A high-reliability cyanoresin wave-absorbing adhesive film with controllable fluidity and a preparation method thereof

By adding inorganic fillers and perforating the absorbing film, the problems of uncontrollable fluidity and poor air permeability of the absorbing film are solved, and the electromagnetic parameters of the absorbing laminate are stabilized and highly reliable.

CN115651601BActive Publication Date: 2024-10-29AEROSPACE INST OF ADVANCED MATERIALS & PROCESSING TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202211413681.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-11
Publication Date
2024-10-29
Estimated Expiration
2042-11-11

AI Technical Summary

Technical Problem

The fluidity of the absorbing film is uncontrollable during the molding process, resulting in changes in the electromagnetic parameters and reduced reliability of the absorbing laminate. The poor air permeability makes it difficult for internal air to be discharged, forming defects and reducing the reliability of the laminate.

Method used

Add inorganic fillers to the absorbing adhesive film to adjust its viscosity and fluidity, use a hole punch to punch ventilation holes, and combine it with a vacuum bag for exhaust to ensure that the adhesive film maintains good fluidity and breathability during the curing process. .

Benefits of technology

It effectively maintains the stability of the electromagnetic parameters of the absorbing film, prevents absorber migration, ensures the high reliability and excellent internal quality of the absorbing laminate, and avoids the occurrence of defects after curing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115651601B_ABST
    Figure CN115651601B_ABST
Patent Text Reader

Abstract

The present invention relates to a highly reliable cyano resin absorbing adhesive film with controllable fluidity and a preparation method thereof. The absorbing adhesive film is composed of a cyano resin matrix, an absorbent, and an inorganic filler. The main steps are as follows: a cyano resin system is prepared, the absorbent, the inorganic filler and the cyano resin system are roughly mixed by banburying, and after the rough mixing, an open mill is used for fine mixing, and after the mixing is uniform, a calender is used to calender the absorbing resin into a film. After the film is formed, a puncher is used to punch holes in an array on the absorbing adhesive film to improve the exhaust characteristics of the absorbing adhesive film. The cyano resin absorbing adhesive film prepared by the method has controllable curing fluidity, strong absorbing performance, and high reliability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of preparing absorbing materials, and in particular relates to a highly reliable cyano resin absorbing adhesive film with controllable fluidity and a preparation method thereof. Background Art

[0002] Absorbing materials refer to a type of material that can absorb and attenuate incident electromagnetic waves, and convert their electromagnetic energy into heat energy to dissipate or make the electromagnetic waves disappear due to interference. With the development of science and technology, absorbing materials have been widely used in various fields. For example, they are of great significance in electromagnetic protection, microwave darkroom, mobile communications, and military stealth. Due to the advantages of resin-based absorbing composite materials such as strong designability and large-area integral molding, they have become one of the most important application materials in the field of aerospace stealth.

[0003] Absorbent film is an intermediate material for preparing resin-based absorbing composite materials. It is mainly composed of electromagnetic wave absorbers and resin matrices. The absorbent film is formed by mixing the absorbent and the matrix resin and then calendering it into a film. It is then laminated with composite prepreg and cured to prepare a laminate material with both load-bearing and absorbing functions. Since absorbing laminates generally require a wider absorption frequency band, absorbing films with different electromagnetic parameters are required for matching laminations, so the fluidity of the absorbing film needs to be precisely controlled. Too high fluidity will lead to absorbent migration between different types of absorbing films, resulting in changes in electromagnetic parameters. Too low fluidity will cause the resin to be unable to fill the defects inside the laminate, resulting in reduced reliability of the absorbing laminate. At the same time, although the high-density absorbing film prepared by the calendering method has excellent electrical and mechanical properties, its air permeability is poor. It is difficult to effectively discharge the internal air during the molding process, and defects will form after curing, which will reduce the reliability of the laminate. Summary of the invention

