.8g of the modified absorbent after 35min;
[0030] 100g of polystyrene was dissolved in 5.5L of ethyl acetate solution, and mechanical stirring was used at a stirring speed of 240r / min, and a mixed solution A was obtained after 18min; then the mixed solution A was transferred to a 10°C environment, and 5g of azobisisobutyronitrile and 14g of modified absorbent were added to the mixed solution A, and mechanical stirring was continued at a stirring speed of 420r / min, and ultrasonic dispersion was continuously performed at an ultrasonic power of 500W and a frequency of 50kHz, and an absorbing resin dispersion was obtained after 40min; then a high-purity carbon dioxide gas flow was continuously introduced into the absorbing resin dispersion at a gas flow rate of 30ml / min; then 4g of 4,4-diaminodiphenylmethane, 2g of melamine and 2.5g of nano-conductive graphite powder were added to the absorbing resin dispersion, and mechanical stirring was used at a stirring speed of 720r / min, and an electromagnetic shielding mixed solution was obtained after 110min;
[0031] 300g of ethylene-vinyl alcohol resin and 15g of flake graphene were added to 10L of anhydrous ethanol, and mechanical stirring was used at a stirring speed of 160r / min. Ultrasonic dispersion was continuously performed at an ultrasonic power of 200W and a frequency of 50kHz. Mechanical stirring was stopped after 28min, and ultrasonic dispersion was continued for 34min to obtain modified ethylene-vinyl alcohol resin. Aramid non-woven fabric was cut into 48mmx98mm cloth pieces, and the modified ethylene-vinyl alcohol resin was applied on the upward side of the cloth piece, and then the coated aramid non-woven fabric pieces were quickly and regularly stacked with 14 layers with the coated surface facing upward to obtain a bulletproof aramid chip, which was then placed on a 50mmx100mm x30mm hot pressing mold; then pour the above electromagnetic shielding mixture to fill the mold containing the bulletproof aramid chip, and place the mold in a hot press at 80℃ for hot pressing with a pressure of 6.5MPa. After 6h, a foam electromagnetic shielding material precursor with bulletproof function is obtained; then the foam electromagnetic shielding material precursor with bulletproof function is placed in a tubular furnace at 360℃ for heat treatment. After 60min, a foam electromagnetic shielding material with bulletproof function is obtained.
[0032] Example 2
[0033] 8g of silicon carbide fiber, 6g of nano zinc oxide powder, 7g of nano silicon dioxide powder, 3g of polycrystalline iron fiber and 1.7g of silane coupling agent were added to 850ml of anhydrous ethanol, heated to 38°C, and mechanically stirred at a stirring speed of 280r / min to obtain a modified dispersion after 25min; the modified dispersion was filtered to obtain a modified absorbent precursor, and the modified absorbent precursor was placed in a 90°C oven to obtain 24.9g of the modified absorbent after 45min;
[0034] 150g of polymethacrylimide was dissolved in 9.5L of methyl formate solution, and mechanical stirring was used at a stirring speed of 260r / min, and a mixed solution A was obtained after 14min; then the mixed solution A was transferred to an 8°C environment, and 7.5g of azobisisobutyronitrile and 22g of modified absorber were added to the mixed solution A, and mechanical stirring was continued at a stirring speed of 350r / min, and ultrasonic dispersion was continuously performed at an ultrasonic power of 500W and a frequency of 50kHz, and an absorbing resin dispersion was obtained after 38min; then a high-purity carbon dioxide gas flow was continuously introduced into the absorbing resin dispersion at a gas flow rate of 45ml / min; then 6g of 4,4-diaminodiphenylmethane, 3.5g of melamine and 4g of nano-conductive graphite powder were added to the absorbing resin dispersion, and mechanical stirring was used at a stirring speed of 580r / min, and an electromagnetic shielding mixed solution was obtained after 100min;
[0035] 400 g of ethylene-vinyl alcohol resin and 22 g of flake graphene were added to 15 L of anhydrous ethanol, and mechanical stirring was used at a stirring speed of 120 r / min. Ultrasonic dispersion was continuously performed at an ultrasonic power of 200 W and a frequency of 50 kHz. Mechanical stirring was stopped after 35 minutes, and ultrasonic dispersion was continued for 45 minutes to obtain modified ethylene-vinyl alcohol resin. Aramid non-woven fabric was cut into 48 mm x 98 mm cloth pieces, and the modified ethylene-vinyl alcohol resin was applied on the upward side of the cloth piece, and then the coated aramid non-woven fabric pieces were quickly and regularly stacked with 12 layers with the coated surface facing upward to obtain a bulletproof aramid chip, which was then placed on a 50 mm x 100 mm x30mm hot pressing mold; then pour the above electromagnetic shielding mixture to fill the mold containing the bulletproof aramid chip, and place the mold in a 75℃ hot press for hot pressing with a pressure of 7.3MPa. After 7.5h, a foam electromagnetic shielding material precursor with bulletproof function is obtained; then the foam electromagnetic shielding material precursor with bulletproof function is placed in a 320℃ tubular furnace for heat treatment, and after 55min, a foam electromagnetic shielding material with bulletproof function is obtained.
