Methods for improving the quality of flash welding joints of medium carbon low alloy rails

By adding the forging stage during the rail welding process, and using forging to improve the quality of welded joints of medium-carbon and low-alloy rails, the problem that rail joints in plateau and high-altitude areas are difficult to meet service requirements, and the high quality and safety of welded joints are improved.

CN115673505BActive Publication Date: 2024-11-26PANZHIHUA IRON & STEEL RES INST OF PANGANG GROUP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211479634.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-24
Publication Date
2024-11-26
Estimated Expiration
2042-11-24

AI Technical Summary

Technical Problem

Due to large temperature differences and complex working conditions, the welding quality of the joints of rails on plateaus and high-altitude areas is difficult to meet service requirements, and it is prone to abrasions of martensite tissue and the risk of rail breakage, which affects safety.

Method used

A method is adopted, including pre-flash, flash, accelerated burning, top forging and forging stages. The consumption of the forging stage is 2.0mm~4.0mm, the time is 2.0s~3.0s, and the average speed is 0.60mm/s~2.0mm/ s, the pressure is 50T~80T, and the plasticity and toughness of the rail welded joint are improved through forging.

Benefits of technology

It can pass hammer drop inspection and static bending test without post-welding heat treatment, significantly improve joint quality, simplify process and reduce costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115673505B_ABST
    Figure CN115673505B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for improving the quality of flash welding joints of medium-carbon low-alloy rails, comprising sequentially performing pre-flash, flash, accelerated burning, top forging and forging on the rails, wherein the rail consumption in the forging stage is 2.0 mm to 4.0 mm, the forging time is 2.0 s to 3.0 s, the average speed is 0.8 mm / s to 2.0 mm / s, and the forging pressure is 50 T to 80 T. The method obtains a high-quality medium-carbon low-alloy rail welded joint with good plasticity and toughness by adding a forging stage after flash welding.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of welding, and in particular relates to a method for improving the quality of flash welding joints of medium-carbon low-alloy rails. Background Art

[0002] The carbon content of pearlite rails is usually 0.70% to 0.84%, the strength of hot-rolled rails ranges from 880 to 1080 MPa, and the hardness is 260 to 350 HBW; the strength of heat-treated rails is 1080 to 1280 MPa, and the hardness is 320 to 400 HB. The main representative rail grades are U71Mn, U75V, and U78CrV. This type of rail is mainly used for domestic high-speed railways, mixed passenger and freight transportation, and heavy-load lines. This type of rail has a high carbon content, a high content of alloy elements, high strength and hardness, and good wear resistance. Normalizing must be performed after welding the joints to ensure the quality of the joints. In view of the special natural conditions such as plateaus and high-cold areas, large temperature differences throughout the year and large day and night temperatures, higher requirements are placed on the impact toughness of rails. At present, for railway lines in plateaus and high-cold areas, large temperature differences throughout the year and large day and night temperature differences, and complex line conditions, there is no rail that can fully meet its service requirements. Therefore, the treads of steel rails laid on ultra-long downhill sections in plateau and cold regions are prone to abrasion of the martensitic structure, leading to the risk of rail breakage, which seriously affects service safety.

[0003] Therefore, the railway engineering field is in urgent need of a process method to improve the quality of flash welding joints of medium-carbon low-alloy rails. Summary of the invention

[0004] The invention discloses a method for improving the quality of flash welded joints of medium-carbon low-alloy rails. A forging stage is added after flash welding to obtain high-quality medium-carbon low-alloy rail welded joints with good plasticity and toughness.

[0005] In order to solve at least one of the above technical problems, the present invention adopts the following technical solution:

[0006] According to the present invention, a method for improving the quality of flash welded joints of medium-carbon low-alloy rails is provided, comprising sequentially performing pre-flash, flash, accelerated burning, top forging and forging on the rails, wherein the rail consumption in the forging stage is 2.0 mm to 4.0 mm, the forging time is 2.0 s to 3.0 s, the average speed is 0.60 mm / s to 2.0 mm / s, and the forging pressure is 50 T to 80 T.

[0007] According to one embodiment of the present invention, the rail consumption in the forging stage is 2.0 mm to 4.0 mm, the forging time is 2.0 s to 3.0 s, the average speed is 0.8 mm / s to 2.0 mm / s, and the forging pressure is 50 T to 80 T.

[0008] According to one embodiment of the present invention, the medium carbon low alloy rail contains the following components in mass fractions: C: 0.50% to 0.63%, Si: 0.30% to 0.60%, Mn: 0.55% to 0.80%, Cr+Ni+V: 0.30% to 0.9%, P, S≤0.025%, and the balance is Fe and unavoidable impurities.

[0009] According to one embodiment of the present invention, in the pre-flash stage: the setting time is 15s to 30s, the voltage is 370V to 400V, the setting current 1 is 180A to 220A, the current 2 is 270A to 400A, the current 3 is 350A to 450A, the pre-flash displacement is 3mm to 7mm, the forward speed is 1mm / s to 1.5mm / s, and the backward speed is 0.5mm / s to 1.2mm / s.

