Interface plating flux for tin-steel bimetal casting
By using quaternary solutions of saturated zinc chloride, saturated ammonium chloride, saturated cerium chloride and saturated potassium fluoride as interface plating agents, the surface oxidation of steel matrix and the intact tin film in tin-steel bimetallic composites is solved. The problem of this problem is to achieve the continuity and density of metallurgy bonding of tin-steel, and improve the bonding strength and performance of the material.
Patent Information
- Application Number
- CN202211217446.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-04
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-10-04
AI Technical Summary
In the casting of existing tin-steel bimetallic composite materials, the problems of oxidation of the steel matrix surface and the incontinuous tin film of the tin film lead to uneven metallurgical bonding, affecting the material performance.
Using quaternary solutions of saturated zinc chloride, saturated ammonium chloride, saturated cerium chloride and saturated potassium fluoride as interface plating agents, a dense salt film is formed by uniform mixing and heat treatment to prevent oxidation of the steel matrix and improve the tin film. continuity and density.
Effectively prevent the surface of the steel matrix from oxidizing, forming a continuous and dense tin film, promoting tin-steel metallurgy bonding, and improving the bonding strength and performance of the material.
Smart Images

Figure CN115652239B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of bimetal casting, and relates to an interface plating aid for tin-steel bimetal casting, which is used for preventing surface oxidation of a steel substrate during high-temperature preheating. Background Art
[0002] Tin-steel bimetallic composite materials are compatible with the wear resistance, thermal conductivity, corrosion resistance and embedding properties of tin-based babbitt alloy, as well as the high strength and stiffness of steel. They have excellent comprehensive performance and are widely used in bearings, bushings, and sleeves of large-scale mechanical spindles, such as cement machinery, steel machinery, chemical machinery, papermaking machinery, petroleum machinery, ship machinery, compression machinery, coal mining machinery, mineral processing equipment, etc. They can also be used on large machine tools to replace brass, and also have very good results.
[0003] The key to the success of tin-steel bimetallic composite casting lies in whether it can form a metallurgical bond, produce a diffusion layer, and form an intermetallic compound. In this process, it is necessary not only to ensure the cleanliness of the steel substrate surface, but also to ensure that there is no oxidation on the steel substrate surface before bonding, and to increase the surface tension and activity of the steel substrate surface, so as to ensure that a uniform tin film is hung on the steel substrate surface, and rely on the diffusion of the steel substrate and the metal tin to form a transition layer to ensure the close metallurgical bonding of the tin-based babbitt alloy and the steel.
[0004] At present, most of the tinning treatment in the casting of tin-steel bimetallic composite materials uses a single fluoride, chloride or other salt compound saturated solution as a plating agent, and obtains a tin film by hot dipping (Improved steel / aluminum bonding in bimetallic castings by a compound casting process[J].Journal of Materials Processing Technology, 2015, 226: 25-31.). However, the salt film formed by these plating agents adheres to the surface of the steel substrate and cannot be completely detached when entering the tin bath, so that the obtained tin film is not dense, uneven, discontinuous, or even leaking plating occurs, so that the steel substrate cannot be completely protected, affecting the metallurgical bonding of the composite material. Summary of the invention
[0005] The purpose of the present invention is to provide an interface plating agent for tin-steel bimetal casting, which can form a continuous and dense tin film on a steel substrate during hot dipping in a tin bath, which can not only prevent surface oxidation of the steel substrate, but also allow pure tin to fully diffuse with the steel substrate to form a transition layer, thereby ensuring the metallurgical bonding of the bimetal.
[0006] To achieve the above object, the interface plating aid for tin-steel bimetallic casting of the present invention is prepared by mixing the following raw materials in percentage by volume:
[0007] Saturated zinc chloride solution 30-40%
[0008] Saturated ammonium chloride solution 5-10%
[0009] Saturated cerium chloride solution 2-5%
[0010] Saturated potassium fluoride solution 2-5%
[0011] Water replenishment 100%.
