Antibacterial and deodorizing functional fiber and preparation method thereof

Through layer-by-layer self-assembly of antibacterial agents and carboxylated β-cyclodextrin on cellulose fibers, the existing problems of poor solubility and deodorizing effect of antibacterial agents are solved, and non-dissolving antibacterial and deodorizing functions are achieved. fiber, significantly improving the safety and durability of sanitary products.

CN115652630BActive Publication Date: 2024-10-11CHINA NAT PULP & PAPER RES INST CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210785645.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-05
Publication Date
2024-10-11
Estimated Expiration
2042-07-05

AI Technical Summary

Technical Problem

Existing antibacterial agents have dissolution problems, which may cause potential harm to human health, and cannot effectively remove the odor in excrement. The effect of existing deodorization technology is not long-lasting.

Method used

Use chloroacetic acid to modify β-cyclodextrin, disperse the antibacterial agent into the cellulose fiber aqueous solution, load it on the cellulose fiber through hydrogen bonding, combine with carboxylated β-cyclodextrin, and self-assemble through layers The technology prepares antibacterial and deodorizing functional fibers to achieve non-dissolving antibacterial and deodorizing effects.

Benefits of technology

The prepared antibacterial and deodorizing functional fiber can effectively inhibit the reproduction and survival of microorganisms, remove odor molecules, and achieve controllable antibacterial and deodorizing performance through layer-by-layer assembly technology, avoiding the dissolution of antibacterial agents and improving the safety and durability of the material. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GSB0000208978290000061
    Figure GSB0000208978290000061
  • Figure GSB0000208978290000071
    Figure GSB0000208978290000071
  • Figure GSB0000208978290000072
    Figure GSB0000208978290000072
Patent Text Reader

Abstract

The present invention discloses an antibacterial and deodorizing functional fiber and a preparation method thereof. First, β-cyclodextrin is modified by chloroacetic acid, and then an antibacterial agent is dispersed into a cellulose fiber aqueous solution so that it is loaded on the cellulose fiber through hydrogen bonding. Finally, the antibacterial agent and carboxylated β-cyclodextrin are combined by layer-by-layer self-assembly technology, and an antibacterial and deodorizing functional fiber emulsion is obtained after centrifugation. The present application loads the antibacterial agent and carboxylated β-cyclodextrin on the cellulose fiber by layer-by-layer self-assembly technology to obtain a non-dissolving antibacterial and deodorizing functional fiber with good chemical stability, high antibacterial efficiency and significant deodorizing effect. The antibacterial and deodorizing functional fiber is used to post-treat a non-woven fabric material by dipping, spraying or surface coating, and the prepared non-woven fabric material has good liquid permeability and excellent antibacterial and deodorizing performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of functional fibers, and in particular to an antibacterial and deodorizing functional fiber and a preparation method thereof. Background Art

[0002] With the improvement of people's living standards and the enhancement of health awareness, environmental problems in today's society are becoming increasingly serious, making people pay more and more attention to their living environment and physical health. Additional properties such as skin care, safety, antibacterial and deodorization have become the focus of product value-added innovation. With the sudden outbreak of COVID-19, masks have become essential sanitary products for people to travel. However, wearing masks for a long time or reusing masks that have been worn can easily cause skin problems. This is because the masks cover the facial skin for a long time, and the exhaled gas of the human body will make the local microclimate moist, the temperature is correspondingly high, and the hydration degree is large, which creates a favorable environment for the survival and reproduction of bacteria and viruses. For excretory sanitary products such as diapers, sanitary napkins, and pet pads, when used, they come into contact with warm skin and excreta such as urine and menstrual blood. The environment is humid and the temperature is suitable, so it is particularly easy to breed a large number of bacteria, causing itching, diaper rash, skin ulcers, odor and other problems. In addition, sanitary products such as masks, excretory sanitary products, toilet paper, etc. that are discarded after use can also cause a large number of bacteria and viruses to multiply, and even lead to the spread of viruses. If textiles have antibacterial and deodorizing functions, they can not only block the spread of germs, but also eliminate the odors produced by microbial reproduction and excrement, thereby avoiding skin irritation.