[0010] According to one embodiment of the present invention, in the flash stage: Flash sub-stage 1: set time to 10s-25s, voltage to 330V-360V, set current 1 to 200A-280A, current 2 to 350A-500A, current 3 to 450A-550A, pre-flash displacement to 6mm-12mm, forward speed to 1.2mm / s-1.7mm / s, and backward speed to 0.5mm / s-1.2mm / s; Flash sub-stage 2: set time to 10s-25s, voltage to 300V-340V, set current 1 to 220A-250A, current 2 to 310A-460A, current 3 to 400A-530A, pre-flash displacement to 6mm-10mm, forward speed to 1.5mm / s-2.5mm / s, and backward speed to 0.5mm / s~1.2mm / s; Flash sub-stage 3: set time to 5s~15s, voltage to 300V~330V, set current 1 to 230A~300A, current 2 to 300A~450A, current 3 to 380A~520A, pre-flash displacement to 3mm~6mm, forward speed to 1.3mm / s~2.3mm / s, and backward speed to 0.5mm / s~1.5mm / s; Flash sub-stage 4: set time to 5s~15s, voltage to 320V~360V, set current 1 to 150A~300A, current 2 to 300A~400A, current 3 to 350A~500A, pre-flash displacement to 3mm~5mm, forward speed to 0.6mm / s~1.3mm / s, and backward speed to 0.3mm / s~1.0mm / s.

[0011] According to one embodiment of the present invention, in the accelerated burning stage: accelerated burning sub-stage 1: set time to 3s~8s, voltage to 350V~380V, set current 1 to 150A~300A, current 2 to 350A~500A, current 3 to 450A~550A, pre-flash displacement to 5mm~10mm, forward speed to 0.6mm / s~1.3mm / s, and backward speed to 0.3mm / s~0.8mm / s; accelerated burning sub-stage 2: set time to 1s~5s, voltage to 360V~400V, set current 1 to 200A~300A, current 2 to 350A~500A, current 3 to 450A~550A, pre-flash displacement to 5mm~10mm, forward speed to 0.6mm / s~1.3mm / s, and backward speed to 0.1mm / s~0.4mm / s.

[0012] According to one embodiment of the present invention, in the upset stage: the charged upset time is set to 0.1s to 2.0s, and the upset amount is set to 12mm to 15.0mm.

[0013] According to one embodiment of the present invention, after the forging stage, the flash welded joint is placed in air to cool naturally to room temperature.

[0014] By adopting the above technical solution, the present invention has at least one of the following advantages compared with the prior art:

[0015] 1. The method of the present invention adds a forging stage, so that the metal atoms on the end face of the steel rail to be welded penetrate and diffuse each other under the action of the forging force, forming a connection between the metal atoms, and completing crystallization under the action of pressure, so that the joint forms a forged structure, which greatly improves the quality of the joint;

[0016] 2. The technical solution of the present invention does not require post-weld heat treatment. Even in the welded state, it can pass the drop hammer test and static bending test, effectively simplifying the welding process and reducing welding costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0018] Figure 1 The present invention is a flow chart of a method for improving the quality of flash welded joints of medium carbon low alloy rails. DETAILED DESCRIPTION

[0019] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0020] The main indicators for quality evaluation of rail flash welds in my country include drop hammer test and static bending test. Drop hammer test is the most difficult item to pass in the rail welding type inspection process. For the drop hammer test of 60kg / m rail flash welds, the hammer mass is 1000kg, the drop hammer height is 3.1m, and it is qualified if it is continuous for 2 times, or the drop hammer height is 5.2m, and it is continuous for 1 time. For the drop hammer test of 75kg / m rail flash welds, the hammer mass is 1000kg, the drop hammer height is 3.8m, and it is continuous for 2 times, or the drop hammer height is 6.4m, and it is continuous for 1 time. The heating temperature of the rail flash weld exceeds the melting point of the rail, and the welding heat input, upsetting amount and final burning speed are not properly matched. The joints are prone to overburning, gray spots and other defects. It is very difficult for the joints to pass the drop hammer type inspection. In order to pass the drop hammer type inspection, a large amount of process optimization is usually required. The number of test joints alone is as high as 150-500 joints, which consumes a lot of manpower and material resources.

[0021] The static bending test of the flash weld joint can reflect the quality of the rail flash weld joint. The standard requirements of my country are 60kg / m, the rail head is under pressure, and the breaking load is not less than 1450kN; 75kg / m, the rail head is under pressure, and the breaking load is not less than 1850kN. There is no requirement for deflection. The static bending load mainly reflects the bonding strength and internal defect index of the joint, and the deflection mainly reflects the strength and toughness index of the joint. If the welding process of the joint is poor, it is very likely that the joint will break before the load value specified in the standard is reached due to defects such as gray spots, lack of fusion or overburning, or because the joint heat input and upsetting amount are improperly matched, or the post-weld treatment method is improper, resulting in the joint being too hard or too soft, so that the joint deflection does not meet the standard requirements.

[0022] In the rail flash welding method, the heating temperature of the joint exceeds the melting point of the rail, the welding heat input, the amount of upsetting and the final burning speed are not properly matched, and the joint is prone to overburning, gray spots and other defects. It is very difficult for 15 joints to pass the drop hammer type inspection in a row. In order to pass the drop hammer type inspection, a large amount of process optimization is usually required. The number of test joints alone is as high as 150-500 joints, which consumes a lot of manpower and material resources. According to the method for improving the quality of flash welded joints of medium-carbon low-alloy rails, the pulsating flash process of the K950 welding machine produced in Ukraine is adopted. After welding, the weld of the flash welded joint of the rail has no welding defects such as gray spots, unwelded and overburned, and the joint quality is stable. After the flash welding is completed, the joint is placed in the air to cool naturally to room temperature. Even in the welded state, it can pass the drop hammer inspection and static bending test.

[0023] Figure 1The flow chart of the method for improving the hardness of the flash welded joint of a medium carbon low alloy rail according to the present invention is shown. The method can be applied to medium carbon low alloy rails, and the chemical composition of the welding base material and the weight percentage of each component are preferably: C: 0.50% to 0.63%, Si: 0.30% to 0.60%, Mn: 0.55% to 0.80%, Cr+Ni+V: 0.30% to 0.9%, P, S ≤ 0.025%, and the balance is Fe and unavoidable impurities. The method can generally include the following steps:

[0024] Step S1, pre-flash stage;

[0025] Step S2, flashing stage;

[0026] Step S3, accelerating the burning stage;

[0027] Step S4, upsetting stage; and

[0028] Step S5, forging stage.