[0012] The interface plating aid of the present invention is prepared with saturated solutions of four salts as raw materials, and its purpose is to increase the anti-oxidation effect and plating effect of the interface plating aid. Therefore, in the process of preparing the interface plating aid, in order to prevent the precipitation of the quaternary system, it is necessary to gradually mix the saturated solutions of the volume percentage with water under continuous stirring to finally prepare the interface plating aid of the present invention.
[0013] The invention also provides a method for using the interface plating aid.
[0014] The interface plating aid prepared by the present invention is heated to 60-80° C., evenly applied on a steel substrate, placed in an oven at 250-280° C. to dry the moisture, and after repeated application and drying for 3-5 times, a dense interface plating aid salt film is attached to the surface of the steel substrate to protect the surface of the steel substrate from oxidation during preheating and increase the interfacial tension on the surface of the steel substrate, so that the steel substrate can achieve good metallurgical bonding with the tin liquid.
[0015] The present invention comprises mixing saturated zinc chloride solution, saturated ammonium chloride solution, saturated cerium chloride solution and saturated potassium fluoride solution to obtain ZnCl 2 -NH 4 Cl-CeCl 3-KF quaternary system, the melting point of this quaternary system in the solid state is just between the preheating temperature of the steel substrate 250-280℃ and the hot dipping temperature of the tin bath 300-350℃. Therefore, this quaternary system can first form a dense molten salt protective layer on the surface of the steel substrate to prevent oxidation of the steel substrate surface and improve its activity and wettability. In the process of hot dipping in the tin bath, the molten salt can be completely dissolved, float on the surface of the tin bath based on the density difference with the tin liquid and then evaporate, exposing the clean surface of the steel substrate, solving the shortcomings of a single salt plating agent that is partially insoluble in the tin bath and partially dissolved and floats on the surface of the tin bath, ensuring the effect of the hot-dip tinning film, and enabling the formation of a complete, continuous and dense tin film on the steel substrate, laying the foundation for the subsequent bimetallic metallurgical bonding.
[0016] Experiments have shown that the zinc chloride and ammonium chloride in the interface plating agent of the present invention can form a molten salt compound film on the surface of the steel substrate, which can protect the surface of the steel substrate and improve the solid-liquid wetting behavior of the steel substrate surface; and the addition of a small amount of potassium fluoride can increase the interfacial tension between the steel substrate and the tin liquid.
[0017] In particular, the viscosity or fluidity of the interface plating agent has an important influence on whether the interface plating agent in the tin bath can be smoothly removed from the surface of the steel substrate. If the viscosity is too high, the interface plating agent cannot be smoothly separated from the surface of the steel substrate, resulting in leakage of the tin film. The addition of a small amount of cerium chloride in the interface plating agent of the present invention can effectively reduce the viscosity of the interface plating agent, so that the interface plating agent on the surface of the steel substrate can be smoothly separated from the surface of the steel substrate in the tin bath, which helps to form a continuous and dense tin film on the surface of the steel substrate.
[0018] Furthermore, the present invention also provides a method for preparing a tin-steel bimetallic composite material based on the interface plating aid of the present invention.
[0019] The steel substrate with a dense interface plating aid salt film attached to the surface is placed in a 300-350°C tin bath, and taken out after hot dipping for 3-5 minutes, so that a uniform tin film is formed on the surface of the steel substrate; the steel substrate after the surface tinning treatment is placed in a mold, and a tin-based babbitt alloy melted to 450-500°C is poured on the steel substrate to prepare a tin-steel bimetallic composite material.
[0020] The interface plating aid of the invention is applied by brushing, is simple and convenient to use, has good adhesion effect on the surface of the steel substrate, provides conditions for subsequent bimetallic bonding, promotes the generation of tin-steel intermetallic compounds, improves the bonding strength of the tin-steel bimetallic interface, and achieves good metallurgical bonding. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a surface effect diagram of the steel substrate after tinning treatment in Example 1.
