A B / P / N ternary synergistic flame retardant and its preparation method and application
Through the preparation method of boron, phosphorus and nitrogen combined with the hydrophobic modification of polyethyleneimine, the problems of insufficient flame retardant performance of cotton fabrics and water solubility of flame retardant are solved, achieving efficient and environmentally friendly flame retardant effect, improving the The flame retardant properties of cotton fabrics and reduce the amount of use, complying with green environmental protection standards.
Patent Information
- Application Number
- CN202211386646.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-07
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-11-07
AI Technical Summary
In the prior art, the flame retardant performance of cotton fabrics is insufficient, and traditional flame retardants have water solubility problems during the finishing process, which is difficult to meet the requirements of efficient flame retardant, and some flame retardants have biotoxicity and environmental pollution risks.
The preparation method of boron, phosphorus and nitrogen combined with flame retardant is adopted. By esterification of hydroxyl groups, boric acid and phosphoric acid, the ionic characteristics of polyethyleneimine and hydrophobic chain segments are combined to reduce the water solubility of the flame retardant and regulate the flame retardant elements. The content and ratio of the product are prepared to produce green and environmentally friendly high-efficiency flame-retardant cotton fabrics.
It realizes the efficient and environmentally friendly flame retardant effect of cotton fabrics, improves flame retardant performance, reduces the use of flame retardant, and the raw materials and processes meet the requirements of green and environmental protection, and has broad application prospects.
Smart Images

Figure BDA0003930153310000031 
Figure BDA0003930153310000041 
Figure BDA0003930153310000101
Abstract
Description
Technical Field
[0001] The invention belongs to the field of textile technology, and specifically relates to a B / P / N ternary synergistic flame retardant and a preparation method and application thereof. Background Art
[0002] Cotton fabrics have excellent properties such as softness, breathability, moisture absorption, comfort, easy dyeing and processing, and have broad application prospects in the fields of clothing, medical treatment, packaging, and home furnishing. However, the LOI of cotton fabrics is about 18%, which is very easy to burn, posing a major hidden danger to people's life safety and property. Therefore, it is necessary to develop new flame retardants to perform flame retardant finishing on them and improve their flame retardant properties.
[0003] Flame retardants for cotton are divided into three categories: organic, inorganic, and organic-inorganic composites. Organic flame retardants have the following characteristics: (1) Low dosage and excellent flame retardant properties. (2) Easy covalent grafting to achieve flame retardant durability. However, some organic flame retardants have been proven to be biotoxic, such as halogen flame retardants, which have been banned. The commercial flame retardants Pyrovatex CP and Proban have formaldehyde release problems during finishing, storage and use, and are gradually being eliminated. Therefore, the development of green and environmentally friendly biomass-based textile flame retardants is the focus of current research. Glucamine is derived from glucose and is an amino sugar that is often used in the fields of pharmaceuticals, food and cosmetics. It has the advantages of high safety and biodegradability. In addition, glucamine is easy to obtain, contains N elements, and has many hydroxyl functional groups for chemical modification. It is a good flame retardant modification matrix.
[0004] Esterification of phosphoric acid and polyols is a popular method for preparing flame retardants. This method can not only select biomass polyols to meet environmental protection requirements, but also use active ammonium phosphate groups to give cotton fabrics washability. However, studies have shown that in the synthesis process of phosphate ester polyols, the efficiency of phosphate esterification is low and it is difficult to have efficient flame retardant properties. Some researchers have used phosphoric acid and sorbitol to prepare sorbitol-based flame retardants with a yield of 66%.
[0005] However, in order to further enhance the flame retardant effect of phosphorus-nitrogen flame retardants, boron-phosphorus-nitrogen synergistic flame retardant can be used. Boron-based flame retardants mainly include inorganic borates such as zinc borate, borax, calcium metaborate, sodium metaborate, and a few organic boric acid esters, which have the advantages of good thermal stability, low toxicity, smoke elimination, low toxicity, and easy availability of raw materials. It has been reported that boron-based flame retardants can be compounded with nitrogen-based or phosphorus-based flame retardants to achieve a synergistic flame retardant effect. At present, although there are reports on B / P / N ternary synergistic flame retardants, there have been no reports at home and abroad on the further grafting reaction of boric acid and phosphorylated meglumine to prepare a structure-controllable B / P / N ternary synergistic flame retardant.