[0029] The main function of the pre-flash stage is to make the cross section of the rail to be welded flat and clean through flash blasting, and provide relatively uniform and flat favorable conditions and basic heat for subsequent flashing. To achieve the above purpose, the pulsating flash process of the present invention is controlled by setting eight variables, namely, pre-flash time, voltage, current 1, 2, 3, pre-flash displacement, forward and backward speeds. In an embodiment of the present invention, the pre-flash stage of step S1 can be set to a time of 15s to 30s, a voltage of 370V to 400V, current 1 of 180A to 220A, current 2 of 270A to 400A, current 3 of 350A to 450A, pre-flash displacement of 3mm to 7mm, forward speed of 1mm / s to 1.5mm / s, and backward speed of 0.5mm / s to 1.2mm / s.

[0030] The main function of the flash stage is to continue to heat the rail surface to be welded through pulsating flash on the basis of the heat accumulated in the previous pre-flash, so as to form a certain temperature gradient in the longitudinal direction of the rail, heat the end face of the rail to a sufficient temperature and lay the foundation for accelerating the burning process. In the early flash stage, the temperature of the rail end face is relatively low, and a higher voltage and current are required to make the flash process normal. After the temperature of the rail end face rises, the higher voltage and current will cause the burning speed to be too fast, and too much heat will be taken away, which is not conducive to heat accumulation. Therefore, the flash is divided into 4 sub-stages. The voltage and current of the latter sub-stage are lower than those of the previous sub-stage, so as to heat the end face of the rail to a sufficient temperature and lay the foundation for accelerating the burning process. The 4 sub-stages all need to set 8 variables, such as flash time, voltage, current 1, 2, 3, pre-flash displacement, forward and backward speed. In the embodiment of the present invention, the flash sub-stage of step S2 is divided into 4 sub-stages. Among them, flash sub-stage 1: set time to 10s~25s, voltage to 330V~360V, set current 1 to 200A~280A, current 2 to 350A~500A, current 3 to 450A~550A, pre-flash displacement to 6mm~12mm, forward speed to 1.2mm / s~1.7mm / s, and backward speed to 0.5mm / s~1.2mm / s; flash sub-stage 2: set time to 10s~25s, voltage to 300V~340V, set current 1 to 220A~250A, current 2 to 310A~460A, current 3 to 400A~530A, pre-flash displacement to 6mm~10mm, forward speed to 1.5mm / s~2.5mm / s, and backward speed to 0.5mm / s~1.2m m / s; Flash sub-stage 3: set time to 5s~15s, voltage to 300V~330V, set current 1 to 230A~300A, current 2 to 300A~450A, current 3 to 380A~520A, pre-flash displacement to 3mm~6mm, forward speed to 1.3mm / s~2.3mm / s, and backward speed to 0.5mm / s~1.5mm / s; Flash sub-stage 4: set time to 5s~15s, voltage to 320V~360V, set current 1 to 150A~300A, current 2 to 300A~400A, current 3 to 350A~500A, pre-flash displacement to 3mm~5mm, forward speed to 0.6mm / s~1.3mm / s, and backward speed to 0.3mm / s~1.0mm / s.

[0031] The main function of the accelerated burning stage is to form a protective atmosphere in the entire welding area to prevent end face oxidation, and finally form a suitable temperature field distribution to provide conditions for top forging. The accelerated burning stage has strong flash and fast burning speed. The accelerated burning stage is divided into two sub-stages, and the current and voltage gradually increase. Each sub-stage requires setting eight variables such as flash time, setting voltage, setting current 1, 2, 3, setting pre-flash displacement, and setting forward and backward speeds. In an embodiment of the present invention, the accelerated burning sub-stage of step S3 is divided into two stages. Among them, the accelerated burning sub-stage 1: the set time is 3s~8s, the voltage is 350V~380V, the set current 1 is 150A~300A, the current 2 is 350A~500A, the current 3 is 450A~550A, the pre-flash displacement is 5mm~10mm, the forward speed is 0.6mm / s~1.3mm / s, and the backward speed is 0.3mm / s~0.8mm / s; the accelerated burning sub-stage 2: the set time is 1s~5s, the voltage is 360V~400V, the set current 1 is 200A~300A, the current 2 is 350A~500A, the current 3 is 450A~550A, the pre-flash displacement is 5mm~10mm, the forward speed is 0.6mm / s~1.3mm / s, and the backward speed is 0.1mm / s~0.4mm / s.

[0032] In the upset stage of step S4, the live upset time can be set to 0.1s to 2.0s, and the upset amount can be set to 12mm to 15.0mm.

[0033] In step S5, the forging stage is mainly used to continuously apply load to the rail joint during the metal crystallization process of the joint after the rail top forging to enhance the joint quality. After the forging stage is completed, there is no need to perform any heat treatment on the joint after welding, and it can be directly placed in the air to cool naturally to room temperature.

[0034] Alternatively, technicians can also perform normalizing on the joint after welding to further improve the plasticity and toughness of the joint.

[0035] The following is a specific embodiment of the method for improving the hardness of a flash welded joint of a medium carbon low alloy rail according to the present invention.

[0036] Example 1

[0037] In this embodiment, the chemical composition of the rail is measured to have a carbon mass fraction of 0.61%, a Si mass fraction of 0.55%, a Mn mass fraction of 0.7%, a Cr+Ni+V mass fraction of 0.5%, and P and S ≤ 0.025%.