[0022] Figure 2 It is the bonding surface effect diagram and metallographic diagram of the tin-steel bimetallic composite material prepared in Example 1.
[0023] Figure 3 This is a surface effect diagram of the steel substrate after tinning treatment in Example 1.
[0024] Figure 4 These are the bonding surface effect diagram and metallographic diagram of the tin-steel bimetallic composite material prepared in Comparative Example 1.
[0025] Figure 5 This is a surface effect diagram of the steel substrate after tinning treatment in Example 2.
[0026] Figure 6 This is a metallographic image of the bonding surface of the tin-steel bimetallic composite material prepared in Comparative Example 2. DETAILED DESCRIPTION
[0027] The specific implementation of the present invention is further described in detail below in conjunction with the accompanying drawings and examples. The following examples are only used to more clearly illustrate the technical solution of the present invention so that those skilled in the art can well understand and utilize the present invention, rather than limiting the scope of protection of the present invention.
[0028] The production processes, experimental methods or detection methods involved in the embodiments of the present invention, unless otherwise specified, are all conventional methods in the prior art, and their names and / or abbreviations are all conventional names in the field, and are very clear and definite in the relevant application fields. Technical personnel in the field can understand the conventional process steps based on the names and apply the corresponding equipment, and implement them according to conventional conditions or the conditions recommended by the manufacturer.
[0029] The various instruments, equipment, raw materials or reagents used in the embodiments of the present invention are not particularly limited in terms of their sources, and are all conventional products that can be purchased through regular commercial channels, or can be prepared according to conventional methods well known to those skilled in the art.
[0030] The steel substrate used in the following embodiments and comparative examples of the present invention is 20# steel, and conventional treatment methods are adopted to remove oil and perform acid and alkali pretreatment on the surface of the steel substrate in advance.
[0031] Example 1.
[0032] 35 ml of saturated zinc chloride solution, 7 ml of saturated ammonium chloride solution, 3 ml of saturated cerium chloride solution, and 3 ml of saturated potassium fluoride solution were measured and mixed evenly, and then 52 ml of water was added, and the mixture was stirred and mixed evenly to prepare an interface plating agent for tin-steel bimetallic casting.
[0033] After the interface plating agent is heated to 70°C in a water bath, a high temperature resistant brush is used to dip the solution, evenly smear it on the steel substrate, and then placed in a 250°C oven to dry the moisture. It can be observed that a sparse salt film is attached to the surface of the steel substrate.
[0034] The above operation is repeated, and after three applications, a dense salt film is attached to the surface of the steel substrate.
[0035] The steel substrate with the interface plating agent salt film attached thereto is placed in a 300°C tin solution for tinning treatment, and is taken out after hot dipping for 3 minutes. Figure 1 As shown, it can be observed that a bright tin film is evenly coated on the outer surface of the steel substrate, and the tinning quality of the steel substrate after using the interface plating agent of the present invention is good.
[0036] A steel substrate with tin on its surface is placed in a mold, and a tin-based babbitt alloy with a melting temperature of 460° C. is poured on the outer surface of the steel substrate to prepare a tin-steel bimetallic composite material.
[0037] After the prepared composite material is machined, according to the obtained Figure 2 The cross-sectional view of the bonding surface shown in a and the metallographic image of the bonding joint shown in b show no obvious defects in the bimetallic bonding joint, achieving good metallurgical bonding.
[0038] According to the GB 12948-91 method, the interface shear strength test was carried out on the bimetallic joint of the composite material, and the results showed that the interface shear strength reached 55.35MPa.
[0039] Comparative example 1.
[0040] 35 ml of saturated zinc chloride solution, 7 ml of saturated ammonium chloride solution and 3 ml of saturated potassium fluoride solution were measured and mixed evenly, and then 55 ml of water was added, and the mixture was fully stirred to prepare an interface plating agent for tin-steel bimetallic casting.