[0006] So far, a variety of finishing methods have been developed to prepare flame-retardant cotton fabrics, including impregnation, padding-drying-curing, sol-gel, layer-by-layer self-assembly, etc. The common purpose of these methods is to load or graft the flame retardant on the surface of cotton fibers. Among them, padding-drying-baking is easy to operate and can easily make cotton fabrics achieve efficient flame retardant functions. However, due to the water solubility of flame retardants, a high concentration of flame retardant finishing liquid needs to be prepared during the finishing process to meet the flame retardant performance, which is difficult to meet the requirements of high efficiency. Summary of the invention
[0007] In order to solve the problems existing in the prior art, the present invention provides a green, environmentally friendly and efficient B / P / N ternary synergistic flame retardant and its preparation method and application. The preparation method utilizes the synergistic flame retardant mechanism of boron, phosphorus and nitrogen and the strategy of polyethyleneimine to reduce the water solubility of the flame retardant to prepare a green, environmentally friendly and efficient flame retardant cotton fabric.
[0008] The invention adopts the idea of synergistic flame retardancy of boron, phosphorus and nitrogen and the strategy of reducing water solubility to achieve efficient and environmentally friendly flame retardant effect of cotton fabric. By utilizing the esterification reaction of hydroxyl with boric acid and phosphoric acid, the content and ratio of flame retardant elements in the flame retardant are regulated to achieve high flame retardancy requirements; further utilizing the ionic characteristics and hydrophobic segments of polyethyleneimine to reduce the water solubility of the flame retardant, meet the requirements of efficient flame retardancy, and have broad application prospects.
[0009] A method for preparing a B / P / N ternary synergistic flame retardant comprises the following steps:
[0010] (1) meglumine and phosphoric acid react in a solvent to obtain solution A;
[0011] (2) adding boric acid to solution A to react and obtain solution B;
[0012] (3) adding urea to solution B for reaction, and obtaining the B / P / N ternary synergistic flame retardant after the reaction is completed.
[0013] The reaction process in the above preparation method is as follows:
[0014]
[0015] However, due to the low efficiency of phosphation, not all R
[0016] Phosphoric acid first undergoes an esterification reaction with part of the hydroxyl groups on meglumine to prepare phosphorylated meglumine; after adding boric acid, boric acid undergoes an esterification reaction with all or part of the hydroxyl groups on the phosphorylated meglumine to obtain boric acid and phosphorylated meglumine; and then urea is added to react to prepare ammonium phosphate, i.e., a B / P / N ternary synergistic flame retardant.
[0017] Preferably, the molar ratio of meglumine to phosphoric acid is 1:(3-10). Due to the low efficiency of phosphoric acid esterification, adding too much phosphoric acid does not improve the esterification rate, but increases the cost and the occurrence of side reactions. Therefore, as a further preference, the molar ratio of meglumine to phosphoric acid is 1:5.
[0018] Preferably, the molar ratio of meglumine to boric acid is 1:(1-5), more preferably 1:(3-5), and even more preferably 1:(3.5-4.5).
[0019] Preferably, the molar ratio of phosphoric acid to urea is 1:(0.5 to 1.1). More preferably, it is 1:
[0020] (0.9~1.1).
[0021] Preferably, the solvent is one or more of N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO), and dichloromethane, and more preferably an anhydrous N,N-dimethylformamide (DMF) solution.
[0022] Preferably, in step (1), the reaction temperature of meglumine and phosphoric acid is 120-140°C, and the reaction time is 1-3 hours. More preferably, the reaction temperature is 125-135°C, and the reaction time is 1.5-2 hours.
[0023] Preferably, in step (2), the reaction temperature after adding boric acid is 110-150°C, and the reaction time is 1-3 hours. More preferably, the reaction temperature is 110-140°C, and the reaction time is 1.5-2.5 hours. More preferably, the reaction temperature is 125-140°C.