[0038] The rails are subjected to pre-flashing, flashing, accelerated burning, upsetting and forging in sequence. Among them, the specific operating parameters are:

[0039] In the pre-flash stage, the time is 15s, the voltage is 400V, the setting current 1 is 180A, the current 2 is 270A, the current 3 is 350A, the pre-flash displacement is 7mm, the forward speed is 1.5mm / s, and the backward speed is 1.2mm / s;

[0040] Flash sub-stage 1, set time to 25s, voltage to 360V, set current 1 to 200A, current 2 to 350A, current 3 to 450A, flash displacement to 6mm, forward speed to 1.5mm / s, backward speed to 1.2mm / s;

[0041] Flash sub-stage 2, set time to 25s, voltage to 330V, set current 1 to 250A, current 2 to 310A, current 3 to 400A, flash displacement to 6mm, forward speed to 1.5mm / s, backward speed to 1.2mm / s;

[0042] Flash sub-stage 3, set time to 5s, voltage to 330V, set current 1 to 300A, current 2 to 450A, current 3 to 520A, flash displacement to 6mm, forward speed to 1.3mm / s, backward speed to 1.5mm / s;

[0043] Flash sub-stage 4, set time to 5s, voltage to 320V, set current 1 to 150A, current 2 to 300A, current 3 to 350A, flash displacement to 3mm, forward speed to 0.6mm / s, backward speed to 0.3mm / s;

[0044] The setting time of the accelerated burning sub-stage 1 is 8s, the voltage is 380V, the setting current 1 is 300A, the current 2 is 500A, the current 3 is 550A, the burning displacement is 5mm, the forward speed is 0.6mm / s, and the backward speed is 0.3mm / s;

[0045] The setting time of the accelerated burning sub-stage 2 is 2s, the voltage is 400V, the setting current 1 is 300A, the current 2 is 500A, the current 3 is 450A, the burning displacement is 10mm, the forward speed is 0.6mm / s, and the backward speed is 0.4mm / s;

[0046] During the upsetting stage, the charged upsetting time is 0.5s and the upsetting amount is 15mm.

[0047] The main function of the forging stage is to continuously apply load to the rail joint during the metal crystallization process of the joint after the rail top forging to enhance the joint quality. To achieve the above purpose, the rail consumption in the forging stage is 2.0mm, the forging time is 2s, the average speed is 1.0mm / s, and the forging pressure is 50T.

[0048] In the drop hammer test of the rail flash welded joint in this embodiment, the hammer head mass is 1000kg, the drop hammer height is 3.1m, and no fracture occurs after two drops of the hammer. The maximum deflection is 18.2mm, and the joint quality is high.

[0049] Example 2

[0050] In this embodiment, the chemical composition of the rail is measured to have a carbon mass fraction of 0.60%, a Si mass fraction of 0.55%, a Mn mass fraction of 0.72%, a Cr+Ni+V mass fraction of 0.72%, and P and S ≤ 0.025%.

[0051] In the pre-flash stage, the time is 30s, the voltage is 380V, the setting current 1 is 220A, the current 2 is 400A, the current 3 is 450A, the pre-flash displacement is 7mm, the forward speed is 1mm / s, and the backward speed is 0.5mm / s;

[0052] Flash sub-stage 1, set time to 20s, voltage to 350V, set current 1 to 280A, current 2 to 350A, current 3 to 450A, flash displacement to 6mm, forward speed to 1.2mm / s, backward speed to 0.7mm / s;

[0053] Flash sub-stage 2, set time to 10s, voltage to 340V, set current 1 to 250A, current 2 to 330A, current 3 to 400A, flash displacement to 6mm, forward speed to 1.5mm / s, backward speed to 0.5mm / s;

[0054] Flash sub-stage 3, set time to 15s, voltage to 330V, set current 1 to 300A, current 2 to 450A, current 3 to 380A, flash displacement to 6mm, forward speed to 2.3mm / s, backward speed to 1.5mm / s;

[0055] Flash sub-stage 4, set time to 15s, voltage to 360V, set current 1 to 300A, current 2 to 400A, current 3 to 500A, flash displacement to 5mm, forward speed to 1.3mm / s, backward speed to 1.0mm / s;

[0056] The setting time of accelerated burning sub-stage 1 is 3s, the voltage is 380V, the setting current 1 is 300A, the current 2 is 350A, the current 3 is 450A, the burning displacement is 5mm, the forward speed is 0.6mm / s, and the backward speed is 0.8mm / s;

[0057] The setting time of the accelerated burning sub-stage 2 is 5s, the voltage is 400V, the current 1 is 300A, the current 2 is 500A, the current 3 is 550A, the burning displacement is 10mm, the forward speed is 0.9mm / s, and the backward speed is 0.1mm / s;

[0058] During the upsetting stage, the charged upsetting time is 1.0s and the upsetting amount is 15mm.

[0059] The main function of the forging stage is to continuously apply load to the rail joint during the metal crystallization process of the joint after the rail top forging to enhance the joint quality. To achieve the above purpose, the rail consumption in the forging stage is 2.8mm, the forging time is 2s, the average speed is 1.4mm / s, and the forging pressure is 60T.

[0060] In the drop hammer test of the rail flash welded joint in this embodiment, the hammer head mass is 1000kg, the drop hammer height is 3.1m, and no fracture occurs after two drops of the hammer. The maximum deflection is 19.1mm, and the joint quality is high.

[0061] Example 3

[0062] In this embodiment, the chemical composition of the rail is measured to have a carbon mass fraction of 0.58%, a Si mass fraction of 0.53%, a Mn mass fraction of 0.70%, a Cr+Ni+V mass fraction of 0.52%, and P and S ≤ 0.025%.