[0004] In order to solve the problem of uncontrollable fluidity of absorbing film during the molding process and the problem of reduced reliability of absorbing layer due to exhaust difficulties, the present invention provides a high-reliability cyanoresin absorbing film with controllable fluidity and a preparation method thereof. Although related patents such as CN202010950674.3 and CN201910201141.2 mention the preparation method of absorbing film, the fluidity of the absorbing film prepared therefrom is uncontrollable. Too high fluidity of the absorbing film will lead to absorbent migration between different types of absorbing films, resulting in changes in electromagnetic parameters. Too low fluidity will result in the inability of the resin to fill the defects inside the ply, resulting in reduced reliability of the absorbing layer. At the same time, due to the dense internal structure of the absorbing film, its air permeability is poor, and it is difficult to effectively discharge the internal air during the molding process. Defects are formed after curing, which will reduce the reliability of the layer.

[0005] In order to solve the above problems of the absorbing film, this patent will add inorganic fillers to the absorbing film. The concentration of inorganic fillers can effectively adjust the viscosity of the absorbing film, so that the thickness and fluidity of the film can be controlled during the curing process. At the same time, the inorganic fillers are low dielectric constant materials, which can adjust the fluidity of the film without affecting its absorbing performance. At the same time, a puncher is used to prepare air holes in the absorbing film, and a vacuum bag can be used to vent it after laying, effectively improving the reliability of the absorbing layer after curing.

[0006] In order to achieve the above object, the present invention provides, in a first aspect, a highly reliable cyano resin absorbing adhesive film with controllable fluidity and a preparation method thereof, the method comprising the following steps:

[0007] (1) mixing a cyano resin matrix and a catalyst to compound a cyano resin system;

[0008] (2) placing the cyano resin system obtained in step (1), the absorbent, and the inorganic filler into a resin internal mixer for rough mixing, and then performing fine mixing using an open mixer after rough mixing to obtain an absorbing resin blank;

[0009] (3) placing the absorbing resin blank obtained in step (2) into a precision calender to calender an absorbing film, and obtaining an absorbing resin film after calendering;

[0010] (4) The absorbing resin film obtained in step (3) is punched with air holes by a puncher to complete the preparation of the absorbing resin film.

[0011] Preferably, in the step (1), the cyano resin matrix and the catalyst are mixed using a vertical kneader to compound the cyano resin system; the mixing temperature of the vertical kneader is 20-300°C, the mixing time is 10min-120min, and the stirring blade speed is 10-250r / min; the ratio of the catalyst to the cyano resin is 0.04-3:1.

[0012] Preferably, the banburying temperature of the rough mixing in step (2) is 20-300° C., the mixing time is 10 min-120 min, and the banburying rotor speed is 10-250 r / min.

[0013] Preferably, in step (2), an open mill is used for fine mixing, the open mill temperature is 20-300° C., the mixing time is 10-80 min, and the mixing roller speed is 2-17 m / min.

[0014] Preferably, in step (3), the calendering temperature is 20-300° C., the calendering thickness is 0.1-5 mm, the calendering pressure is 1-200 tons, and the calendering speed is 0.5-8 m / s.

[0015] Preferably, in step (4), the diameter of the air holes is 0.1 mm-2 mm, and the distance between the holes is between 0.5 mm and 15 mm.

[0016] Preferably, the mass fraction of each constituent substance in the wave-absorbing adhesive film is:

[0017] Absorbent: 5-85wt%; cyanoresin matrix: 10-45wt%; catalyst: 2-30wt%; inorganic filler: 1-40wt%.

[0018] Preferably, the cyano resin matrix is ​​at least one selected from the group consisting of biphenyl type phthalonitrile resin, isophenyl type phthalonitrile resin, and polyarylether type phthalonitrile resin.

[0019] Preferably, the catalyst is at least one selected from the group consisting of 1,3-bis(3-aminophenoxy)benzene, 1,4-bis(3-aminophenoxy)benzene, bis[4-(3-aminophenoxy)phenyl]sulfone, and bis[4-(4-aminophenoxy)phenyl]sulfone.

