Polymer, resin composition, resin film, semiconductor device and light emitting device
By introducing specific structural units into polymer and resin compositions, optimizing the linear thermal expansion coefficient and absorbance, the problems of warpage and pattern accuracy in semiconductor devices and display devices are solved, and resin film preparation with high precision and reliability is achieved. Excellent performance taking into account drug resistance and absorbance.
Patent Information
- Application Number
- CN202110792213.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-07-13
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-07-13
AI Technical Summary
In the preparation process of semiconductor devices and display devices, the difference in linear thermal expansion coefficients between the substrate and the resin leads to insufficient accuracy in warping and pattern miniaturization, and the performance differences in the photosensitive resin affect the quality of the finished product. In particular, it is difficult to balance drug resistance and absorbance issues. .
Design a polymer and resin composition containing specific structural units, and optimize the linear thermal expansion coefficient and absorbance by introducing a rigid structure and fluorine atoms into the main chain to form a resin film with good drug resistance and high precision.
It effectively suppresses the mark problem, improves pattern refinement, ensures high reliability and high-density performance of semiconductor devices and display devices, and takes into account the excellent performance of drug resistance and absorbance.
Smart Images

Figure CN115678005B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to a polymer, a resin composition, a resin film and a preparation method thereof, as well as a manufacturing method and application thereof in the field of semiconductor devices and light-emitting devices. The present application also relates to a photosensitive resin composition obtained from the resin composition, and a resin film prepared therefrom, as well as a manufacturing method and application thereof in the field of semi-layer devices and light-emitting devices. Background Art
[0002] In recent years, with the rapid development of high functionality, high performance ratio and miniaturization of electronic equipment, people also require miniaturization, thinning or lightening of semiconductor devices and display devices. Therefore, as a wiring board for assembling electronic components, the demand for flexible printed wiring boards is rapidly increasing compared with the rigid printed wiring boards traditionally used.
[0003] In the manufacturing process of semiconductor devices and display devices, patterns need to be formed as required. However, due to the difference in linear thermal expansion coefficients between the device substrate and the resin, the substrate will be warped, resulting in reduced yield and poor device stability. In addition, when the pattern is formed by using a photosensitive resin film for exposure, cleaning and other processes, the performance differences of the photosensitive resin composition will also lead to poor pattern refinement, making it difficult to achieve the high-density, high-speed and high-capacity requirements of semiconductor devices.
[0004] By changing the polymer monomer structure, the linear thermal expansion coefficient, absorbance, or light transmittance, and other properties of the polymer resin can be changed to improve warping, pattern miniaturization accuracy, etc. In order to reduce the linear thermal expansion coefficient, a rigid structure is generally introduced into the main chain, but the introduction of a rigid structure will increase the absorbance of the resin, thereby reducing the photosensitivity of the resin.
[0005] WO2016 / 121691A1 discloses a resin with a small linear thermal expansion coefficient and low absorbance, which is achieved by introducing trifluoromethyl and hydroxyl groups into a 4,4'-diaminobiphenyl derivative monomer. However, the presence of trifluoromethyl increases the solubility of the resin, thereby reducing the chemical resistance (drug resistance), affecting the quality of the finished product; and the resin has a low surface tension, which can easily cause marks when barrier metal is formed on the wiring and bumps, resulting in problems such as uneven amplitude of the substrate wiring in the finished product and reduced yield. Summary of the invention
[0006] The present application provides a polymer and resin composition with excellent performance, which has good drug resistance. After being made into a resin film, its linear thermal expansion coefficient is small, which can effectively suppress the occurrence of the mark problem; it can also make the prepared graphics more refined. The polymer and resin composition involved in the present application also have a small absorbance. The present application also provides a resin film, a semiconductor device and a light-emitting device.
[0007] In a first aspect, the present application provides a polymer comprising a structural unit represented by formula (1) and a structural unit represented by formula (2).
[0008]
[0009]
[0010] Among them, R 1 An organic group having 2 to 20 carbon atoms in the main chain, and R 1 With 1-4 carboxyl groups;
[0011] Among them, R 3 An organic group having 2 to 20 carbon atoms in the main chain, and R 3 With 1-8 F atoms and 1-4 hydroxyl groups;
[0012] Wherein, Y1, Y2, Z1, Z2 are organic groups, and: one of Y1 and Z1 is H, and the other forms an amide structure with N, or Y1 and Z1 are connected by a chemical bond, and at least one of Y1 and Z1 forms an amide structure with N, or Y1 and Z1 form an imide structure with N, or Y1 and Z1 form a double bond structure connected to N; one of Y2 and Z2 is H, and the other forms an amide structure with N, or Y2 and Z2 are connected by a chemical bond, and at least one of Y2 and Z2 forms an amide structure with N, or Y2 and Z2 form an imide structure with N, or Y2 and Z2 form a double bond structure connected to N.