[0003] Most of the antimicrobial agents used in China are organic antimicrobial agents such as biguanides, complex quaternary ammonium salts, isothiazolinones, chlorhexidine, etc., but organic antimicrobial agents will dissolve from the product, and dissolving antimicrobial agents have potential effects on the health of the body. First, although the dissolved antimicrobial agents can kill bacteria, they may enter the reproductive system or the surface of the skin, thereby destroying the originally stable flora environment; secondly, organic antimicrobial agents have certain toxicity. When used for a long time, a large amount of accumulated antimicrobial agents will have toxic side effects on the skin; finally, long-term use of dissolving antimicrobial materials will cause the enrichment of antimicrobial agents in the skin, which will cause the body to develop drug resistance, induce bacterial mutations, and cause harm to the body. Most of the antimicrobial agents used by developed countries, represented by Japan, are inorganic antimicrobial agents such as silver, zinc, copper, etc., which are all dissolvable antimicrobial agents. Inorganic antimicrobial agents often contain heavy metal ions, which are easily absorbed by the human body through contact with human skin, causing great harm to human health. The European Union has issued relevant laws to prohibit the use of silver-containing antimicrobial agents in sanitary products. Although natural antimicrobial agents were discovered earlier, they have problems such as easy decomposition, denaturation, easy dissolution under high temperature conditions, limited antimicrobial activity, and immature production technology, which limits their scope of application.

[0004] At present, domestic manufacturers are accustomed to confusing the "antibacterial" and "deodorizing" functions. However, antibacterial is not equal to deodorizing. The antibacterial function can only reduce the generation of odor by inhibiting the reproduction of bacteria, while the odor of excrement itself cannot be eliminated by antibacterial agents. Therefore, antibacterial products cannot remove odor. The deodorants used in the few sanitary products with deodorizing function are mostly fragrances, which can only cover up the odor and do not fundamentally remove the odor. Some deodorizing products use porous adsorption materials such as activated carbon and coconut shell charcoal for physical adsorption and removal, but the removal effect is limited and the deodorizing effect is not long-lasting. Summary of the invention

[0005] In order to overcome the defects of the prior art, the present invention first uses chloroacetic acid to modify β-cyclodextrin, then disperses the antibacterial agent into the cellulose fiber aqueous solution, so that it is loaded on the cellulose fiber through hydrogen bonding, and finally uses layer-by-layer self-assembly technology to combine the antibacterial agent and carboxylated β-cyclodextrin to prepare antibacterial and deodorizing functional fibers with excellent antibacterial properties, good deodorizing effects, and non-dissolving type. The prepared antibacterial and deodorizing functional fibers can be used to treat non-woven fabrics, paper-based materials, super absorbent resins and other sanitary products by dipping, spraying or surface coating, thereby giving sanitary products antibacterial and deodorizing functions. The technical scheme of the present invention is as follows:

[0006] A method for preparing antibacterial and deodorizing functional fibers, characterized by comprising the following steps:

[0007] (1) preparing sodium hydroxide into a 20-45 g / L aqueous solution, weighing a certain amount of β-cyclodextrin and adding it to an alkaline solution, wherein the mass ratio of β-cyclodextrin to sodium hydroxide is 2-0.5, stirring until β-cyclodextrin is completely dissolved, heating to 80-100° C., adding a certain amount of sodium chloroacetate, wherein the mass ratio of sodium chloroacetate to β-cyclodextrin is 2-0.5, reacting for 1-3 h, adjusting the pH to 5-6, washing with ethanol and deionized water, and drying to obtain a carboxylated β-cyclodextrin powder;

[0008] (2) Weigh a certain amount of cellulose fiber, mix it with deionized water to obtain a 0.05-0.2wt% cellulose fiber suspension, add an antibacterial agent to the suspension, wherein the antibacterial agent is at least one of chitosan quaternary ammonium salts, chitosan oligosaccharides, guanidines, and betaines, and the mass ratio of the antibacterial agent to the cellulose fiber is 5-1, stir at 500-800 rpm for 20-60 min at room temperature to obtain a primary product suspension, take carboxylated β-cyclodextrin powder and add it to the primary product suspension, stir at room temperature for 10-30 min to complete the first layer of self-assembly, and centrifuge to obtain antibacterial and deodorizing functional fibers;

[0009] (3) The antibacterial and deodorizing functional fibers assembled in the first layer are mixed evenly with deionized water, an antibacterial agent is added, and the mixture is stirred at 500-800 rpm for 20-60 min at room temperature, and then carboxylated β-cyclodextrin powder is added, and the mixture is stirred at room temperature for 10-30 min, and the mixture is centrifuged to obtain the antibacterial and deodorizing functional fibers, thereby completing the second layer of self-assembly. The above operation can be repeated as needed to obtain the antibacterial and deodorizing functional fibers self-assembled layer by layer.