[0020] Preferably, the absorbent is at least one selected from the group consisting of carbonyl iron, sendust, ferrite, conductive carbon black, carbon fiber, graphene, carbon nanotubes, and silicon carbide.

[0021] Preferably, the inorganic filler is at least one selected from the group consisting of hollow glass microspheres, nano-silicon dioxide, montmorillonite, and nano-alumina.

[0022] In a second aspect, the present invention provides a highly reliable cyanoresin absorbing adhesive film with controllable fluidity, prepared by the method described in the first aspect of the present invention.

[0023] Compared with the existing wave-absorbing adhesive film with uncontrollable fluidity and low reliability, the present invention has at least the following beneficial effects:

[0024] (1) The absorbing film prepared by the present invention has no interlayer migration of absorbent during the curing process, the electromagnetic parameters of the absorbing film layer can be well maintained before and after curing, and the absorbing layer plate has good absorbing performance after curing.

[0025] (2) In the process of mixing the absorbing film, the vent holes can be used to fully exhaust the air. Meanwhile, during the curing process, the vent holes can be well filled with the absorbing resin. The internal quality of the absorbing layer is excellent and the reliability is high. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 .Microscopic photograph of the interlayer of the absorbing layer after curing in Example 1.

[0027] Figure 2 .Example 1 Ultrasonic scanning internal quality photos of the absorbing layer after curing.

[0028] Figure 3 Comparative Example 1: Ultrasonic scanning internal quality photo of the absorbing layer after curing. DETAILED DESCRIPTION

[0029] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] Example 1

[0031] In this embodiment, the method for preparing a high-reliability wave-absorbing adhesive film with controllable fluidity comprises the following steps:

[0032] (1) Using a vertical kneader, different types of cyano resin bases, catalysts, etc. are mixed to compound a cyano resin system. The mixing temperature of the vertical kneader is 250° C., the mixing time is 120 min, and the stirring blade speed is 200 r / min; the cyano resin base is a biphenyl type phthalonitrile resin and an isophthalonitrile type phthalonitrile resin. The catalyst is 1,3-bis(3-aminophenoxy)benzene.

[0033] (2) The cyano resin system obtained in step (1), the absorbent, and the inorganic solid filler are placed in a resin internal mixer for internal mixing and rough mixing. After rough mixing, fine mixing is performed using an open mixer to obtain an absorbing resin blank. In this step, the internal mixing temperature is 200°C, the mixing time is 100 min, and the internal mixing rotor speed is 150 r / min; in the step, the open mixing temperature is 200°C, the mixing time is 60 min, and the mixing roller speed is 15 m / min. The mass fraction of each substance is: absorbent: 30wt%; cyano resin matrix: 40wt%; catalyst: 15wt%; inorganic filler: 15wt%. The absorbent is carbonyl iron; and the inorganic filler is hollow glass microspheres.

[0034] (3) The absorbing resin blank obtained in step (2) is placed in a precision calender to calender an absorbing film to obtain an absorbing resin film. In this step, the calendering temperature is 200° C., the calendering thickness is 3 mm, the calendering pressure is 180 tons, and the calendering speed is 6 m / s.

[0035] (4) The microwave-absorbing film obtained in step (3) is punched with a puncher to form air holes, thereby completing the preparation of the microwave-absorbing film. In this step, the pinhole diameter is 2 mm and the pinhole spacing is 12 mm.

[0036] Example 2

[0037] In this embodiment, the method for preparing a high-reliability wave-absorbing adhesive film with controllable fluidity comprises the following steps:

[0038] (1) Using a vertical kneader, different types of cyano resin bases, catalysts, etc. are mixed to compound a cyano resin system. The mixing temperature of the vertical kneader is 200° C., the mixing time is 100 min, and the stirring blade speed is 200 r / min; the cyano resin base is a group consisting of a biphenyl type phthalonitrile resin, an isophthalonitrile type phthalonitrile resin, and a polyarylether type phthalonitrile resin. The catalyst is 1,3-bis(3-aminophenoxy)benzene.