[0013] In a preferred embodiment, the R 1 The main chain is preferably any one or more of an aromatic hydrocarbon group and an aromatic group containing heteroatoms; wherein the heteroatoms may be any one or more of O, S, and N. wherein the aromatic hydrocarbon group or the aromatic group containing heteroatoms may be a cyclic structure or multiple cyclic structures, for example, any one or more of a parallel ring, a linked ring, and a spiro ring structure.
[0014] Specifically, the R 1The main chain structure may preferably contain any one or more of: phenyl, biphenyl, anthracenyl, naphthyl, pyrenyl, pyridyl, pyridyl, pyrrolyl, pyranyl, benzothiophenyl, thienyl, indolyl, isoindolyl, imidazolyl, benzimidazolyl, carbazolyl, oxazole, thiazolyl, isothiazolyl, pyridazinyl, pyrazolyl, acridinyl, benzopyrenyl, quinolyl, or a connected structure of any two or more of the above groups.
[0015] For example, the R 1 The main chain structure may contain:
[0016] Any one of the structures, where A is any one of O, N, and S.
[0017] Among them, the R 1 The carboxyl group can be: A) directly connected to R by a C—C covalent bond through the carbon atom of the carboxyl group 1 The main chain structure, and / or B) connected to R through other carbon atoms 1 The main chain structure, but preferably A) the carbon atom of the carboxyl group is directly connected to R through a CC covalent bond 1 On the main chain structure.
[0018] For example, R 1 Part of the H on the main chain structure is substituted by carboxyl, or part of the H is substituted by HOOC-V1-T1-, wherein x is an integer of 1-3, V1 does not exist or is an alkyl group, and preferably a C1-C10 alkyl group, T1 does not exist or is any one or more of -O-, -CO-O-, -NH-, -CO-NH-, -S-, and -N=CH-.
[0019] Among them, -V1-T1- is not recommended to have large steric hindrance, for example, it is not recommended to contain tertiary carbon atoms or groups or cyclic structures, etc. For example, V1 is preferably a straight-chain alkyl group, or an alkyl group with a side chain length of no more than 3 carbon atoms, or a side chain carbon atom totaling no more than 10% of the main chain carbon atom number.
[0020] In a preferred embodiment, the R 1 It can also have one or more R 2 Group,
[0021] The more R 2 The group may be independently selected from any one or more of H, halogen atoms, hydroxyl, mercapto, normal hydrocarbon group, isoalkyl group, alkoxy, alkylthio, alkylamino, and alkyl acyloxy. 2The group may be one or more independently selected from H, a halogen atom, a hydroxyl group, a mercapto group, a methyl group, a methoxy group, a methylamino group, a formyloxy group, an ethyl group, an ethoxy group, an ethylamino group, an acetoxy group, a propyl group, a propoxy group, a propylamino group, and a propionyloxy group. 2 The group is preferably H, a halogen atom, a monovalent organic group containing 1 to 20 carbon atoms, or a hydroxyl group.
[0022] In a preferred embodiment, the structure represented by formula (1) accounts for 0.1-50% of the total number of monomer units of the polymer, and more preferably 0.2-30%. For example, in a polymer chain synthesized from monomers, when the monomer units total 100 moles, the molar number of the structure represented by formula (1) is 0.1-50 moles, more preferably 0.2-30 moles, more preferably 0.5-20 moles, and more preferably 1-10 moles.
[0023] In a preferred embodiment, the R 3 The main chain is preferably any one or more of an aromatic hydrocarbon group and an aromatic group containing a heteroatom, wherein the heteroatom may be any one or more of O, S, and N.
[0024] List, the R 3 The main chain structure can be preferably a structure containing any one or more of phenyl, biphenyl, anthracene, naphthyl, pyrenyl, pyridyl, bipyridyl, pyrrolyl, pyranyl, benzothiophenyl, thienyl, indolyl, isoindolyl, imidazolyl, benzimidazolyl, carbazolyl, oxazolyl, thiazolyl, isothiazolyl, pyridazinyl, pyrazolyl, acridinyl, benzopyrenyl, quinolyl, triazolyl, or any two or more of the above groups.
[0025] For example, the R 3 The main chain structure can contain:
[0026]
[0027] Any one of the structures, where A is any one of O, N, and S.
[0028] In a preferred embodiment, the R 3 In addition to the above structure, the main chain structure may also preferably contain -MQ-, wherein M is selected from any one or more of aliphatic hydrocarbons, aromatic hydrocarbons, and aromatic compounds containing heteroatoms; N is connected to M; wherein, more preferably, the heteroatom may be any one or more of O, S, and N; and Q may be any one or more of -O-, -CO-O-, -NH-, -CO-NH-, -S-, and -N=CH-.