[0024] Preferably, in step (3), the reaction temperature after adding urea is 110-130°C, and the reaction time is 0.5-2h. More preferably, the reaction temperature is 115-125°C, and the reaction time is 0.5-1.5h.
[0025] Preferably, in step (3), after the reaction is completed, the following post-treatment is performed:
[0026] The reaction product was washed with ethanol for several times to remove unreacted raw materials, and dried at 60-80° C. to obtain a B / P / N ternary synergistic flame retardant.
[0027] A B / P / N ternary synergistic flame retardant is prepared by any of the preparation methods described above.
[0028] The present invention also provides a flame retardant finishing liquid, in which the concentration of the flame retardant is 20 to 200 g / L;
[0029] The flame retardant is the B / P / N ternary synergistic flame retardant mentioned above.
[0030] Preferably, in the flame retardant finishing liquid, the concentration of the B / P / N ternary synergistic flame retardant is 20 to 100 g / L.
[0031] Preferably, the flame retardant finishing liquid is obtained by mixing an aqueous solution of the B / P / N ternary synergistic flame retardant and an aqueous solution of polyethyleneimine (PEI) and reacting the mixture. The reaction process is as follows:
[0032]
[0033] During the above reaction process, the ionized amino group in polyethyleneimine replaces the ammonium ion of ammonium phosphate in the flame retardant, an ion exchange reaction occurs, a "cross-linking point" is formed between the two, and ammonia gas is released at the same time, thereby reducing the water solubility of the flame retardant.
[0034] As a further preference, in the flame retardant finishing liquid, the mass ratio of the B / P / N ternary synergistic flame retardant to the polyethyleneimine is 10:(0.2-2). More preferably, it is 10:(0.5-1.5). More preferably, it is 10:(0.75-1.25).
[0035] As a further preferred embodiment, the concentration of the B / P / N ternary synergistic flame retardant aqueous solution is 10 to 200 g / L;
[0036] The concentration of the polyethyleneimine aqueous solution is 1 to 20 g / L.
[0037] As a further preference, the reaction temperature of the mixed reaction of the aqueous solution of the B / P / N ternary synergistic flame retardant and the polyethyleneimine aqueous solution is 25-70°C, and the reaction time is 10-60 minutes. More preferably, the reaction temperature is 40-60°C, and the reaction time is 30-50 minutes.
[0038] A use of any of the flame retardant finishing liquids described above in flame retardant treatment of cotton fabrics.
[0039] Specifically, the cotton fabric is immersed in the flame retardant finishing liquid for a set time, and the green, environmentally friendly, efficient and durable flame retardant cotton fabric is obtained through padding and drying.
[0040] Preferably, the immersion temperature is 25 to 70° C., and the immersion time is 0 to 40 min. More preferably, the immersion temperature is 60° C., and the immersion time is 20 min.
[0041] Preferably, the bath ratio of the cotton fabric to the flame retardant finishing liquid is 1:(20-60), and more preferably 1:(40-60).
[0042] Preferably, the padding method is double-dipping and double-padding, and the liquid carrying rate is 80 to 100%.
[0043] Preferably, the drying temperature is 60-80°C and the drying time is 10-50 min. More preferably, the drying temperature is 70-80°C and the drying time is 20-40 min.
[0044] Compared with the prior art, the present invention has the following beneficial effects:
[0045] (1) The preparation method of the present invention uses amino polyol as a matrix, and improves the flame retardancy of phosphorylated polyol through the esterification of boric acid and phosphoric acid, so that the prepared B / P / N ternary synergistic flame retardant has excellent flame retardancy. In addition, the ionized amino group in polyethyleneimine can undergo a substitution reaction with the ammonium ion of ammonium phosphate in the B / P / N ternary synergistic flame retardant to reduce the water solubility of the flame retardant. Then, the hydrophobic force is used to achieve a high flame retardant effect at a low concentration of the flame retardant.