[0039] (2) The cyano resin system obtained in step (1), the absorbent, and the inorganic solid filler are placed in a resin internal mixer for internal mixing and rough mixing. After rough mixing, fine mixing is performed using an open mixer to obtain an absorbing resin blank. In this step, the internal mixing temperature is 200°C, the mixing time is 100 min, and the internal mixing rotor speed is 100 r / min; in the step, the open mixing temperature is 200°C, the mixing time is 60 min, and the mixing roller speed is 15 m / min. The mass fraction of each substance is: absorbent: 20wt%; cyano resin matrix: 45wt%; catalyst: 25wt%; inorganic filler: 10wt%. The absorbent is carbonyl iron; and the inorganic filler is hollow glass microspheres.

[0040] (3) The absorbing resin blank obtained in step (2) is placed in a precision calender for calendering an absorbing film to obtain an absorbing resin film. In this step, the calendering temperature is 200° C., the calendering thickness is 3 mm, the calendering pressure is 100 tons, and the calendering speed is 5 m / s.

[0041] (4) The microwave-absorbing film obtained in step (3) is punched with a puncher to form air holes, thereby completing the preparation of the microwave-absorbing film. In this step, the pinhole diameter is 2 mm and the pinhole spacing is 10 mm.

[0042] Example 3

[0043] In this embodiment, the method for preparing a high-reliability wave-absorbing adhesive film with controllable fluidity comprises the following steps:

[0044] (1) A cyano resin matrix, a catalyst, etc. are mixed using a vertical kneader to compound a cyano resin system. The mixing temperature of the vertical kneader is 300° C., the mixing time is 120 min, and the stirring blade speed is 250 r / min; the cyano resin matrix is ​​a biphenyl type phthalonitrile resin. The catalyst is 1,4-bis(3-aminophenoxy)benzene.

[0045] (2) Put the cyano resin system obtained in step (1) and the absorbent and inorganic solid filler into a resin internal mixer for internal mixing, and then use an open mixer for fine mixing to obtain an absorbing resin blank. In this step, the internal mixing temperature is 300°C, the mixing time is 120min, and the internal mixing rotor speed is 250r / min; in the step, the open mixing temperature is 300°C, the mixing time is 80min, and the mixing roller speed is 17m / min. The mass fraction of each substance is: absorbent: 40wt%; cyano resin matrix: 45wt%; catalyst: 5wt%; inorganic filler: 10wt%. The absorbent is sendust; the inorganic filler is nano-silicon dioxide.

[0046] (3) The absorbing resin blank obtained in step (2) is placed in a precision calender for calendering an absorbing film to obtain an absorbing resin film. In this step, the calendering temperature is 300° C., the calendering thickness is 5 mm, the calendering pressure is 200 tons, and the calendering speed is 8 m / s.

[0047] (4) The microwave-absorbing film obtained in step (3) is punched with a puncher to form air holes, thereby completing the preparation of the microwave-absorbing film. In this step, the pinhole diameter is 2 mm and the pinhole spacing is 15 mm.

[0048] Example 4

[0049] In this embodiment, the method for preparing a high-reliability wave-absorbing adhesive film with controllable fluidity comprises the following steps:

[0050] (1) A cyano resin matrix, a catalyst, etc. are mixed using a vertical kneader to compound a cyano resin system. The mixing temperature of the vertical kneader is 20° C., the mixing time is 10 minmin, and the stirring blade speed is 10 r / min; the cyano resin matrix is ​​a polyarylether type phthalonitrile resin. The catalyst is bis[4-(3-aminophenoxy)phenyl]sulfone.