[0036] Example 3
[0037] 10g of silicon carbide fiber, 16g of nano zinc oxide powder and 1.6g of silane coupling agent were added to 800ml of anhydrous ethanol, heated to 34°C, and mechanically stirred at a stirring speed of 250r / min to obtain a modified dispersion after 26min; the modified dispersion was filtered to obtain a modified absorber precursor, and the modified absorber precursor was placed in a 95°C oven to obtain 26.7g of the modified absorber after 40min;
[0038] 170g of polypropylene was dissolved in 10.5L of tetrahydrofuran solution, and mechanical stirring was used at a stirring speed of 220r / min, and a mixed solution A was obtained after 28min; then the mixed solution A was transferred to a 12°C environment, and 10g of azobisisobutyronitrile and 24g of modified absorber were added to the mixed solution A, and mechanical stirring was continued at a stirring speed of 380r / min, and ultrasonic dispersion was continuously performed at an ultrasonic power of 500W and a frequency of 50kHz, and an absorbing resin dispersion was obtained after 46min; then a high-purity carbon dioxide gas flow was continuously introduced into the absorbing resin dispersion at a gas flow rate of 42ml / min; then 6.4g of 4,4-diaminodiphenylmethane, 4.8g of melamine and 3.6g of nano-conductive graphite powder were added to the absorbing resin dispersion, and mechanical stirring was used at a stirring speed of 650r / min, and an electromagnetic shielding mixed solution was obtained after 95min;
[0039] 700g of ethylene-vinyl alcohol resin and 38g of flake graphene were added to 28L of anhydrous ethanol, and mechanical stirring was used at a stirring speed of 240r / min. Ultrasonic dispersion was continuously performed at an ultrasonic power of 200W and a frequency of 50kHz. Mechanical stirring was stopped after 24min, and ultrasonic dispersion was continued for 42min to obtain modified ethylene-vinyl alcohol resin. Aramid non-woven fabric was cut into 48mmx98mm cloth pieces, and the modified ethylene-vinyl alcohol resin was applied on the upward side of the cloth piece, and then the coated aramid non-woven fabric pieces were quickly and regularly stacked with 18 layers with the coated surface facing upward to obtain a bulletproof aramid chip, which was then placed on a 50mmx100mm x30mm hot pressing mold; then pour the above electromagnetic shielding mixture to fill the mold containing the bulletproof aramid chip, and place the mold in a hot press at 85℃ for hot pressing with a pressure of 6.4MPa. After 7h, a foam electromagnetic shielding material precursor with bulletproof function is obtained; then the foam electromagnetic shielding material precursor with bulletproof function is placed in a tubular furnace at 340℃ for heat treatment, and after 65min, a foam electromagnetic shielding material with bulletproof function is obtained.