[0010] The method for preparing the antibacterial and deodorizing functional fiber is characterized in that the cellulose fiber has a diameter of 10-500 nm and an electrical conductivity of 20-70 μs.

[0011] A non-woven fabric material contains the antibacterial and deodorizing functional fiber.

[0012] The non-woven fabric material is characterized in that the antibacterial and deodorizing functional fibers can be post-treated by dipping, spraying or surface coating, and the glue amount of the non-woven fabric material is 0.1 g / m 2 Up to 3.0g / m 2 , preferably 0.3g / m 2 Up to 1.0g / m 2 .

[0013] The beneficial effects of the present invention include:

[0014] (1) The present invention prepares fibers with antibacterial and deodorizing functions by introducing antibacterial agents, carboxylated β-cyclodextrin and cellulose fibers. The introduction of antibacterial agents effectively inhibits the reproduction and survival of microorganisms, thereby achieving an antibacterial effect; the introduction of carboxylated β-cyclodextrin and cellulose fibers achieves a deodorizing effect. First, the cavity of carboxylated β-cyclodextrin can be used to embed odor molecules, and secondly, the active groups of carboxylated β-cyclodextrin react chemically with ammonia and hydrogen sulfide to decompose the gas. Finally, cellulose fibers contain a large number of alcohol hydroxyl groups and a small number of carboxyl groups, and there are a large number of sieve holes in cellulose fibers, which makes it very easy to adsorb small molecules, thereby achieving the removal of acidic gases such as ammonia, hydrogen sulfide, and isovaleric acid.

[0015] (2) The present invention prepares non-dissolving antibacterial and deodorizing functional fibers through layer-by-layer self-assembly technology of antibacterial agents, carboxylated β-cyclodextrin and cellulose fibers, and realizes the controllability of the antibacterial and deodorizing properties of the materials. Cellulose fiber is one of the most widely distributed and highest content natural polymers in nature. It is prepared from natural cellulose and has the advantages of low cost, renewability, biodegradability, biocompatibility, non-toxicity, no pollution, stable chemical properties, good mechanical properties, etc. First, the advantages of large specific surface area and large number of hydroxyl groups of cellulose fibers are used to provide a large number of binding sites for the antibacterial agent, and the antibacterial agent is deposited on the cellulose fibers, and then dispersed into the carboxylated β-cyclodextrin after screening. Then, by using the layer-by-layer alternating deposition method, with the help of the interaction between the molecules of each layer, the cellulose fibers, the antibacterial agent and the carboxylated β-cyclodextrin are spontaneously associated to form a molecular aggregate or supramolecular structure with complete structure, stable performance and antibacterial and deodorizing functions, thereby realizing the preparation of non-dissolving antibacterial and deodorizing functional fibers. Finally, the amount of antibacterial agent and deodorant glue is controlled by adjusting the number of self-assembly layers, thereby achieving controllable antibacterial and deodorant performance. The antibacterial agent and deodorant assembled layer by layer are subject to intermolecular repulsion, and the molecular chains are independent of each other. The layer-by-layer assembly structure has a large specific surface area, which can better play the role of antibacterial agent and deodorant.

[0016] (3) Polypropylene, polyethylene, and polyester polymer materials used to prepare non-woven fabrics have low polarity and weak interaction with antimicrobial agents. If antimicrobial agents are directly applied to non-woven fabrics, they are easily eluted from the non-woven fabrics, posing a potential threat to human health. Therefore, it is necessary to modify and graft antimicrobial agents onto non-woven fabrics through special methods such as high temperature, plasma, and ultraviolet radiation to achieve non-elution of antimicrobial substances. These methods have the disadvantages of destroying the structure of the non-woven fabric, unstable modification effects, high energy consumption, and low efficiency, which limits their industrial application. By utilizing the characteristics of cellulose fibers such as large specific surface area, high reaction activity, and easy adhesion, the bonding strength between cellulose fibers and the substrate is improved, thereby preventing the dissolution of antimicrobial agents and deodorants from non-woven fabrics. In addition, by utilizing the capillary properties of cellulose fibers, the liquid penetration performance and surface hydrophilicity of non-woven fabrics can be further improved.