[0051] (2) The cyano resin system obtained in step (1), the absorbent, and the inorganic solid filler are placed in a resin internal mixer for internal mixing and rough mixing. After rough mixing, an open mixer is used for fine mixing to obtain an absorbing resin blank. In this step, the internal mixing temperature is 20°C, the mixing time is 10 minutes, and the internal mixing rotor speed is 10 r / min; in the step, the open mixing temperature is 20°C, the mixing time is 10 minutes, and the mixing roller speed is 2 m / min. The mass fractions of each substance are: absorbent: 5wt%; cyano resin matrix: 45wt%; catalyst: 30wt%; inorganic filler: 20wt%. The absorbent is conductive carbon black; and the inorganic filler is montmorillonite.

[0052] (3) The absorbing resin blank obtained in step (2) is placed in a precision calender to calender an absorbing film to obtain an absorbing resin film. In this step, the calendering temperature is 20° C., the calendering thickness is 0.1 mm, the calendering pressure is 1 ton, and the calendering speed is 0.5 m / s.

[0053] (4) The microwave-absorbing film obtained in step (3) is punched with a puncher to form air holes, thereby completing the preparation of the microwave-absorbing film. In this step, the pinhole diameter is 0.1 mm and the pinhole spacing is 0.5 mm.

[0054] Example 5

[0055] In this embodiment, the method for preparing a high-reliability wave-absorbing adhesive film with controllable fluidity comprises the following steps:

[0056] (1) Using a vertical kneader, different types of cyano resin bases, catalysts, etc. are mixed to compound a cyano resin system. The mixing temperature of the vertical kneader is 100° C., the mixing time is 60 min, and the stirring blade speed is 100 r / min; the cyano resin base is a biphenyl type phthalonitrile resin and an isophthalonitrile type phthalonitrile resin. The catalyst is bis[4-(4-aminophenoxy)phenyl]sulfone.

[0057] (2) Put the cyano resin system obtained in step (1) and the absorbent and inorganic solid filler into a resin internal mixer for internal mixing, and then use an open mixer for fine mixing to obtain an absorbing resin blank. In this step, the internal mixing temperature is 100°C, the mixing time is 80 minutes, and the internal mixing rotor speed is 100r / min; in the step, the open mixing temperature is 80°C, the mixing time is 50 minutes, and the mixing roller speed is 10m / min. The mass fraction of each substance is: absorbent: 30wt%; cyano resin matrix: 40wt%; catalyst: 10wt%; inorganic filler: 20wt%. The absorbent is carbon fiber; and the inorganic filler is nano-alumina.

[0058] (3) The absorbing resin blank obtained in step (2) is placed in a precision calender to calender an absorbing film to obtain an absorbing resin film. In this step, the calendering temperature is 200° C., the calendering thickness is 2 mm, the calendering pressure is 100 tons, and the calendering speed is 5 m / s.

[0059] (4) The microwave-absorbing film obtained in step (3) is punched with a puncher to form air holes, thereby completing the preparation of the microwave-absorbing film. In this step, the pinhole diameter is 1 mm and the pinhole spacing is 6 mm.

[0060] Comparative Example 1

[0061] This embodiment is consistent with the first three steps of embodiment 1, but does not include the fourth step, that is, no air holes are prepared.

[0062] The present invention provides a highly reliable cyano resin wave-absorbing adhesive film with controllable fluidity and a preparation method thereof. Figure 1 This is a microscope photograph of the interlayers of the absorbing layer after curing of Example 1. As shown in the figure, the interface between the absorbing adhesive film layers of the absorbing layer material prepared by the present invention is clear, and there is no absorbent migration between the layers, which means that the fluidity of the absorbing adhesive film is controllable during the curing process and the layer structure is well maintained. Figure 2 This is a nondestructive ultrasonic test diagram of Example 1 after preparing air holes and then curing. It can be seen from the figure that there are no obvious defects in the layer board and the material has high reliability. Figure 3 This is the non-destructive test result of the laminate after curing of the wave-absorbing film without air-permeable holes prepared in comparative example 1. It can be seen that the laminate has large-area internal defects. Due to poor exhaust performance, there is air holding inside the laminate, which reduces the reliability of the laminate.