[0041] After heating the interface plating agent to 70°C in a water bath, use a brush to dip the solution, apply it evenly on the steel substrate, and place it in a 250°C oven to dry the moisture. It can be observed that a sparse salt film is attached to the surface of the steel substrate.
[0042] The above operation is repeated, and after three applications, a dense salt film is attached to the surface of the steel substrate.
[0043] The steel substrate with the interface plating agent salt film attached is placed in a 300°C tin solution for tinning. After hot dipping for 3 minutes, it is observed that leakage plating occurs on the outer surface of the steel substrate. Figure 3 shown.
[0044] A steel substrate with tin on its surface is placed in a mold, and a tin-based babbitt alloy with a melting temperature of 460° C. is poured on the outer surface of the steel substrate to prepare a tin-steel bimetallic composite material.
[0045] After the prepared composite material is machined, according to the obtained Figure 4 From the cross-sectional view of the bonding surface shown in a and the metallographic image of the bonding joint shown in b, it can be clearly seen that there is a crack defect at the bonding joint.
[0046] According to the GB 12948-91 method, the interface shear strength test was carried out on the bimetallic bonding of the composite material. The results showed that the shear strength was very small, only 3.45MPa, and basically no bonding occurred.
[0047] Comparative example 2.
[0048] 35 ml of saturated zinc chloride solution, 7 ml of saturated ammonium chloride solution, 1 ml of saturated cerium chloride solution and 3 ml of saturated potassium fluoride solution were measured and mixed evenly, and then 54 ml of water was added, and the mixture was stirred and mixed evenly to prepare an interface plating agent for tin-steel bimetallic casting.
[0049] After heating the interface plating agent to 70°C in a water bath, use a brush to dip the solution, apply it evenly on the steel substrate, and place it in a 250°C oven to dry the moisture. It can be observed that a sparse salt film is attached to the surface of the steel substrate.
[0050] The above operation is repeated, and after three applications, a dense salt film is attached to the surface of the steel substrate.
[0051] The steel substrate with the interface plating agent salt film attached was placed in a 300°C tin solution for tinning. After hot dipping for 3 minutes, it was taken out and it was still found that the outer surface of the steel substrate had leakage plating, such as Figure 5 shown.
[0052] A steel substrate with tin on its surface is placed in a mold, and a tin-based babbitt alloy with a melting temperature of 460° C. is poured on the outer surface of the steel substrate to prepare a tin-steel bimetallic composite material.
[0053] The prepared composite material is machined to obtain the metallographic image of the joint. Figure 6 , it can be seen that there are obvious cracks at the joint.
[0054] According to the GB 12948-91 method, the interface shear strength test was carried out on the bimetallic joint of the composite material. The results showed that its shear strength was relatively low, only 23.45MPa.
[0055] It can be seen from the above two comparative examples that the lack of cerium chloride or insufficient cerium chloride content in the interface plating agent will have a direct impact on the tinning quality of the steel substrate surface, thereby significantly affecting the bonding strength of the bimetal.
[0056] Example 2.
[0057] 38 ml of saturated zinc chloride solution, 6 ml of saturated ammonium chloride solution, 4 ml of saturated cerium chloride solution, and 2 ml of saturated potassium fluoride solution were measured and mixed evenly, and then 50 ml of water was added, and the mixture was fully stirred to prepare an interface plating agent for tin-steel bimetallic casting.
[0058] After the interface plating agent is heated to 70°C in a water bath, the solution is dipped with a brush and evenly applied on the steel substrate, and then placed in an oven at 250°C to dry the moisture. It can be observed that a sparse salt layer is attached to the surface of the steel substrate.
[0059] The above operation is repeated, and after three applications, a dense salt layer is attached to the surface of the steel substrate.
[0060] The steel substrate with the interface plating agent attached thereto was placed in a 300°C tin solution, and after hot dipping for 3 minutes, it was taken out, and a layer of bright tin film was hung on the outer surface of the steel substrate.