[0063] In the pre-flash stage, the time is 20s, the voltage is 400V, the setting current 1 is 200A, the current 2 is 350A, the current 3 is 400A, the pre-flash displacement is 5mm, the forward speed is 1mm / s, and the backward speed is 0.5mm / s;

[0064] Flash sub-stage 1, set time to 15s, voltage to 350V, set current 1 to 200A, current 2 to 400A, current 3 to 500A, flash displacement to 6mm, forward speed to 1.7mm / s, backward speed to 0.7mm / s;

[0065] Flash sub-stage 2, set time to 15s, voltage to 340V, set current 1 to 220A, current 2 to 380A, current 3 to 400A, flash displacement to 6mm, forward speed to 1.5mm / s, backward speed to 0.5mm / s;

[0066] In flash sub-stage 3, the setting time is 10s, the voltage is 330V, the setting current 1 is 300A, the current 2 is 450A, the current 3 is 500A, the flash displacement is 6mm, the forward speed is 1.9mm / s, and the backward speed is 0.9mm / s.

[0067] Flash sub-stage 4, set time to 10s, voltage to 355V, set current 1 to 180A, current 2 to 400A, current 3 to 500A, flash displacement to 3mm, forward speed to 0.8mm / s, backward speed to 0.5mm / s;

[0068] The setting time of accelerated burning sub-stage 1 is 5s, the voltage is 360V, the setting current 1 is 180A, the current 2 is 390A, the current 3 is 450A, the burning displacement is 6mm, the forward speed is 1.0mm / s, and the backward speed is 0.3mm / s;

[0069] The setting time of the accelerated burning sub-stage 2 is 3s, the voltage is 390V, the setting current 1 is 250A, the current 2 is 400A, the current 3 is 500A, the burning displacement is 9mm, the forward speed is 1.2mm / s, and the backward speed is 0.1mm / s;

[0070] During the upsetting stage, the charged upsetting time is 1.0s and the upsetting amount is 13.6mm.

[0071] The main function of the forging stage is to continuously apply load to the rail joint during the metal crystallization process of the joint after the rail top forging to enhance the joint quality. To achieve the above purpose, the rail consumption in the forging stage is 3.6mm, the forging time is 3s, the average speed is 1.2mm / s, and the forging pressure is 70T.

[0072] In the drop hammer test of the rail flash welded joint in this embodiment, the hammer head mass is 1000kg, the drop hammer height is 3.1m, and no fracture occurs after the hammer is dropped 3 times. The maximum deflection is 27.0mm, and the joint quality is high.

[0073] Example 4

[0074] In this embodiment, the chemical composition of the rail is measured to have a carbon mass fraction of 0.58%, a Si mass fraction of 0.53%, a Mn mass fraction of 0.70%, a Cr+Ni+V mass fraction of 0.52%, and P and S ≤ 0.025%.

[0075] In the pre-flash stage, the time is 20s, the voltage is 400V, the setting current 1 is 200A, the current 2 is 350A, the current 3 is 400A, the pre-flash displacement is 5mm, the forward speed is 1mm / s, and the backward speed is 0.5mm / s;

[0076] Flash sub-stage 1, set time to 15s, voltage to 350V, set current 1 to 200A, current 2 to 400A, current 3 to 500A, flash displacement to 6mm, forward speed to 1.7mm / s, backward speed to 0.7mm / s;

[0077] Flash sub-stage 2, set time to 15s, voltage to 340V, set current 1 to 220A, current 2 to 380A, current 3 to 400A, flash displacement to 6mm, forward speed to 1.5mm / s, backward speed to 0.5mm / s;

[0078] Flash sub-stage 3, set time to 10s, voltage to 330V, set current 1 to 300A, current 2 to 450A, current 3 to 500A, flash displacement to 6mm, forward speed to 1.9mm / s, backward speed to 0.9mm / s;

[0079] Flash sub-stage 4, set time to 10s, voltage to 355V, set current 1 to 180A, current 2 to 400A, current 3 to 500A, flash displacement to 3mm, forward speed to 0.8mm / s, backward speed to 0.5mm / s;

[0080] The setting time of accelerated burning sub-stage 1 is 5s, the voltage is 360V, the setting current 1 is 180A, the current 2 is 390A, the current 3 is 450A, the burning displacement is 6mm, the forward speed is 1.0mm / s, and the backward speed is 0.3mm / s;

[0081] The setting time of the accelerated burning sub-stage 2 is 3s, the voltage is 390V, the setting current 1 is 250A, the current 2 is 400A, the current 3 is 500A, the burning displacement is 9mm, the forward speed is 1.2mm / s, and the backward speed is 0.1mm / s;

[0082] During the upsetting stage, the charged upsetting time is 1.0s and the upsetting amount is 13.6mm.

[0083] The main function of the forging stage is to continuously apply load to the rail joint during the metal crystallization process of the joint after the rail top forging to enhance the joint quality. To achieve the above purpose, the rail consumption in the forging stage is 4.0mm, the forging time is 2s, the average speed is 2mm / s, and the forging pressure is 80T.

[0084] In the drop hammer test of the rail flash welded joint in this embodiment, the hammer head mass is 1000kg, the drop hammer height is 3.1m, and no fracture occurs after the hammer is dropped 3 times. The maximum deflection is 27.9mm, and the joint quality is high.

[0085] Example 5

[0086] In this embodiment, the chemical composition of the rail is measured to have a carbon mass fraction of 0.59%, a Si mass fraction of 0.63%, a Mn mass fraction of 0.80%, a Cr+Ni+V mass fraction of 0.62%, and P and S ≤ 0.025%.

