A slag-forming agent for silicon mud smelting and preparation method thereof
By using slag-making agent for silicon sludge smelting prepared with raw materials such as calcium oxide, calcium carbonate, barium sulfate, magnesium carbonate, etc., the problem of silica adhesion in silicon smelting is solved, the yield and recycling efficiency of silicon sludge are improved, and the Efficient utilization of resources and environmental protection.
Patent Information
- Application Number
- CN202211519986.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-30
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-11-30
AI Technical Summary
In the prior art, due to the existence of silica during the smelting process, the furnace wall adherence is difficult to clean, and traditional slag-making agents are not suitable, resulting in waste of resources and environmental pollution, and the recycling efficiency of silicon sludge is low.
The slag-making agent for smelting of silicon sludge prepared by raw materials such as calcium oxide, calcium carbonate, barium sulfate, magnesium carbonate, etc. is prepared by stirring, drying, crushing and screening, and is added to the silicon sludge for smelting, and is separated by chemical reactions. Slag and liquid silicon to control moisture and particle size.
It effectively improves the yield and smelting effect of silicon sludge, avoids resource waste and environmental pollution, reduces treatment costs, and improves the recycling rate of silicon resources.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of silicon mud smelting, and in particular to a slag-forming agent for silicon mud smelting and a preparation method thereof. Background Art
[0002] Silicon mud is a process waste generated by cutting silicon wafers during the production process of solar photovoltaic panels. With the rapid development of the photovoltaic (PV) industry, the demand for solar-grade silicon has increased dramatically as it is the main photoelectric conversion material. Crystalline silicon wafers are the core material of solar cells, accounting for more than 90% of photovoltaic energy materials. However, a large amount of silicon powder chips will be generated during the silicon wafer cutting process, accounting for 35% to 40% of silicon ingots. Based on the annual production of 342,000 tons of polysilicon in 2019 alone, 137,000 tons of waste silicon powder will be generated, and the output of cutting waste is huge. Improper disposal of large amounts of silicon mud not only occupies land, but also causes waste of resources and environmental pollution. With the vigorous promotion of global waste comprehensive utilization policies and the urgent need for environmental protection, the reuse of valuable waste resources has gradually received more and more attention.
[0003] In the prior art, the recycling and treatment of silicon mud mostly adopts medium frequency electric furnace for smelting. The purchased diamond wire cutting silicon mud is directly dried. After the moisture content of the silicon mud is reduced to about 5%, it is directly put into the medium frequency electric furnace for smelting production. After the silicon mud is melted into silicon liquid in large quantities, the solid slag produced is poured out of the furnace, and then the temperature is continued to rise and the dried silicon mud is repeatedly added until the furnace is full. Then, all the silicon liquid and slag liquid are poured into the mold to prepare metallic silicon to recover silicon resources.
[0004] Since silicon mud contains a large amount of silicon dioxide, the melting temperature of silicon mud is increased during the smelting process. At the same time, silicon dioxide becomes sticky and sticks to the furnace wall after melting, which is difficult to clean. The furnace body can be completely covered with sticky paste after 2-3 furnaces. The traditional slag-making agent refining method is alkaline earth metal oxides. The main smelting purpose is to replace Fe, Ca, Al and other metal ions in silicon melt to achieve the purpose of purification. It is not suitable for use in silicon mud smelting. Summary of the invention
[0005] In order to solve the existing silicon mud smelting problems, the present invention provides a slag-forming agent for silicon mud smelting and a preparation method thereof. The first purpose of the present invention is to provide a slag-forming agent for silicon mud smelting; the second purpose is to provide a preparation method of the slag-forming agent for silicon mud smelting; the third purpose is to provide the application of the slag-forming agent for silicon mud smelting.