[0029] More preferably, M can be any one or more of phenyl, biphenyl, anthracenyl, naphthyl, pyrenyl, pyridyl, bipyridyl, pyrrolyl, pyranyl, benzothiophenyl, thienyl, indolyl, isoindolyl, imidazolyl, benzimidazolyl, carbazolyl, oxazolyl, thiazolyl, isothiazolyl, pyridazinyl, pyrazolyl, acridinyl, benzopyrenyl, quinolyl, triazolyl, or a connected structure of any two or more of the above groups.
[0030] For example, the M may be preferably:
[0031] Any one of the structures, where A is any one of O, N, and S.
[0032] In the above content of this application, R 3 The fluorine atoms contained can be directly connected to R 3 on the main chain.
[0033] For example, R 3 Some H on the main chain C of the group is replaced by F, but it should be noted that R 3 Some of the H on the main chain C of the group can also be replaced by F x H 3-x C-V2-T2-substituted, wherein x is an integer from 1 to 3, V2 does not exist or is an alkyl group, and preferably a C1-C10 alkyl group, T2 does not exist or is any one or more of -O-, -CO-O-, -NH-, -CO-NH-, -S-, -N=CH-.
[0034] Among them, the F x H 3-x It is recommended that C-V2-T2- is a group with less steric hindrance, which can be specifically listed as F, CHF2, CH2F, CF3, C2H4F, C2H3F2, C2H2F3, C2HF4, C2F5, trifluoromethoxy, pentafluoroethoxy, etc.
[0035] For example, V2 is preferably a straight chain alkyl group, or an alkyl group with a side chain not exceeding 3 carbon atoms in length, or an alkyl group with a side chain carbon atom totaling not exceeding 10% of the number of main chain carbon atoms.
[0036] In the above content of this application, R 3 The hydroxyl group contained can be directly connected to R by the oxygen atom of the hydroxyl group through a covalent bond. 3 on the main chain.
[0037] For example, R 3Part of the H on the main chain C of the group is substituted by hydroxyl, or part of the H is substituted by HO-V3-T3-, wherein V3 does not exist or is an alkyl group, and preferably a C1-C10 alkyl group, and T3 does not exist or is any one or more of -O-, -CO-O-, -NH-, -CO-NH-, -S-, and -N=CH-.
[0038] Among them, -V3-T3- is not recommended to have large steric hindrance, for example, it is not recommended to contain tertiary carbon atoms or groups or cyclic structures, etc. For example, V3 is preferably a straight chain alkyl group, or an alkyl group with a side chain length of no more than 3 carbon atoms, or a side chain carbon atom totaling no more than 10% of the main chain carbon atom number.
[0039] For example, R 3 It can be:
[0040] In a preferred embodiment, the polymer described in the present application also contains an acyl group connected to -NH-, or an acyl group connected to N, to form an amide or imide group. For example, formula (1) may form the following structural units:
[0041] A1 is a residue of a compound providing an acyl group.
[0042] For example, formula (2) may be a structural unit formed as follows: A2 is a residue of a compound providing an acyl group.
[0043] Alternatively, in a preferred embodiment, the structural unit represented by formula (2) is an imide structure represented by formula (3) and / or an amide structure represented by formula (4):
[0044]
[0045] Wherein, X is a tetravalent organic group containing 6 to 30 carbon atoms; R 4 and R 5Each independently selected from H, alkali metal ions, Si1-Si20 silyl, C1-C10 hydrocarbon, C1-C10 hydrocarbon amine, C1-C20 hydrocarbon substituted imidazolyl, C1-C20 hydrocarbon substituted pyridyl, C1-C20 hydrocarbon substituted pyrrolyl, C1-C20 hydrocarbon substituted pyranyl, C1-C20 hydrocarbon substituted benzothiophenyl, C1-C20 hydrocarbon substituted thienyl, C1-C20 hydrocarbon substituted indolyl , C1-C20 alkyl-substituted isoindolyl, C1-C20 alkyl-substituted benzimidazolyl, C1-C20 alkyl-substituted carbazolyl, C1-C20 alkyl-substituted oxazolyl, C1-C20 alkyl-substituted thiazolyl, C1-C20 alkyl-substituted isothiazolyl, C1-C20 alkyl-substituted pyridazinyl, C1-C20 alkyl-substituted pyrazolyl, C1-C20 alkyl-substituted acridinyl, C1-C20 alkyl-substituted quinolyl.
[0046] In a preferred embodiment, the hydrocarbon group is preferably any one or more of an alkyl group, an aromatic hydrocarbon group, an alkyl-substituted aromatic hydrocarbon group, an aromatic hydrocarbon-substituted alkane hydrocarbon group, or any two or more of the hydrocarbon groups are connected by covalent bonds to form a hydrocarbon group.