[0040] Example 4
[0041] 8 g of nano silicon dioxide powder, 10 g of polycrystalline iron fiber and 1.4 g of silane coupling agent were added to 680 ml of anhydrous ethanol, heated to 35° C., and mechanically stirred at a stirring speed of 240 r / min, and a modified dispersion was obtained after 23 minutes; the modified dispersion was filtered to obtain a modified absorbent precursor, and the modified absorbent precursor was placed in an oven at 85° C., and 18.8 g of the modified absorbent was obtained after 50 minutes;
[0042] 120g of epoxy resin was dissolved in 7L of anhydrous ethanol, and mechanical stirring was used at a stirring speed of 280r / min, and a mixed solution A was obtained after 25min; then the mixed solution A was transferred to a 7°C environment, and 8g of azobisisobutyronitrile and 16g of modified absorbent were added to the mixed solution A, and mechanical stirring was continued at a stirring speed of 460r / min, and ultrasonic dispersion was continuously performed at an ultrasonic power of 500W and a frequency of 50kHz, and an absorbing resin dispersion was obtained after 42min; then a high-purity carbon dioxide gas flow was continuously introduced into the absorbing resin dispersion at a gas flow rate of 38ml / min; then 4.5g of 4,4-diaminodiphenylmethane, 3.2g of melamine and 3.8g of nano-conductive graphite powder were added to the absorbing resin dispersion, and mechanical stirring was used at a stirring speed of 680r / min, and an electromagnetic shielding mixed solution was obtained after 120min;
[0043] 500g of ethylene-vinyl alcohol resin and 30g of flake graphene were added to 18L of anhydrous ethanol, and mechanical stirring was used at a stirring speed of 280r / min. Ultrasonic dispersion was continuously performed at an ultrasonic power of 200W and a frequency of 50kHz. Mechanical stirring was stopped after 36min, and ultrasonic dispersion was continued for 38min to obtain modified ethylene-vinyl alcohol resin. Aramid non-woven fabric was cut into 48mmx98mm cloth pieces, and the modified ethylene-vinyl alcohol resin was applied on the upward side of the cloth piece, and then the coated aramid non-woven fabric pieces were quickly and regularly stacked with 16 layers with the coated surface facing upward to obtain a bulletproof aramid chip, which was then placed on a 50mmx100mm x30mm hot pressing mold; then pour the above electromagnetic shielding mixture to fill the mold containing the bulletproof aramid chip, and place the mold in a 72℃ hot press for hot pressing with a pressure of 7.2MPa. After 5.5h, a foam electromagnetic shielding material precursor with bulletproof function is obtained; then the foam electromagnetic shielding material precursor with bulletproof function is placed in a 380℃ tubular furnace for heat treatment, and after 75min, a foam electromagnetic shielding material with bulletproof function is obtained.
[0044] Example 5
[0045] 6 g of silicon carbide fiber, 10 g of nano silicon dioxide powder, 14 g of polycrystalline iron fiber and 2.2 g of silane coupling agent were added to 1300 ml of anhydrous ethanol, heated to 40° C., and mechanically stirred at a stirring speed of 220 r / min, and a modified dispersion was obtained after 28 minutes; the modified dispersion was filtered to obtain a modified absorbent precursor, and the modified absorbent precursor was placed in an oven at 82° C., and 31.3 g of the modified absorbent was obtained after 55 minutes;
[0046] 180g of polymethacrylimide was dissolved in 11.5L of methyl formate solution, and mechanical stirring was used at a stirring speed of 270r / min, and a mixed solution A was obtained after 22min; then the mixed solution A was transferred to a 6°C environment, and 12g of azobisisobutyronitrile and 28g of modified absorber were added to the mixed solution A, and mechanical stirring was continued at a stirring speed of 440r / min, and ultrasonic dispersion was continuously performed at an ultrasonic power of 500W and a frequency of 50kHz, and an absorbing resin dispersion was obtained after 35min; then a high-purity carbon dioxide gas flow was continuously introduced into the absorbing resin dispersion at a gas flow rate of 40ml / min; then 8g of 4,4-diaminodiphenylmethane, 4.5g of melamine and 5.5g of nano-conductive graphite powder were added to the absorbing resin dispersion, and mechanical stirring was used at a stirring speed of 750r / min, and an electromagnetic shielding mixed solution was obtained after 90min;
[0047] 450g of ethylene-vinyl alcohol resin and 25g of flake graphene are added to 16L of anhydrous ethanol, and mechanical stirring is used at a stirring speed of 180r / min. At the same time, ultrasonic dispersion is continuously performed with an ultrasonic power of 200W and a frequency of 50kHz. Mechanical stirring is stopped after 25min, and ultrasonic dispersion is continued for 35min to obtain modified ethylene-vinyl alcohol resin; aramid non-woven fabric is cut into 48mmx98mm cloth pieces, and the modified ethylene-vinyl alcohol resin is applied on the upward side of the cloth piece, and then the coated aramid non-woven fabric pieces are quickly and regularly stacked with 15 layers with the coated surface facing upward to obtain a bulletproof aramid chip, which is then placed on a 50mmx100mm x30mm hot pressing mold; then pour the above electromagnetic shielding mixture to fill the mold containing the bulletproof aramid chip, and place the mold in a 84℃ hot press for hot pressing with a pressure of 6.6MPa. After 6.5h, a foam electromagnetic shielding material precursor with bulletproof function is obtained; then the foam electromagnetic shielding material precursor with bulletproof function is placed in a 350℃ tubular furnace for heat treatment. After 85min, a foam electromagnetic shielding material with bulletproof function is obtained.