[0061] A steel substrate with tin on its surface is placed in a mold, and a tin-based babbitt alloy with a melting temperature of 460° C. is poured on the outer surface of the steel substrate to prepare a tin-steel bimetallic composite material.
[0062] After the prepared composite material was machined, its bonding surface was visually inspected and observed under a metallographic microscope, and it can be seen that its bimetallic bonding surface is well bonded.
[0063] Then, the interface shear strength test was carried out on the bimetallic joint according to the GB 12948-91 method, and the results showed that the shear strength was 50.32MPa.
[0064] Example 3.
[0065] 32 ml of saturated zinc chloride solution, 10 ml of saturated ammonium chloride solution, 5 ml of saturated cerium chloride solution and 3 ml of saturated potassium fluoride solution were measured and mixed evenly, and then 50 ml of water was added, and the mixture was stirred thoroughly to prepare an interface plating agent for tin-steel bimetallic casting.
[0066] After the interface plating agent is heated to 80°C in a water bath, the solution is dipped with a brush and evenly applied to the steel substrate, and then placed in an oven at 280°C to dry the moisture. It can be observed that a sparse salt layer is attached to the surface of the steel substrate.
[0067] The above operation is repeated, and after five times of application, a dense salt layer is attached to the surface of the steel substrate.
[0068] The steel substrate with the interface plating agent attached thereto was placed in a 320°C tin solution and taken out after hot dipping for 3 minutes. A layer of bright tin film was hung on the outer surface of the steel substrate.
[0069] A steel substrate with tin on its surface is placed in a mold, and a tin-based babbitt alloy with a melting temperature of 480° C. is poured on the outer surface of the steel substrate to prepare a tin-steel bimetallic composite material.
[0070] After the prepared composite material was machined, its bonding surface was visually inspected and observed under a metallographic microscope, and it can be seen that its bimetallic bonding surface is well bonded.
[0071] Then, the interface shear strength test was carried out on the bimetallic joint according to the GB 12948-91 method, and the results showed that the shear strength was 52.34 MPa.
[0072] The above embodiments of the present invention do not describe all the details in detail, nor limit the present invention to the above embodiments. Various changes, modifications, substitutions and variations made by ordinary technicians in this field without departing from the principles and purpose of the present invention should be included in the protection scope of the present invention.
Claims
1. An interface plating agent for tin-steel bimetal casting is prepared by mixing the following raw materials in percentage by volume: Saturated zinc chloride solution 30-40% Saturated ammonium chloride solution 5-10% Saturated cerium chloride solution 2-5% Saturated potassium fluoride solution 2-5% Water replenishment 100%.
2. The method for preparing the interface plating aid according to claim 1 is to mix the saturated solutions of the volume percentages with water under continuous stirring to prepare the interface plating aid.
3. The method for using the interface plating aid according to claim 1 is to heat the interface plating aid to 60-80°C, evenly apply it on a steel substrate, place it in an oven at 250-280°C to dry out the moisture, repeat the application and drying 3-5 times, and a dense interface plating aid salt film is attached to the surface of the steel substrate.
4. A method for preparing a tin-steel bimetallic composite material based on the interface plating aid for tin-steel bimetallic casting according to claim 1, comprising: The interface plating agent is heated to 60-80° C., evenly applied on the steel substrate, placed in a 250-280° C. oven to dry out moisture, and after repeated application and drying 3-5 times, a dense interface plating agent salt film is attached to the surface of the steel substrate; The steel substrate with the dense interface plating agent salt film attached to the surface is placed in a 300-350° C. tin bath, and after hot dipping for 3-5 minutes, it is taken out to form a uniform tin film on the surface of the steel substrate; The steel substrate with the surface tinned is then placed in a mold, and the tin-based babbitt alloy melted to 450-500° C. is poured on the steel substrate to prepare a tin-steel bimetallic composite material.