[0087] In the pre-flash stage, the time is 20s, the voltage is 400V, the setting current 1 is 200A, the current 2 is 350A, the current 3 is 400A, the pre-flash displacement is 5mm, the forward speed is 1mm / s, and the backward speed is 0.5mm / s;

[0088] Flash sub-stage 1, set time to 15s, voltage to 350V, set current 1 to 200A, current 2 to 400A, current 3 to 500A, flash displacement to 6mm, forward speed to 1.7mm / s, backward speed to 0.7mm / s;

[0089] Flash sub-stage 2, set time to 15s, voltage to 340V, set current 1 to 220A, current 2 to 380A, current 3 to 400A, flash displacement to 6mm, forward speed to 1.5mm / s, backward speed to 0.5mm / s;

[0090] Flash sub-stage 3, set time to 10s, voltage to 330V, set current 1 to 300A, current 2 to 450A, current 3 to 500A, flash displacement to 6mm, forward speed to 1.9mm / s, backward speed to 0.9mm / s;

[0091] Flash sub-stage 4, set time to 10s, voltage to 355V, set current 1 to 180A, current 2 to 400A, current 3 to 500A, flash displacement to 3mm, forward speed to 0.8mm / s, backward speed to 0.5mm / s;

[0092] The setting time of accelerated burning sub-stage 1 is 5s, the voltage is 360V, the setting current 1 is 180A, the current 2 is 390A, the current 3 is 450A, the burning displacement is 6mm, the forward speed is 1.0mm / s, and the backward speed is 0.3mm / s;

[0093] The setting time of the accelerated burning sub-stage 2 is 3s, the voltage is 390V, the setting current 1 is 250A, the current 2 is 400A, the current 3 is 500A, the burning displacement is 9mm, the forward speed is 1.2mm / s, and the backward speed is 0.1mm / s;

[0094] During the upsetting stage, the charged upsetting time is 1.0s and the upsetting amount is 14.6mm.

[0095] The main function of the forging stage is to continuously apply load to the rail joint during the metal crystallization process of the joint after the rail top forging to enhance the joint quality. To achieve the above purpose, the rail consumption in the forging stage is 3.0mm, the forging time is 2s, the average speed is 1.5mm / s, and the forging pressure is 70T.

[0096] In the static bending test of the rail flash welded joint in this embodiment, the test load is 2000KN continuously and the maximum deflection is 18.2mm.

[0097] Example 6

[0098] In this embodiment, the chemical composition of the rail is measured to have a carbon mass fraction of 0.56%, a Si mass fraction of 0.58%, a Mn mass fraction of 0.78%, a Cr+Ni+V mass fraction of 0.62%, and P and S ≤ 0.025%.

[0099] In the pre-flash stage, the time is 20s, the voltage is 400V, the setting current 1 is 200A, the current 2 is 350A, the current 3 is 400A, the pre-flash displacement is 5mm, the forward speed is 1mm / s, and the backward speed is 0.5mm / s;

[0100] Flash sub-stage 1, set time to 15s, voltage to 350V, set current 1 to 200A, current 2 to 400A, current 3 to 500A, flash displacement to 6mm, forward speed to 1.7mm / s, backward speed to 0.7mm / s;

[0101] Flash sub-stage 2, set time to 15s, voltage to 340V, set current 1 to 220A, current 2 to 380A, current 3 to 400A, flash displacement to 6mm, forward speed to 1.5mm / s, backward speed to 0.5mm / s;

[0102] Flash sub-stage 3, set time to 10s, voltage to 330V, set current 1 to 300A, current 2 to 450A, current 3 to 500A, flash displacement to 6mm, forward speed to 1.9mm / s, backward speed to 0.9mm / s;

[0103] Flash sub-stage 4, set time to 10s, voltage to 355V, set current 1 to 180A, current 2 to 400A, current 3 to 500A, flash displacement to 3mm, forward speed to 0.8mm / s, backward speed to 0.5mm / s;

[0104] The setting time of accelerated burning sub-stage 1 is 5s, the voltage is 360V, the setting current 1 is 180A, the current 2 is 390A, the current 3 is 450A, the burning displacement is 6mm, the forward speed is 1.0mm / s, and the backward speed is 0.3mm / s;

[0105] The setting time of the accelerated burning sub-stage 2 is 3s, the voltage is 390V, the setting current 1 is 250A, the current 2 is 400A, the current 3 is 500A, the burning displacement is 9mm, the forward speed is 1.2mm / s, and the backward speed is 0.1mm / s;

[0106] During the upsetting stage, the charged upsetting time is 1.0s and the upsetting amount is 14.6mm.

[0107] The main function of the forging stage is to continuously apply load to the rail joint during the metal crystallization process of the joint after the rail top forging to enhance the joint quality. To achieve the above purpose, the rail consumption in the forging stage is 3.0mm, the forging time is 2.0s, the average speed is 1.5mm / s, and the forging pressure is 80T.

[0108] In this embodiment, the rail flash weld joint static bending test is carried out. In this embodiment, the rail flash weld joint static bending test is carried out with a test load of 2000KN and a maximum deflection of 17.1mm.

[0109] Comparative Example 1

[0110] In this embodiment, the chemical composition of the rail is measured to have a carbon mass fraction of 0.59%, a Si mass fraction of 0.63%, a Mn mass fraction of 0.80%, a Cr+Ni+V mass fraction of 0.62%, and P and S ≤ 0.025%.