[0048] Example 6
[0049] 23 g of polycrystalline iron fiber and 1.6 g of silane coupling agent were added to 900 ml of anhydrous ethanol, heated to 30° C., and mechanically stirred at a stirring speed of 300 r / min, and a modified dispersion was obtained after 27 minutes; the modified dispersion was filtered to obtain a modified absorbent precursor, and the modified absorbent precursor was placed in a 94° C. oven, and 24.1 g of the modified absorbent was obtained after 45 minutes;
[0050] 140g of polymethacrylimide was dissolved in 8L of methyl formate solution, and mechanical stirring was used at a stirring speed of 250r / min, and a mixed solution A was obtained after 16min; then the mixed solution A was transferred to a 9°C environment, and 7.5g of azobisisobutyronitrile and 21g of modified absorber were added to the mixed solution A, and mechanical stirring was continued at a stirring speed of 400r / min, and ultrasonic dispersion was continuously performed at an ultrasonic power of 500W and a frequency of 50kHz, and an absorbing resin dispersion was obtained after 45min; then a high-purity carbon dioxide gas flow was continuously introduced into the absorbing resin dispersion at a gas flow rate of 36ml / min; then 5.8g of 4,4-diaminodiphenylmethane, 3.4g of melamine and 4.3g of nano-conductive graphite powder were added to the absorbing resin dispersion, and mechanical stirring was used at a stirring speed of 660r / min, and an electromagnetic shielding mixed solution was obtained after 105min;
[0051] 550g of ethylene-vinyl alcohol resin and 32g of flake graphene were added to 22L of anhydrous ethanol, and mechanical stirring was used at a stirring speed of 250r / min. Ultrasonic dispersion was continuously performed at an ultrasonic power of 200W and a frequency of 50kHz. Mechanical stirring was stopped after 38min, and ultrasonic dispersion was continued for 40min to obtain modified ethylene-vinyl alcohol resin. Aramid non-woven fabric was cut into 48mmx98mm cloth pieces, and the modified ethylene-vinyl alcohol resin was applied on the upward side of the cloth piece, and then the coated aramid non-woven fabric pieces were quickly and regularly stacked with 17 layers with the coated surface facing upward to obtain a bulletproof aramid chip, which was then placed on a 50mmx100mm x30mm hot pressing mold; then pour the above electromagnetic shielding mixture to fill the mold containing the bulletproof aramid chip, and place the mold in a 78℃ hot press for hot pressing with a pressure of 7.8MPa. After 8h, a foam electromagnetic shielding material precursor with bulletproof function is obtained; then the foam electromagnetic shielding material precursor with bulletproof function is placed in a 300℃ tubular furnace for heat treatment. After 80min, a foam electromagnetic shielding material with bulletproof function is obtained.
[0052] Effect verification
[0053] The foam electromagnetic shielding materials with bulletproof function prepared in Example 1, Example 2, Example 3, Example 4, Example 5 and Example 6 were subjected to performance tests. The electromagnetic shielding performance test results showed that the electromagnetic shielding effect was excellent, the reflectivity at 2 to 18 GHz was better than -20 dB, and the reflectivity at 18 to 26.5 GHz was better than -30 dB; the ballistic performance test results showed that the ballistic performance was excellent, the concave value was less than 20 mm, and the bulletproof standard of the Ministry of Public Security was met.