[0063] The specific embodiments of the present invention disclosed above are intended to help understand the content of the present invention and implement it accordingly. It can be understood by those skilled in the art that various replacements, changes and modifications are possible without departing from the spirit and scope of the present invention. The present invention should not be limited to the contents disclosed in the embodiments of this specification, and the scope of protection of the present invention shall be subject to the scope defined in the claims.

Claims

1. A method for preparing a highly reliable cyanoresin absorbing film with controllable fluidity, characterized in that: The method comprises the following steps: The cyano resin matrix and the catalyst are mixed to compound the cyano resin system; the cyano resin matrix is ​​at least one selected from the group consisting of biphenyl type phthalonitrile resin, isophthalonitrile type phthalonitrile resin, and polyarylether type phthalonitrile resin; the cyano resin matrix and the catalyst are mixed using a vertical kneader, the mixing temperature of the vertical kneader is 250° C., the mixing time is 120 min, and the stirring blade speed is 200 r / min; The cyano resin system, the absorbent and the inorganic solid filler are placed in a resin internal mixer for internal mixing and rough mixing, and then fine mixing is performed using an open mixer to obtain an absorbing resin blank; the internal mixing temperature of the internal mixing rough mixing is 200° C., the mixing time is 100 min, and the internal mixing rotor speed is 150 r / min; the fine mixing using the open mixer has an open mixing temperature of 200° C., a mixing time of 60 min, and a mixing roller speed of 15 m / min; the inorganic solid filler is at least one selected from the group consisting of hollow glass microspheres, nano-silica, montmorillonite, and nano-alumina; The absorbing resin blank is placed in a precision calender to calender the absorbing film to obtain a cyano absorbing resin film; the calendering temperature is 200° C., the calendering thickness is 3 mm, the calendering pressure is 180 tons, and the calendering speed is 6 m / s; Punching air holes in the microwave-absorbing resin film through a puncher to complete the preparation of the microwave-absorbing film; The mass fractions of the constituent substances in the wave absorbing film are as follows: absorbent: 5-85wt%; cyanoresin matrix: 10-45wt%; catalyst: 2-30wt%; inorganic solid filler: 1-40wt%; The absorbent is at least one selected from the group consisting of carbonyl iron, sendust, ferrite, conductive carbon black, carbon fiber, graphene, carbon nanotubes, and silicon carbide.

2. The preparation method according to claim 1, characterized in that: The ratio of the catalyst to the cyano resin is 0.04-3:

1.

3. The preparation method according to claim 1, characterized in that: The diameter of the air holes is 0.1 mm to 2 mm, and the hole spacing is between 0.5 mm and 15 mm.

4. The preparation method according to any one of claims 1 to 3, characterized in that: The catalyst is at least one selected from the group consisting of 1,3-bis(3-aminophenoxy)benzene, 1,4-bis(3-aminophenoxy)benzene, bis[4-(3-aminophenoxy)phenyl]sulfone, and bis[4-(4-aminophenoxy)phenyl]sulfone.

5. A high-reliability cyanoresin absorbing adhesive film with controllable fluidity prepared according to the method of any one of claims 1 to 4.

Citation Information

Patent Citations

  • Wave-absorbing adhesive film and preparation method thereof

    CN111704868A

  • Wave-absorbing adhesive film material and preparation method thereof

    CN112029421A

  • Broadband wave-absorbing force-bearing composite material and preparation method thereof

    CN112644103A

  • High-temperature-resistant wave-absorbing plate and preparation method thereof

    CN114274623A

  • Electromagnetic wave absorbing paste including reactive inorganic composition and method of manufacturing for electromagnetic wave absorbing material using the same

    JP2001152026A