[0111] In the pre-flash stage, the time is 20s, the voltage is 400V, the setting current 1 is 200A, the current 2 is 350A, the current 3 is 400A, the pre-flash displacement is 5mm, the forward speed is 1mm / s, and the backward speed is 0.5mm / s;

[0112] Flash sub-stage 1, set time to 15s, voltage to 350V, set current 1 to 200A, current 2 to 400A, current 3 to 500A, flash displacement to 6mm, forward speed to 1.7mm / s, backward speed to 0.7mm / s;

[0113] Flash sub-stage 2, set time to 15s, voltage to 340V, set current 1 to 220A, current 2 to 380A, current 3 to 400A, flash displacement to 6mm, forward speed to 1.5mm / s, backward speed to 0.5mm / s;

[0114] Flash sub-stage 3, set time to 10s, voltage to 330V, set current 1 to 300A, current 2 to 450A, current 3 to 500A, flash displacement to 6mm, forward speed to 1.9mm / s, backward speed to 0.9mm / s;

[0115] Flash sub-stage 4, set time to 10s, voltage to 355V, set current 1 to 180A, current 2 to 400A, current 3 to 500A, flash displacement to 3mm, forward speed to 0.8mm / s, backward speed to 0.5mm / s;

[0116] The setting time of accelerated burning sub-stage 1 is 5s, the voltage is 360V, the setting current 1 is 180A, the current 2 is 390A, the current 3 is 450A, the burning displacement is 6mm, the forward speed is 1.0mm / s, and the backward speed is 0.3mm / s;

[0117] The setting time of the accelerated burning sub-stage 2 is 3s, the voltage is 390V, the setting current 1 is 250A, the current 2 is 400A, the current 3 is 500A, the burning displacement is 9mm, the forward speed is 1.2mm / s, and the backward speed is 0.1mm / s;

[0118] During the upsetting stage, the charged upsetting time is 1.0s and the upsetting amount is 12.6mm.

[0119] The main function of the forging stage is to continuously apply load to the rail joint during the metal crystallization process of the joint after the rail top forging to enhance the joint quality. To achieve the above purpose, the rail consumption in the forging stage is 0.5mm, the forging time is 1s, the average speed is 0.5mm / s, and the forging pressure is 45T.

[0120] In the drop hammer test of the rail flash welded joint in this embodiment, the mass of the hammer head is 1000 kg, the drop hammer height is 3.1 m, and the rail breakage occurs at the second drop hammer, which does not meet the standard requirements.

[0121] Comparative Example 2

[0122] In this embodiment, the chemical composition of the rail is measured to have a carbon mass fraction of 0.60%, a Si mass fraction of 0.65%, a Mn mass fraction of 0.82%, a Cr+Ni+V mass fraction of 0.60%, and P and S ≤ 0.025%.

[0123] In the pre-flash stage, the time is 20s, the voltage is 400V, the setting current 1 is 200A, the current 2 is 350A, the current 3 is 400A, the pre-flash displacement is 5mm, the forward speed is 1mm / s, and the backward speed is 0.5mm / s;

[0124] Flash sub-stage 1, set time to 15s, voltage to 350V, set current 1 to 200A, current 2 to 400A, current 3 to 500A, flash displacement to 6mm, forward speed to 1.7mm / s, backward speed to 0.7mm / s;

[0125] Flash sub-stage 2, set time to 15s, voltage to 340V, set current 1 to 220A, current 2 to 380A, current 3 to 400A, flash displacement to 6mm, forward speed to 1.5mm / s, backward speed to 0.5mm / s;

[0126] Flash sub-stage 3, set time to 10s, voltage to 330V, set current 1 to 300A, current 2 to 450A, current 3 to 500A, flash displacement to 6mm, forward speed to 1.9mm / s, backward speed to 0.9mm / s;

[0127] Flash sub-stage 4, set time to 10s, voltage to 355V, set current 1 to 180A, current 2 to 400A, current 3 to 500A, flash displacement to 3mm, forward speed to 0.8mm / s, backward speed to 0.5mm / s;

[0128] The setting time of accelerated burning sub-stage 1 is 5s, the voltage is 360V, the setting current 1 is 180A, the current 2 is 390A, the current 3 is 450A, the burning displacement is 6mm, the forward speed is 1.0mm / s, and the backward speed is 0.3mm / s;

[0129] The setting time of the accelerated burning sub-stage 2 is 3s, the voltage is 390V, the setting current 1 is 250A, the current 2 is 400A, the current 3 is 500A, the burning displacement is 9mm, the forward speed is 1.2mm / s, and the backward speed is 0.1mm / s;

[0130] During the upsetting stage, the live upsetting time is 1.0s and the upsetting amount is 13.4mm.

[0131] The main function of the forging stage is to continuously apply load to the rail joint during the metal crystallization process of the joint after the rail top forging to enhance the joint quality. To achieve the above purpose, the rail consumption in the forging stage is 6.4mm, the forging time is 3.2s, the average speed is 2.0mm / s, and the forging pressure is 90T.

[0132] In the drop hammer test of the rail flash welded joint in this embodiment, the mass of the hammer head is 1000 kg, the drop hammer height is 3.1 m, and the rail breakage occurs at the second drop hammer, which does not meet the standard requirements.

[0133] Comparative Example 3

[0134] In this embodiment, the chemical composition of the rail is measured to have a carbon mass fraction of 0.61%, a Si mass fraction of 0.62%, a Mn mass fraction of 0.85%, a Cr+Ni+V mass fraction of 0.60%, and P and S ≤ 0.025%.