[0017] (4) The antibacterial and deodorizing functional fibers prepared by the present invention have the advantages of good hydrophilicity, high temperature resistance, and adjustable viscosity range. The non-woven fabric materials or paper-based materials can be post-treated by dipping, spraying or surface coating. The non-woven fabric materials prepared by the present invention can be widely used in pet pads, insoles, socks, and wipes, and are particularly suitable for disposable sanitary products such as diapers (sheets, pads), sanitary napkins, and masks. DETAILED DESCRIPTION

[0018] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention. It should be noted that the embodiments in this application and the features in the embodiments can be combined with each other arbitrarily without conflict.

[0019] Example 1

[0020] (1) preparing a 40 g / L aqueous solution of sodium hydroxide, weighing a certain amount of β-cyclodextrin and adding it to the alkali solution, wherein the mass ratio of β-cyclodextrin to sodium hydroxide is 1, stirring until the β-cyclodextrin is completely dissolved, heating to 90° C., adding a certain amount of sodium chloroacetate, wherein the mass ratio of sodium chloroacetate to β-cyclodextrin is 2, reacting for 1 h, adjusting the pH to 5-6, washing with ethanol and deionized water, and drying to obtain a carboxylated β-cyclodextrin powder;

[0021] (2) Weigh a certain amount of cellulose fiber, mix it with deionized water to obtain a 0.2wt% cellulose fiber suspension, add the antibacterial agent hydroxypropyltrimethylammonium chloride chitosan to the suspension, the mass ratio of the antibacterial agent to the cellulose fiber is 2, stir at 700rpm for 30min at room temperature to obtain a primary product suspension, take carboxylated β-cyclodextrin powder and add it to the primary product suspension, stir at room temperature for 20min to complete the first layer of self-assembly, and centrifuge to obtain antibacterial and deodorizing functional fibers.

[0022] Example 2

[0023] (1) preparing a 40 g / L aqueous solution of sodium hydroxide, weighing a certain amount of β-cyclodextrin and adding it to the alkali solution, wherein the mass ratio of β-cyclodextrin to sodium hydroxide is 1, stirring until the β-cyclodextrin is completely dissolved, heating to 90° C., adding a certain amount of sodium chloroacetate, wherein the mass ratio of sodium chloroacetate to β-cyclodextrin is 2, reacting for 1 h, adjusting the pH to 5-6, washing with ethanol and deionized water, and drying to obtain a carboxylated β-cyclodextrin powder;

[0024] (2) Weigh a certain amount of cellulose fiber, mix it with deionized water to obtain a 0.2wt% cellulose fiber suspension, add the antibacterial agent hydroxypropyltrimethylammonium chloride chitosan to the suspension, the mass ratio of the antibacterial agent to the cellulose fiber is 2, stir at 700 rpm for 30 minutes at room temperature to obtain a primary product suspension, take carboxylated β-cyclodextrin powder and add it to the primary product suspension, stir at room temperature for 20 minutes to complete the first layer of self-assembly, and centrifuge to obtain antibacterial and deodorizing functional fibers;

[0025] (3) The first layer of antibacterial and deodorizing functional fibers assembled were mixed evenly with deionized water, an antibacterial agent was added, and the mixture was stirred at 700 rpm for 30 min at room temperature. Then, carboxylated β-cyclodextrin powder was added, and the mixture was stirred at room temperature for 20 min. The antibacterial and deodorizing functional fibers were obtained by centrifugation. The second layer of self-assembly was completed, and the layer-by-layer assembled antibacterial and deodorizing functional fibers were obtained by centrifugation.