[0006] The technical solution adopted by the present invention is:
[0007] A slag-making agent for silicon mud smelting comprises the following raw materials in percentage by mass:
[0008] Calcium oxide 20-30%, calcium carbonate 40-50%, barium sulfate 10%, magnesium carbonate 10-20%, the total of all components is 100%.
[0009] A method for preparing the above-mentioned slag-forming agent for silicon mud smelting comprises the following steps:
[0010] Step 1: prepare commercially available calcium oxide, calcium carbonate, barium sulfate, and magnesium carbonate according to the following mass percentages: 20-30% calcium oxide, 40-50% calcium carbonate, 10% barium sulfate, and 10-20% magnesium carbonate, the total of which is 100%;
[0011] Step 2, stirring the components in step 1 together, mixing evenly, and then drying at a constant temperature of 100-350° C. for 1-3 hours, controlling the moisture content to less than 0.5%, to obtain a mixture;
[0012] Step three, crushing, screening, cooling and packaging the mixture.
[0013] Furthermore, in step 2, the constant temperature drying temperature is 180° C. and the drying time is 2 hours.
[0014] Furthermore, in step three, the crushing and screening particle size is controlled at 20 mesh-80 mesh.
[0015] Furthermore, in step three, the packaging process is vacuum bag sealing packaging.
[0016] Furthermore, the added weight of the slag-forming agent for silicon mud smelting is 3% to 5% of the weight of the silicon mud.
[0017] A silicon mud smelting method adopts the above-mentioned slag-forming agent for silicon mud smelting as a slag-forming agent to carry out silicon mud smelting.
[0018] Furthermore, the weight of the slag-forming agent added for silicon mud smelting is 3% to 5% of the weight of the silicon mud; the adding method is: adding after the silicon mud is melted and fills the furnace, or sprinkling on the surface of the silicon mud and shoveling it into the furnace together with the silicon mud for smelting, or mixing with the silicon mud and then shoveling it into the furnace for smelting.
[0019] The beneficial effects of the present invention are:
[0020] 1. The slag-making agent for smelting effectively avoids waste of resources and environmental pollution, is conducive to the recycling of silicon mud, and reduces processing costs and hazardous waste inventory.
[0021] 2. The slag-forming agent for smelting solves the problem that the traditional refining slag-forming agent is not suitable for silicon mud smelting. After the silicon mud is smelted, the slag and silicon liquid are separated well, the silicon mud yield is high, and the smelting slag does not stick to the furnace wall, thereby utilizing recycled silicon resources. DETAILED DESCRIPTION
[0022] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] In order to make the purpose, technical solution and beneficial effects of the present invention clearer, the preferred cases of the present invention are described in detail below:
[0024] Implementation Case 1
[0025] A. Prepare commercially available calcium oxide, calcium carbonate, barium sulfate and magnesium carbonate according to the following mass percentages: 25 parts of calcium oxide, 45 parts of calcium carbonate, 10 parts of barium sulfate and 20 parts of magnesium carbonate, the sum of the above components being 100%;
[0026] B. Stir and mix the components in step A, and dry the mixture at a constant temperature of 100-350°C for 1-3 hours to control the moisture content to less than 0.5%;
[0027] C. Crushing and screening the raw materials in step B, and controlling the particle size to 20-80 mesh;
[0028] D. After the operation of step C is completed and the temperature is lowered to 50-60°C, vacuum seal and pack into bags, each bag weighing 2-5 kg.
[0029] After the silicon mud in the furnace is melted and fills the furnace, the prepared slag-forming agent for smelting is sprinkled into the furnace at a ratio of 3% of the weight of the silicon mud; since the mud contains relatively high levels of metallic silicon and silicon dioxide, the melting point of metallic silicon is 1410°C, and the melting point of silicon dioxide is 1600-1700°C; during the smelting process in the medium frequency furnace, the silicon liquid containing silicon dioxide has a large viscosity and poor thermal conductivity, and the furnace building materials are mostly made of silicon dioxide. Due to the high local temperature, part of the molten silicon dioxide in the liquid silicon is sticky and easily adheres to the furnace wall. The invented slag-forming agent reacts with the silicon dioxide in the silicon mud to generate high-melting-point, low-density silicates and subsilicates, which are separated from the metallic silicon, thereby improving the separation of slag and silicon liquid.