[0046] (2) The B / P / N ternary synergistic flame retardant prepared by the present invention has a controllable structure, an adjustable ratio of the flame retardant elements phosphorus, boron and nitrogen, and a synergistic flame retardant effect between the three elements. When the flame retardant is used alone to finish the fabric, the LOI value of the cotton fabric treated with a flame retardant concentration of 200g / L in the flame retardant finishing liquid reaches 40.3%, which is 128.9% higher than that of the unfinished cotton fabric, indicating that the B / P / N ternary synergistic flame retardant prepared by the present invention has an excellent flame retardant effect.
[0047] After further hydrophobic modification using polyethyleneimine, the flame retardant finishing liquid contained 100 g / L of B / P / N ternary synergistic flame retardant, and the LOI of the cotton fabric finished with it was 40.1%. This shows that hydrophobic modification of the above flame retardant using polyethyleneimine can effectively reduce the amount of flame retardant used, achieving the purpose of efficient flame retardancy.
[0048] (3) The reaction raw materials and reagents used in the preparation method of the present invention meet the requirements of green environmental protection and are low in price; the preparation method is simple and convenient, the reaction conditions are mild, the controllability is strong, and the reproducibility is good; it has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] Figure 1 This is the infrared spectrum of the B / P / N ternary synergistic flame retardant prepared when the boric acid reaction temperature is 130° C. in Example 2;
[0050] Figure 2 This is a graph showing the precipitation change of the flame retardant finishing liquid prepared in Example 1 over time. DETAILED DESCRIPTION
[0051] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only intended to illustrate the present invention and are not intended to limit the scope of the present invention. After reading the content taught by the present invention, those skilled in the art may make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0052] Example 1: Selection of the molar ratio of meglumine to boric acid
[0053] (1) 6 portions of 75 mL DMF were placed in 6 flasks for standby use, 0.05 mol of meglumine and 0.25 mol of phosphoric acid were added to the six portions of DMF, and the mixture was reacted at 130°C for 2 h. Boric acid (wherein the molar mass of boric acid was 0 mol, 0.05 mol, 0.10 mol, 0.15 mol, 0.20 mol, and 0.25 mol) was then added to the six flasks, and the mixture was reacted at 130°C for 2 h. Finally, 0.25 mol of urea was added to the six flasks, and the mixture was reacted at 120°C for 1 h. The reaction products were washed with ethanol several times and dried at 80°C to obtain 6 B / P / N ternary synergistic flame retardants, which were respectively recorded as 1#, 2#, 3#, 4#, 5#, and 6# flame retardants.
[0054] (2) The above six B / P / N ternary synergistic flame retardants were prepared into aqueous solutions for standby use, and six portions of the same PEI aqueous solution were prepared for standby use. The six portions of PEI aqueous solution were poured into the six flame retardant aqueous solutions (the concentration of B / P / N ternary synergistic flame retardant in the six mixed solutions was 100 g / L, and the concentration of PEI was 10 g / L), and the mixed solutions were reacted at 50°C for 40 minutes to obtain six different flame retardant finishing solutions, which were respectively recorded as 1#, 2#, 3#, 4#, 5#, and 6# flame retardant finishing solutions.
[0055] (3) Six pieces of cotton fabrics were immersed in the six flame retardant finishing liquids prepared one by one, the immersion temperature was 60°C, the immersion time was 20 min, the bath ratio was 1:20, two immersions and two rollings were performed, the liquid carrying rate was kept at 100%, and six different flame retardant cotton fabrics were obtained by drying at 80°C for 30 min, which were respectively recorded as 1#, 2#, 3#, 4#, 5#, and 6# flame retardant cotton fabrics.
[0056] In order to explore the effect of boric acid content on the flame retardant properties of flame retardants, the limiting oxygen index (LOI) of 6 flame retardant cotton fabrics (reference standard is GB / T5454-1997 "Determination of Combustion Performance of Textiles-Determination of Oxygen Index") was tested, and the results are shown in Table 1.