[0026] Example 3

[0027] (1) preparing a 40 g / L aqueous solution of sodium hydroxide, weighing a certain amount of β-cyclodextrin and adding it to the alkali solution, wherein the mass ratio of β-cyclodextrin to sodium hydroxide is 1, stirring until the β-cyclodextrin is completely dissolved, heating to 90° C., adding a certain amount of sodium chloroacetate, wherein the mass ratio of sodium chloroacetate to β-cyclodextrin is 2, reacting for 1 h, adjusting the pH to 5-6, washing with ethanol and deionized water, and drying to obtain a carboxylated β-cyclodextrin powder;

[0028] (2) Weigh a certain amount of cellulose fiber, mix it with deionized water to obtain a 0.2wt% cellulose fiber suspension, add the antibacterial agent hydroxypropyltrimethylammonium chloride chitosan to the suspension, the mass ratio of the antibacterial agent to the cellulose fiber is 2, stir at 700 rpm for 30 minutes at room temperature to obtain a primary product suspension, take carboxylated β-cyclodextrin powder and add it to the primary product suspension, stir at room temperature for 20 minutes to complete the first layer of self-assembly, and centrifuge to obtain antibacterial and deodorizing functional fibers;

[0029] (3) The antibacterial and deodorizing functional fibers assembled in the first layer were mixed evenly with deionized water, an antibacterial agent was added, and the mixture was stirred at 700 rpm for 30 min at room temperature. Then, carboxylated β-cyclodextrin powder was added, and the mixture was stirred at room temperature for 20 min. The antibacterial and deodorizing functional fibers were obtained by centrifugation to complete the second layer of self-assembly.

[0030] (4) The second layer of antibacterial and deodorizing functional fibers assembled were mixed evenly with deionized water, an antibacterial agent was added, and the mixture was stirred at 700 rpm for 30 min at room temperature. Then, carboxylated β-cyclodextrin powder was added, and the mixture was stirred at room temperature for 20 min. The antibacterial and deodorizing functional fibers were obtained by centrifugation to complete the third layer of self-assembly. The layer-by-layer assembled antibacterial and deodorizing functional fibers were obtained by centrifugation.

[0031] Example 4

[0032] (1) preparing a 40 g / L aqueous solution of sodium hydroxide, weighing a certain amount of β-cyclodextrin and adding it to the alkali solution, wherein the mass ratio of β-cyclodextrin to sodium hydroxide is 1, stirring until the β-cyclodextrin is completely dissolved, heating to 90° C., adding a certain amount of sodium chloroacetate, wherein the mass ratio of sodium chloroacetate to β-cyclodextrin is 2, reacting for 1 h, adjusting the pH to 5-6, washing with ethanol and deionized water, and drying to obtain a carboxylated β-cyclodextrin powder;

[0033] (2) Weigh a certain amount of cellulose fiber, mix it with deionized water to obtain a 0.2wt% cellulose fiber suspension, add the antibacterial agent hydroxypropyltrimethylammonium chloride chitosan to the suspension, the mass ratio of the antibacterial agent to the cellulose fiber is 2, stir at 700 rpm for 30 minutes at room temperature to obtain a primary product suspension, take carboxylated β-cyclodextrin powder and add it to the primary product suspension, stir at room temperature for 20 minutes to complete the first layer of self-assembly, and centrifuge to obtain antibacterial and deodorizing functional fibers;

[0034] (3) The antibacterial and deodorizing functional fibers assembled in the first layer were mixed evenly with deionized water, an antibacterial agent was added, and the mixture was stirred at 700 rpm for 30 min at room temperature. Then, carboxylated β-cyclodextrin powder was added, and the mixture was stirred at room temperature for 20 min. The antibacterial and deodorizing functional fibers were obtained by centrifugation to complete the second layer of self-assembly.

[0035] (4) The antibacterial and deodorizing functional fibers assembled in the second layer were mixed evenly with deionized water, an antibacterial agent was added, and the mixture was stirred at 700 rpm for 30 min at room temperature. Then, carboxylated β-cyclodextrin powder was added, and the mixture was stirred at room temperature for 20 min. The antibacterial and deodorizing functional fibers were obtained by centrifugation, and the third layer of self-assembly was completed.

[0036] (5) The third layer of antibacterial and deodorizing functional fibers assembled were mixed evenly with deionized water, and an antibacterial agent was added. The mixture was stirred at 700 rpm for 30 min at room temperature. Then, carboxylated β-cyclodextrin powder was added. The mixture was stirred at room temperature for 20 min. The antibacterial and deodorizing functional fibers were obtained by centrifugation. The fourth layer of self-assembly was completed. The layer-by-layer assembled antibacterial and deodorizing functional fibers were obtained by centrifugation.