[0030] The reaction chemical equation is as follows:
[0031] SiO2+CaO==CaSiO3
[0032] SiO2+CaCO3==CaSiO3+CO2↑
[0033] SiO2+BaSO4==BaSiO3+SO3↑
[0034] SiO2+MgCO3==MgSiO3+CO2↑
[0035] After actual testing, it was found that the separation effect of slag and silicon liquid was good. With the slag-forming agent and the use method, the silicon mud yield was 58%.
[0036] Implementation Case 2
[0037] A. Prepare commercially available calcium oxide, calcium carbonate, barium sulfate and magnesium carbonate according to the following mass percentages: 30 parts of calcium oxide, 40 parts of calcium carbonate, 10 parts of barium sulfate and 20 parts of magnesium carbonate, the sum of the above components being 100%;
[0038] B. Stir and mix the components in step A, and dry the mixture at a constant temperature of 100-350°C for 1-3 hours to control the moisture content to less than 0.5%;
[0039] C. Crushing and screening the raw materials in step B, and controlling the particle size to 20-80 mesh;
[0040] D. After the operation of step C is completed and the temperature is lowered to 50-60°C, vacuum seal and bag the mixture, with a bag weight of 2-5 kg.
[0041] The prepared slag-making agent for smelting is sprinkled on the surface of the silicon mud at a ratio of 5% of the weight of the silicon mud, and shoveled into the furnace for smelting; after actual testing, the silicon mud yield is 62%.
[0042] During the smelting process, the medium frequency furnace is relatively deep at 1200-1600mm, and the effective smelting coils are mainly concentrated in the middle and lower parts of 200-800mm. The metallic silicon in the silicon mud is not magnetic when solid and cannot be heated. Heat can only be transferred through thermal radiation from the crucible, and it is very easy to oxidize in the process.
[0043] The prepared slag-forming agent for smelting is mixed with the materials and added together. During the melting process of metallic silicon, silicon dioxide first reacts with the slag-forming agent it comes into contact with and separates from the silicon liquid. After the molten silicon liquid is magnetic, it rolls and stirs under the action of the magnetic field to continue melting the silicon mud. This process is repeated, which speeds up the melting speed of the silicon mud, reduces oxidation, and ultimately increases the silicon mud yield.
[0044] Implementation Case 3
[0045] A. Prepare commercially available calcium oxide, calcium carbonate, barium sulfate and magnesium carbonate according to the following mass percentages: 25 parts of calcium oxide, 45 parts of calcium carbonate, 10 parts of barium sulfate and 20 parts of magnesium carbonate, the sum of the above components being 100%;
[0046] B. Stir and mix the components in step A, and dry the mixture at a constant temperature of 100-350°C for 1-3 hours to control the moisture content to less than 0.5%;
[0047] C. Crush and screen the raw materials in step B, and control the particle size to 20-80 mesh
[0048] D. After the operation of step C is completed and the temperature is lowered to 50-60°C, vacuum seal and bag the mixture, with a bag weight of 2-5 kg.
[0049] The prepared slag-making agent for smelting is mixed into the silicon mud at a ratio of 5% by weight of the silicon mud, stirred evenly, and shoveled into the furnace for smelting; after actual testing, the silicon mud yield was 68%.
[0050] During the smelting process, the medium frequency furnace is relatively deep at 1200-1600mm, and the effective smelting coils are mainly concentrated in the middle and lower parts of 200-800mm. The metallic silicon in the silicon mud is not magnetic when solid and cannot be heated. Heat can only be transferred through thermal radiation from the crucible, and it is very easy to oxidize in the process.