[0057] Table 1 Effect of different boric acid dosage on flame retardant properties of cotton fabrics treated with flame retardants
[0058] Flame retardant cotton fabric number Molar ratio of meglumine to boric acid LOI / % 1# 1:0 33.7 2# 1:1 35.5 3# 1:2 36.4 4# 1:3 38.2 5# 1:4 40.1 6# 1:5 39.8
[0059] As shown in Table 1, the addition of boric acid can improve the flame retardant properties of phosphorylated meglumine, and with the increase of the amount of boric acid, the LOI of the finished cotton fabric increases accordingly. When the molar ratio of meglumine to boric acid is 1:4 (5#), the LOI reaches a maximum of 40.1%. When too much boric acid is added (6#), the degree of side reactions in the system increases, resulting in a slight decrease in the LOI value.
[0060] Embodiment 2:
[0061] According to the preparation method in Example 1, 5#B / P / N ternary synergistic flame retardant was prepared and formulated into a flame retardant finishing liquid with a concentration of 200 g / L. The flame retardant cotton fabric was prepared using the cotton fabric treatment conditions in step (3) of Example 1, and the limiting oxygen index (LOI) of the flame retardant cotton fabric was tested, and the LOI was 40.3%.
[0062] Another untreated cotton fabric (blank control) was directly tested and its LOI was 17.6%. The LOI of the flame-retardant cotton fabric prepared in this example is significantly higher than the LOI of the untreated cotton fabric, indicating that the flame retardant prepared in this example has excellent flame retardant properties.
[0063] The LOI of the flame retardant cotton fabric prepared in this embodiment is similar to the LOI of the 5# flame retardant cotton fabric in Example 1, but the concentration of the flame retardant in the flame retardant finishing liquid used in this embodiment (200 g / L) is higher than the concentration of the flame retardant in the 5# flame retardant finishing liquid (100 g / L); it shows that the use of polyethyleneimine for appropriate hydrophobic treatment of the flame retardant can effectively reduce the use of the flame retardant, while achieving a better flame retardant effect, greatly reducing the cost of use.
[0064] Example 3: Selection of Boric Acid Reaction Temperature
[0065] (1) 5 portions of 75 mL DMF were placed in five flasks for standby use. 0.05 mol of meglumine and 0.25 mol of phosphoric acid were added to the 5 portions of DMF and reacted at 130°C for 2 h. Subsequently, 0.2 mol of boric acid was added to the 5 flasks and reacted at 110°C, 120°C, 130°C, 140°C, and 150°C for 2 h. Finally, 0.25 mol of urea was added to the five flasks and reacted at 120°C for 1 h. The reaction products were washed with ethanol several times and dried at 80°C to obtain 5 B / P / N ternary synergistic flame retardants.
[0066] (2) The above five B / P / N ternary synergistic flame retardants were prepared into aqueous solutions for standby use, and five identical PEI aqueous solutions were prepared for standby use. Five PEI aqueous solutions were poured into five flame retardant aqueous solutions (the concentration of B / P / N ternary synergistic flame retardants in the five mixed solutions was 100 g / L, and the concentration of PEI was 10 g / L), and the mixed solutions were reacted at 50°C for 40 minutes to obtain five different flame retardant finishing solutions.
[0067] (3) Five pieces of cotton fabrics were immersed in the five flame retardant finishing liquids prepared one by one, the immersion temperature was 60°C, the immersion time was 20 min, the bath ratio was 1:20, two immersions and two rollings were performed, the liquid carrying rate was maintained at 100%, and the five flame retardant cotton fabrics were dried at 80°C for 30 min to obtain five flame retardant cotton fabrics.
[0068] The limiting oxygen index (LOI) of 5 flame retardant cotton fabrics was tested, and the results are shown in Table 2.
[0069] Table 2 Effect of different reaction temperatures on the flame retardant properties of cotton fabrics treated with flame retardants
[0070] Boric acid reaction temperature / ℃ LOI / % 110 36.9 120 38.1 130 40.1 140 39.9 150 39.8
[0071] Since the esterification reaction is a reversible reaction, the generated water needs to be continuously removed from the reaction system to promote the forward reaction, so the reaction temperature cannot be too low, so the effect of temperature on the LOI value was investigated in the range of 110-150°C. As shown in Table 2, when the temperature is low, the reaction is incomplete. As the reaction temperature increases, the LOI value increases and the degree of reaction increases; but when the temperature is too high, the viscosity of the system increases rapidly, affecting the subsequent reaction, and some side reactions will occur in the system, affecting the LOI value, so it is more appropriate to choose a temperature of 130°C.