[0037] Example 5

[0038] In this example, the antibacterial and deodorizing properties of the antibacterial and deodorizing functional fibers prepared in Examples 1, 2, 3, and 4 were tested.

[0039] Antibacterial performance testing basis: WST 65-2019 "Evaluation Methods for Antibacterial and Antibacterial Effects";

[0040] Deodorization performance test method: spray the antibacterial deodorization functional fibers into a closed container with a known odor (H2S, NH3) concentration C0, and place it in a closed container for 60 minutes. Then use a detection instrument to test the odor (H2S, NH3) concentration C1 in the closed instrument, and calculate the odor removal rate of the sample according to the formula odor removal rate (%) = (C0-C1) / C0, where C0 is the initial concentration of the odor (H2S, NH3) in the closed container, and C1 is the concentration of the odor (H2S, NH3) in the closed container after adding the antibacterial deodorization functional fibers. The test results are shown in Table 1.

[0041] Table 1 Antibacterial and deodorizing performance test results

[0042]

[0043] According to Table 1, as the number of assembly layers increases, the antibacterial rate, ammonia and hydrogen sulfide removal rates of the antibacterial and deodorizing functional fibers increase. When the number of assembly layers is 4, the antibacterial rates of the antibacterial and deodorizing functional fibers for Escherichia coli, Staphylococcus aureus and Candida albicans are all 99.9%, the ammonia removal rate is 95%, and the hydrogen sulfide removal rate reaches 75%.

[0044] Example 6

[0045] The antibacterial and deodorizing functional fiber prepared in Example 2 was added to deionized water, stirred and dispersed evenly, and an antibacterial and deodorizing functional fiber finishing agent was obtained; the non-woven fabric was roll-coated by a coating machine, and the non-woven fabric was stretched to a drying channel for drying to obtain an antibacterial and deodorizing functional non-woven fabric material; the glue amount of the non-woven fabric was controlled to be 0.3 g / m by adjusting the pressure of the feeding roller. 2 .

[0046] Example 7

[0047] The antibacterial and deodorizing functional fiber prepared in Example 2 was added to deionized water, stirred and dispersed evenly, and an antibacterial and deodorizing functional fiber finishing agent was obtained; the non-woven fabric was roll-coated by a coating machine, and the non-woven fabric was stretched to a drying channel for drying to obtain an antibacterial and deodorizing functional non-woven fabric material. The glue amount was adjusted to 0.7 g / m by adjusting the pressure of the feeding roller. 2 .

[0048] Example 8

[0049] The antibacterial and deodorizing functional fiber prepared in Example 2 was added to deionized water, stirred and dispersed evenly, and an antibacterial and deodorizing functional fiber finishing agent was obtained; the non-woven fabric was roll-coated by a coating machine, and the non-woven fabric was stretched to a drying channel for drying to obtain an antibacterial and deodorizing functional non-woven fabric material; the glue amount was adjusted to 1.0 g / m by adjusting the pressure of the feeding roller. 2 .

[0050] Example 9

[0051] The antibacterial and deodorizing functional fiber prepared in Example 2 was added to deionized water, stirred and dispersed evenly, and an antibacterial and deodorizing functional fiber finishing agent was obtained; the non-woven fabric was roll-coated by a coating machine, and the non-woven fabric was stretched to a drying channel for drying to obtain an antibacterial and deodorizing functional non-woven fabric material. The glue amount was adjusted to 2.0 g / m by adjusting the pressure of the feeding roller. 2 .

[0052] Example 10

[0053] In this example, the dissolution and non-dissolution properties, antibacterial properties, deodorizing properties, and liquid penetration properties of the antibacterial and deodorizing functional non-woven fabrics prepared in Examples 6, 7, 8, and 9 were tested, and an untreated blank non-woven fabric was used as a control sample.