[0135] In the pre-flash stage, the time is 20s, the voltage is 400V, the setting current 1 is 200A, the current 2 is 350A, the current 3 is 400A, the pre-flash displacement is 5mm, the forward speed is 1mm / s, and the backward speed is 0.5mm / s;

[0136] Flash sub-stage 1, set time to 15s, voltage to 350V, set current 1 to 200A, current 2 to 400A, current 3 to 500A, flash displacement to 6mm, forward speed to 1.7mm / s, backward speed to 0.7mm / s;

[0137] Flash sub-stage 2, set time to 15s, voltage to 340V, set current 1 to 220A, current 2 to 380A, current 3 to 400A, flash displacement to 6mm, forward speed to 1.5mm / s, backward speed to 0.5mm / s;

[0138] Flash sub-stage 3, set time to 10s, voltage to 330V, set current 1 to 300A, current 2 to 450A, current 3 to 500A, flash displacement to 6mm, forward speed to 1.9mm / s, backward speed to 0.9mm / s;

[0139] Flash sub-stage 4, set time to 10s, voltage to 355V, set current 1 to 180A, current 2 to 400A, current 3 to 500A, flash displacement to 3mm, forward speed to 0.8mm / s, backward speed to 0.5mm / s;

[0140] The setting time of accelerated burning sub-stage 1 is 5s, the voltage is 360V, the setting current 1 is 180A, the current 2 is 390A, the current 3 is 450A, the burning displacement is 6mm, the forward speed is 1.0mm / s, and the backward speed is 0.3mm / s;

[0141] The setting time of the accelerated burning sub-stage 2 is 3s, the voltage is 390V, the setting current 1 is 250A, the current 2 is 400A, the current 3 is 500A, the burning displacement is 9mm, the forward speed is 1.2mm / s, and the backward speed is 0.1mm / s;

[0142] During the upsetting stage, the charged upsetting time is 1.0s and the upsetting amount is 13.2mm.

[0143] The main function of the forging stage is to continuously apply load to the rail joint during the metal crystallization process of the joint after the rail top forging to enhance the joint quality. To achieve the above purpose, the rail consumption in the forging stage is 5mm, the forging time is 2s, the average speed is 2.5mm / s, and the forging pressure is 85T.

[0144] In the static bending test of the rail flash welded joint in this embodiment, fracture occurred when the test load was 1731 KN, and the fracture surface was relatively flat.

[0145] The above embodiments only express the implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the present invention. It should be pointed out that, for those of ordinary skill in the art, several modifications and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the present invention patent shall be subject to the attached claims.

Claims

1. A method for improving the quality of flash welded joints of medium carbon low alloy rails, characterized in that: The method comprises performing pre-flashing, flashing, accelerated burning, upsetting and forging on the rail in sequence, wherein the rail consumption in the forging stage is 2.0 mm to 4.0 mm, the forging time is 2.0 s to 3.0 s, the average speed is 0.80 mm / s to 2.0 mm / s, and the forging pressure is 50 T to 80 T. In the pre-flash stage: The setting time is 15s~30s, the voltage is 370V~400V, the setting current 1 is 180A~220A, the current 2 is 270A~400A, the current 3 is 350A~450A, the pre-flash displacement is 3mm~7mm, the forward speed is 1 mm / s~1.5mm / s, and the backward speed is 0.5mm / s~1.2mm / s; During the flash phase: Flash sub-stage 1: set time to 10s-25s, voltage to 330V-360V, current 1 to 200A-280A, current 2 to 350A-500A, current 3 to 450A-550A, pre-flash displacement to 6mm-12mm, forward speed to 1.2mm / s-1.7mm / s, backward speed to 0.5mm / s-1.2mm / s; Flash sub-stage 2: set time to 10s-25s, voltage to 300V-340V, set current 1 to 220A-250A, current 2 to 310A-460A, current 3 to 400A-530A, pre-flash displacement to 6mm-10mm, forward speed to 1.5mm / s-2.5mm / s, backward speed to 0.5mm / s-1.2mm / s; Flash sub-stage 3: set time to 5s-15s, voltage to 300V-330V, set current 1 to 230A-300A, current 2 to 300A-450A, current 3 to 380A-520A, pre-flash displacement to 3mm-6mm, forward speed to 1.3mm / s-2.3mm / s, backward speed to 0.5mm / s-1.5mm / s; Flash sub-stage 4: set time to 5s~15s, voltage to 320V~360V, set current 1 to 150A~300A, current 2 to 300A~400A, current 3 to 350A~500A, pre-flash displacement to 3mm~5mm, forward speed to 0.6mm / s~1.3mm / s, and backward speed to 0.3mm / s~1.0mm / s.

2. The method according to claim 1, characterized in that The medium carbon low alloy rail contains the following components in mass fraction: C: 0.50% to 0.63%, Si: 0.30% to 0.60%, Mn: 0.55% to 0.80%, Cr+Ni+V: 0.30% to 0.9%, P, S≤0.025%, and the balance is Fe and unavoidable impurities.

3. The method according to claim 1, characterized in that In the accelerated burning stage: Accelerated burning sub-stage 1: set the time to 3s~8s, the voltage to 350V~380V, set current 1 to 150A~300A, current 2 to 350A~500A, current 3 to 450A~550A, pre-flash displacement to 5mm~10mm, forward speed to 0.6mm / s~1.3mm / s, and backward speed to 0.3mm / s~0.8mm / s; Accelerated burning sub-stage 2: the set time is 1s~5s, the voltage is 360V~400V, the set current 1 is 200A~300A, the current 2 is 350A~500A, the current 3 is 450A~550A, the pre-flash displacement is 5mm~10mm, the forward speed is 0.6mm / s~1.3mm / s, and the backward speed is 0.1mm / s~0.4mm / s.

4. The method according to claim 1, characterized in that: In the upset forging stage, the charged upset forging time is set to 0.1s to 2.0s, and the upset amount is set to 12mm to 15.0mm.

5. The method according to claim 1, characterized in that After the forging stage, the flash welded joint was left in air to cool naturally to room temperature.