[0051] Stirring the prepared slag-forming agent for smelting with the material is more thorough than sprinkling the slag-forming agent on the surface of silicon mud. Evenly stirring the slag-forming agent and silicon mud will shorten the contact time between silicon dioxide and slag-forming agent during the melting process of metallic silicon, resulting in less oxidation and thus a higher silicon mud yield.
[0052] Example 4
[0053] A. Prepare commercially available calcium oxide, calcium carbonate, barium sulfate and magnesium carbonate according to the following mass percentages: 50 parts of calcium oxide, 40 parts of silicon dioxide, and 10 parts of aluminum oxide, where the sum of the above components of aluminum oxide is 100%;
[0054] B. The components of step A are stirred and mixed to obtain a traditional slag-making agent.
[0055] The traditional slag-making agent is mixed into the silicon mud at a ratio of 5%, stirred evenly, and shoveled into the furnace for smelting; after actual testing, the silicon mud yield is 40%.
[0056] By comparing Example 1, Example 2, Example 3 with Example 4, it is found that the main impurity in silicon mud is silicon dioxide, which is very easy to oxidize during the smelting process. Only by removing silicon dioxide and shortening the smelting time can the purpose of high efficiency and high quality be achieved. In this embodiment, calcium oxide, calcium carbonate, barium sulfate and magnesium carbonate are used to prepare the smelting slag-making agent, and the silicon mud yield is 18% to 28% higher than that of the traditional slag-making agent.
[0057] Finally, it should be noted that the above preferred embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail through the above preferred embodiments, those skilled in the art should understand that various changes can be made in form and details without departing from the scope defined by the claims of the present invention.
Claims
1. A slag-making agent for silicon mud smelting, characterized in that: The following raw materials are used in percentage by mass: Calcium oxide 20-30%, calcium carbonate 40-50%, barium sulfate 10%, magnesium carbonate 10-20%, the total of all components is 100%.
2. The method for preparing the slag-making agent for silicon mud smelting according to claim 1, characterized in that: The following steps are involved: Step 1: prepare commercially available calcium oxide, calcium carbonate, barium sulfate, and magnesium carbonate according to the following mass percentages: 20-30% calcium oxide, 40-50% calcium carbonate, 10% barium sulfate, and 10-20% magnesium carbonate, the total of which is 100%; Step 2, stirring the components in step 1 together, mixing evenly, and then drying at a constant temperature of 100-350° C. for 1-3 hours, controlling the moisture content to less than 0.5%, to obtain a mixture; Step three, crushing, screening, cooling and packaging the mixture.
3. The method for preparing a slag-forming agent for silicon mud smelting according to claim 2, characterized in that: In step 2, the constant temperature drying temperature is 180° C. and the drying time is 2 hours.
4. The method for preparing a slag-forming agent for silicon mud smelting according to claim 2, characterized in that: In step three, the crushing and screening particle size is controlled at 20 mesh-80 mesh.
5. The method for preparing a slag-forming agent for silicon mud smelting according to claim 2, characterized in that: In step three, the packaging process is vacuum bag sealing packaging.
6. The slag-making agent for silicon mud smelting according to claim 1, characterized in that: The added weight of the slag-forming agent for silicon mud smelting is 3% to 5% of the weight of the silicon mud.
7. A silicon mud smelting method, characterized in that: The silicon mud smelting method uses the slag-forming agent for silicon mud smelting according to claim 1 as a slag-forming agent to carry out silicon mud smelting.
8. The silicon mud smelting method according to claim 7, characterized in that: The added weight of slag-making agent for silica mud smelting is 3% to 5% of the weight of silica mud; The adding method is: adding after the silicon mud is melted and fills the furnace, or sprinkling on the silicon mud surface and shoveling it into the furnace together with the silicon mud for smelting, or mixing with the silicon mud and then shoveling it into the furnace for smelting.