Claims
1. A method for preparing a foam electromagnetic shielding material with bulletproof function, characterized in that: The specific steps are as follows: Step 1, according to the mass ratio of base resin, azobisisobutyronitrile, modified absorber, 4,4-diaminodiphenylmethane, melamine and nano-conductive graphite powder of 60:2~5:7~10:2~3:1~2:1~2, respectively weigh base resin, azobisisobutyronitrile, modified absorber, 4,4-diaminodiphenylmethane, melamine and nano-conductive graphite powder; and according to the mass volume ratio of base resin to dispersion solvent of 1 g:50~70 ml, measure the dispersion solvent; The matrix resin is any one of polystyrene (PS), polypropylene (PP), epoxy resin (EP) or polymethacrylimide (PMI); The preparation method of the modified absorber is as follows: weighing the absorber matrix and the silane coupling agent respectively according to the mass ratio of the absorber matrix to the silane coupling agent of 20:1-2; and measuring the anhydrous ethanol according to the mass volume ratio of the absorber matrix to the anhydrous ethanol of 1 g:30-50 ml; then adding the absorber matrix and the silane coupling agent into the anhydrous ethanol, heating to 30-40°C, and using mechanical stirring at a stirring speed of 200-300 r / min, and obtaining the modified dispersion after 20-30 minutes; The modified dispersion is filtered to obtain a modified absorbent precursor, and the modified absorbent precursor is placed in an oven at 80-100°C for 30-60 minutes to obtain the modified absorbent; The absorber matrix is one or more of silicon carbide fiber, nano zinc oxide powder, nano silicon dioxide powder or polycrystalline iron fiber; The average particle size distribution of the nano-conductive graphite powder is 30-70 nm; Step 2: dissolving the base resin weighed in step 1 into the dispersion solvent, and using mechanical stirring at a stirring speed of 200-300 r / min, and obtaining a mixed solution A after 10-30 min; then transferring the mixed solution A to a 5-15 °C environment, and adding the azobisisobutyronitrile and the modified absorber weighed in step 1 to the mixed solution A, continuing mechanical stirring at a stirring speed of 300-500 r / min, and continuously performing ultrasonic dispersion at an ultrasonic power of 500 W and a frequency of 50 kHz, and obtaining an absorbing resin dispersion after 30-50 min; Step 3: maintaining the temperature environment of step 2, continuously introducing a high-purity carbon dioxide (CO2) gas flow into the absorbing resin dispersion obtained in step 2, with a gas flow rate of 30-50 ml / min; then adding the 4,4-diaminodiphenylmethane, melamine and nano-conductive graphite powder weighed in step 1 to the absorbing resin dispersion obtained in step 2, using mechanical stirring at a stirring speed of 500-800 r / min, and obtaining an electromagnetic shielding mixed solution after 90-120 min; The purity of the high-purity carbon dioxide gas stream is ≥99.99%; Step 4: Cut the aramid non-woven fabric into 48 mm x 98 mm pieces, and apply modified ethylene-vinyl alcohol resin (EVOH) on the upward side of the piece, and then quickly stack the coated aramid non-woven fabric pieces in 10 to 20 layers with the coated surface facing upward to obtain a bulletproof aramid chip, which is then placed in a 50 mm x 100 mm x 30 mm hot pressing mold for standby use; The preparation method of the modified ethylene-vinyl alcohol resin is as follows: ethylene-vinyl alcohol resin and flaky graphene are weighed respectively according to a mass ratio of ethylene-vinyl alcohol resin to flaky graphene of 30:1-2; and anhydrous ethanol is measured according to a mass volume ratio of ethylene-vinyl alcohol resin to anhydrous ethanol of 1 g:30-50 ml; then, the ethylene-vinyl alcohol resin and the flaky graphene are added to the anhydrous ethanol, mechanically stirred at a stirring speed of 100-300 r / min, and ultrasonic dispersion is continuously performed at a power of 200 W and a frequency of 50 kHz, mechanical stirring is stopped after 20-40 minutes, and ultrasonic dispersion is continued for 30-50 minutes, so as to obtain the modified ethylene-vinyl alcohol resin; Step 5, pouring the electromagnetic shielding mixed liquid obtained in step 3 into the mold containing the bulletproof aramid chip in step 4; then placing the mold in a 70-90 °C hot press for hot pressing, with a pressure of 6-8 MPa, and obtaining a foam electromagnetic shielding material precursor with a bulletproof function after 5-8 hours; then placing the foam electromagnetic shielding material precursor with a bulletproof function in a 300-400 °C tubular furnace for heat treatment, and obtaining a foam electromagnetic shielding material with a bulletproof function after 50-90 minutes; The tubular furnace uses high-purity argon gas for atmosphere protection, and the purity of the high-purity argon gas is ≥99.99%.
2. The method for preparing a foam electromagnetic shielding material with bulletproof function as claimed in claim 1, characterized in that: The dispersing solvent is any one of anhydrous ethanol, tetrahydrofuran, methyl formate or ethyl acetate.
3. The method for preparing a foam electromagnetic shielding material with bulletproof function as claimed in claim 1, characterized in that: The average particle size distribution of the nano zinc oxide powder and nano silicon dioxide powder is 20-50 nm.
Citation Information
Patent Citations
Low-density conductive wave-absorbing epoxy resin foam material and preparation method thereof
CN113248873A
Carbon nano composite wave-absorbing and heat-insulating epoxy foam material and preparation method thereof
CN113817210A
Carbon foam in-situ growth carbon nanotube composite electromagnetic shielding material and preparation method thereof
CN113831131A
A bulletproof composite material
CN205448840U
Soft armored clothing