[0072] In order to explore the structure of boron-phosphorus-nitrogen flame retardant, infrared test was carried out on the flame retardant with the above optimal preparation conditions (boric acid reaction temperature of 130℃). Figure 1 .
[0073] from Figure 1 It can be seen that the flame retardant is at 1650cm -1 、1450cm -1 、1127cm -1 、1035cm -1 Peaks appear. Among them, 1450cm -1 The characteristic peaks of CN and BOC are 1127 cm -1 and 1035cm -1 The absorption peaks belong to P=O and POC respectively. Figure 1 The infrared results in Figure 4 indicate that the flame retardant was successfully prepared.
[0074] Example 4: Selection of PEI dosage in flame retardant finishing liquid
[0075] (1) 75 mL of DMF was placed in a flask, and 0.05 mol of meglumine and 0.25 mol of phosphoric acid were added, and the mixture was reacted at 130°C for 2 h. Subsequently, 0.20 mol of boric acid was added to the flask, and the mixture was reacted at 130°C for 2 h. Finally, 0.25 mol of urea was added to the flask, and the mixture was reacted at 120°C for 1 h. The reaction product was washed with ethanol several times and dried at 80°C to obtain a B / P / N ternary synergistic flame retardant.
[0076] (2) Prepare 8 portions of aqueous solution of the above B / P / N ternary synergistic flame retardant with the same concentration, and prepare 8 portions of PEI aqueous solution with different concentrations for standby use. Pour 8 portions of PEI aqueous solution into 8 portions of flame retardant aqueous solution one by one (at this time, the concentration of B / P / N ternary synergistic flame retardant in the 8 mixed solutions is 100 g / L, and the concentration of PEI is 0 g / L, 1 g / L, 5 g / L, 7.5 g / L, 10 g / L, 12.5 g / L, 15 g / L, 20 g / L respectively), and react the mixed solution at 50°C for 40 minutes to obtain 8 different flame retardant finishing solutions.
[0077] (3) Eight pieces of cotton fabrics were immersed in eight kinds of flame retardant finishing liquids, respectively, at an immersion temperature of 60°C, an immersion time of 20 min, a bath ratio of 1:20, two immersions and two rollings, with the liquid carrying rate maintained at 100%, and dried at 80°C for 30 min to obtain eight kinds of flame retardant cotton fabrics.
[0078] In order to explore the effect of PEI dosage on the flame retardancy of fabrics, the LOI of the 8 flame retardant cotton fabrics obtained above was tested and the results are shown in Table 3.
[0079] Table 3 Effect of different PEI concentrations on the flame retardant properties of cotton fabrics treated with flame retardants
[0080] PEI concentration g / L LOI / % 0 33.5 1 34.7 5 35.9 7.5 37.1 10 40.1 12.5 38.3 15 37.8 20 36.9
[0081] It can be seen from Table 3 that the LOI of flame retardant cotton fabric increases with the increase of PEI concentration. However, if there is too much PEI, the cross-linking reaches saturation, the amount of flame retardant on the flame retardant cotton fabric cannot be increased, and the PEI content increases, thus reducing the LOI of the flame retardant cotton fabric.
[0082] In order to observe the precipitation of the flame retardant finishing liquid, the prepared flame retardant finishing liquid (PEI concentration is 10g / L) was left to stand for a period of time to observe the precipitation over time. The results are as follows Figure 2 .Depend on Figure 2It can be seen that after the two clear and transparent solutions were mixed and reacted for a period of time, a white opaque turbid liquid was formed. When it was left to stand, the turbid liquid gradually precipitated. After 24 hours, the turbid liquid was completely precipitated. This phenomenon shows that polyethyleneimine and B / P / N ternary synergistic flame retardant underwent a replacement reaction, and the two were cross-linked to form a substance with low water solubility, which improved the hydrophobicity of the flame retardant.