[0054] Dissolution and non-dissolution determination method for antibacterial materials: According to the national standard GB / T 31713-2015 "Safety and Hygiene Requirements for Antibacterial Textiles", the dissolution and non-dissolution of antibacterial and deodorizing functional non-woven fabrics were determined. The results are shown in Table 2:

[0055] Table 2 Antibacterial zone width of nonwoven fabric with antibacterial and deodorizing function

[0056]

[0057] According to Table 2, the antibacterial and deodorizing functional nonwoven fabrics prepared in Examples 6, 7, 8 and 9 have inhibition zone widths of less than 1 mm for Escherichia coli, Staphylococcus aureus and Candida albicans, which shows that the prepared antibacterial and deodorizing functional nonwoven fabrics are non-dissolving materials.

[0058] The antibacterial performance test is carried out in accordance with the national standard GB15979-2002 "Standard for Disposable Hygiene Products" C5 non-dissolving antibacterial product antibacterial performance test method;

[0059] Deodorization performance test: Deodorization performance test was carried out in accordance with the national standard GB / T33610.2-2017 "Determination of deodorization performance of textiles Part 2: Inspection tube method";

[0060] Liquid penetration performance test: Performance test was carried out in accordance with the national standard GB / T24218.13-2010 "Test methods for textile nonwovens Part 13: Determination of liquid multiple penetration time". The test results of antibacterial performance, deodorization performance and liquid penetration performance are shown in Table 3.

[0061] Table 3 Test results of antibacterial and deodorizing performance and liquid penetration performance of nonwoven fabrics with antibacterial and deodorizing functions

[0062]

[0063] According to Table 3, compared with the control sample, the antibacterial and deodorizing functional fiber prepared by the present invention is used for post-processing non-woven fabric materials, and the prepared non-woven fabric materials are non-dissolving antibacterial materials, and have good liquid multiple penetration and excellent antibacterial and deodorizing properties.

[0064] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing antibacterial and deodorizing functional fibers, Features The following steps are involved: (1) preparing sodium hydroxide into a 20-45 g / L aqueous solution, weighing β-cyclodextrin and adding it to an alkaline solution, wherein the mass ratio of β-cyclodextrin to sodium hydroxide is 2-0.5, stirring until β-cyclodextrin is completely dissolved, heating to 80-100° C., adding a certain amount of sodium chloroacetate, wherein the mass ratio of sodium chloroacetate to β-cyclodextrin is 2-0.5, reacting for 1-3 h, adjusting the pH to 5-6, washing with ethanol and deionized water, and drying to obtain a carboxylated β-cyclodextrin powder; (2) weighing cellulose fibers, mixing them with deionized water to obtain a 0.05-0.2wt% cellulose fiber suspension, adding an antibacterial agent to the suspension, wherein the antibacterial agent is at least one of chitosan quaternary ammonium salts, chitosan oligosaccharides, guanidines, and betaines, and the mass ratio of the antibacterial agent to the cellulose fibers is 5-1, stirring at 500-800 rpm for 20-60 min at room temperature to obtain a primary product suspension, taking carboxylated β-cyclodextrin powder and adding it to the primary product suspension, stirring at room temperature for 10-30 min to complete the first layer of self-assembly, and centrifuging to obtain antibacterial and deodorizing functional fibers; (3) Evenly mix the first layer of assembled antibacterial and deodorizing functional fibers and deionized water, add antibacterial agent, stir at 500-800 rpm for 20-60 min at room temperature, then add carboxylated β-cyclodextrin powder, stir at room temperature for 10-30 min, centrifuge to obtain antibacterial and deodorizing functional fibers, complete the second layer of self-assembly, centrifuge to obtain layer-by-layer assembled antibacterial and deodorizing functional fibers, and repeat the above operation as needed to obtain layer-by-layer self-assembled antibacterial and deodorizing functional fibers.

2. The method for preparing the antibacterial and deodorizing functional fiber according to claim 1, It is characterized in that The cellulose fiber has a diameter of 10-500 nm and an electrical conductivity of 20-70 μs.

3. A non-woven material, It is characterized in that Contains the antibacterial and deodorizing functional fiber according to claim 1.

4. The nonwoven material according to claim 3, It is characterized in that The antibacterial and deodorizing functional fibers are post-processed with non-woven fabrics by dipping, spraying or surface coating, and the glue amount of the non-woven fabrics is 0.1 g / m 2 Up to 3g / m 2 .