[0083] Example 5: Effect of different bath ratios on LOI of finished fabrics
[0084] (1) 75 mL of DMF was placed in a flask, and 0.05 mol of meglumine and 0.25 mol of phosphoric acid were added, and the mixture was reacted at 130°C for 2 h. Subsequently, 0.20 mol of boric acid was added to the flask, and the mixture was reacted at 130°C for 2 h. Finally, 0.25 mol of urea was added to the flask, and the mixture was reacted at 120°C for 1 h. The reaction product was washed with ethanol several times and dried at 80°C to obtain a B / P / N ternary synergistic flame retardant.
[0085] (2) Prepare a flame retardant finishing liquid with 100 g / L of B / P / N ternary synergistic flame retardant and 10 g / L of PEI in the mixed solution, and react at 50°C for 40 min. Prepare 5 portions of flame retardant finishing liquid of different volumes for use.
[0086] (3) Five pieces of cotton fabrics were immersed in five parts of flame retardant finishing liquid (the bath ratios of the five finishing liquids were 1:20, 1:30, 1:40, 1:50, and 1:60, respectively), the immersion temperature was 60°C, the immersion time was 20 min, two immersions and two rollings were performed, the liquid carrying rate was maintained at 100%, and five different flame retardant cotton fabrics were obtained by drying at 80°C for 30 min.
[0087] In order to explore the effect of different bath ratios on the flame retardancy of cotton fabrics, the LOI of flame-retardant cotton fabrics was tested and the results are shown in Table 4.
[0088] Table 4 Effect of different bath ratios on the flame retardant properties of cotton fabrics treated with flame retardants
[0089]
[0090]
[0091] It can be seen from Table 4 that as the bath ratio increases, the LOI increases accordingly. When the bath ratio is 1:50, it basically reaches equilibrium.
Claims
1. A method for preparing a B / P / N ternary synergistic flame retardant, characterized in that: The following steps are involved: (1) meglumine and phosphoric acid react in a solvent to obtain solution A; (2) adding boric acid to solution A to react and obtain solution B; (3) adding urea to solution B to react, and obtaining the B / P / N ternary synergistic flame retardant after the reaction is completed; In step (1), the reaction temperature of meglumine and phosphoric acid is 120-140° C.; The solvent is one or more of N,N-dimethylformamide, dimethyl sulfoxide, and dichloromethane; In step (2), the reaction temperature after adding boric acid is 110 to 150° C.; In step (3), the reaction temperature after adding urea is 110-130°C.
2. The method for preparing the B / P / N ternary synergistic flame retardant according to claim 1, characterized in that: The molar ratio of meglumine to phosphoric acid is 1:(3-10); The molar ratio of meglumine to boric acid is 1:(1-5); The molar ratio of phosphoric acid to urea is 1:(0.5-1.1).
3. The method for preparing the B / P / N ternary synergistic flame retardant according to claim 1, characterized in that: In step (1), the reaction time is 1 to 3 hours.
4. The method for preparing the B / P / N ternary synergistic flame retardant according to claim 1, characterized in that: In step (2), the reaction time is 1 to 3 hours.
5. The method for preparing the B / P / N ternary synergistic flame retardant according to claim 1, characterized in that: In step (3), the reaction time is 0.5 to 2 hours.
6. A B / P / N ternary synergistic flame retardant, characterized in that: The method is prepared according to any one of claims 1 to 5.
7. A flame retardant finishing liquid, characterized in that: In the flame retardant finishing liquid, the concentration of the flame retardant is 20 to 200 g / L; The flame retardant is the B / P / N ternary synergistic flame retardant described in claim 6.
8. The flame retardant finishing liquid according to claim 7, characterized in that: The flame retardant finishing liquid is obtained by mixing and reacting an aqueous solution of the B / P / N ternary synergistic flame retardant and an aqueous solution of polyethyleneimine.
9. The flame retardant finishing liquid according to claim 8, characterized in that: In the flame retardant finishing liquid, the mass ratio of the B / P / N ternary synergistic flame retardant to the polyethylene imine is 10:(0.2-2).
10. Use of the flame retardant finishing liquid according to any one of claims 7 to 9 in flame retardant treatment of cotton fabrics.