[0047] In a preferred embodiment, X is a tetracarboxyl compound residue (the portion after removing the carboxyl group) or a tetracarboxylic dianhydride compound residue (the portion after removing the anhydride group). In a preferred embodiment, X is preferably a structure shown in formula (5):
[0048]
[0049] Wherein, the ring in formula (5) is a linear alkyl group, an aliphatic ring, an aromatic ring, or an organic group containing a cycloalkyl group or an organic group containing an aromatic ring. For example, the ring in formula (5) can be preferably selected from: a tetravalent butane group, a cyclopentane group, a cyclobutane group, a biphenyl group, or any one or more of the groups shown in formula (6):
[0050]
[0051] In a preferred embodiment, the ring in formula (6) can be an aromatic ring or an aliphatic ring.
[0052] In a preferred embodiment, R 6 It can be preferably a C1-C10 linear hydrocarbon group, a C3-C30 cyclic hydrocarbon group, a C5-C30 aromatic group containing a heteroatom, -W1-R 7-W2-, any one or more of -HN-, -CO-O-, -O-, -CO-NH-, -CO-, -N=CH-, or any two or more of the above groups connected by covalent bonds; wherein W1 and W2 are independently selected from any one or more of -HN-, -CO-O-, -O-, -CO-NH-, -CO-, -S-, -N=CH-, and R 7 selected from C5-C30 aromatic groups, C5-C30 aromatic groups containing heteroatoms, Si1-Si20 silyl groups, C1-C10 linear hydrocarbon groups, C1-C20 hydrocarbon-substituted imidazolyl groups, C1-C20 hydrocarbon-substituted pyridyl groups, C1-C20 hydrocarbon-substituted pyrrolyl groups, C1-C20 hydrocarbon-substituted pyranyl groups, C1-C20 hydrocarbon-substituted benzothiophenyl groups, C1-C20 hydrocarbon-substituted thienyl groups, C1-C20 hydrocarbon-substituted indolyl groups, C1-C20 hydrocarbon-substituted any one or more of a C1-C20 alkyl-substituted isoindolyl, a C1-C20 alkyl-substituted benzimidazolyl, a C1-C20 alkyl-substituted carbazolyl, a C1-C20 alkyl-substituted oxazolyl, a C1-C20 alkyl-substituted thiazolyl, a C1-C20 alkyl-substituted isothiazolyl, a C1-C20 alkyl-substituted pyridazinyl, a C1-C20 alkyl-substituted pyrazolyl, a C1-C20 alkyl-substituted acridinyl, and a C1-C20 alkyl-substituted quinolyl.
[0053] For example, X can be a structure shown in formula (7):
[0054]
[0055] For example, X could be:
[0056]
[0057] One or more of; wherein n is R 8 The number of groups, m is R 9 The number of groups, R 8 , R 9Each of the following groups is independently selected from H, a C1-C10 linear alkyl group, a C3-C20 cycloalkyl group, and a C5-C30 aromatic group, such as any one or more of a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a tert-butyl group, an n-pentyl group, a cyclopentyl group, a phenyl group, a biphenyl group, an anthracenyl group, a naphthyl group, a pyrenyl group, a pyridyl group, a bipyridyl group, a pyrrolyl group, a pyranyl group, a benzothiophenyl group, a thienyl group, an indolyl group, an isoindolyl group, an imidazolyl group, a benzimidazolyl group, a carbazolyl group, an oxazolyl group, a thiazolyl group, an isothiazolyl group, a pyridazinyl group, a pyrazolyl group, an acridinyl group, a benzopyrenyl group, a quinolyl group, and a triazolyl group, or a connected structure of any two or more of the above groups.
[0058] Specifically, the available R 6 Examples include:
[0059]
[0060]
[0061] In a preferred embodiment, the polymer described in the first aspect of the present application is preferably at least one or more of polyamide, polyimide, polyimide precursor, polybenzoxazole, polybenzoxazole precursor, or copolymers thereof.
[0062] In a preferred embodiment, the weight average molecular weight of the polymer described in the first aspect of the present application is preferably 3000-1000000, more preferably 5000-500000, and more preferably 8000-200000.
[0063] The second aspect of the present application is to provide a resin composition, which includes the polymer described in the first aspect of the present application; or, includes a first polymer containing a structural unit represented by formula (1) and a second polymer containing a structural unit represented by formula (2).
[0064] Wherein, the first polymer and the second polymer can be independently selected from at least one or more of polyamide, polyimide, polyimide precursor, polybenzoxazole, polybenzoxazole precursor, or copolymers thereof. For example, the second polymer can be a polymer containing structural formula (3) and / or a polymer containing structural formula (4), and a combination of polymers.
[0065] In a preferred embodiment, the resin composition preferably includes at least one or more of polyamide, polyimide, polyimide precursor, polybenzoxazole, polybenzoxazole precursor, or copolymers thereof.
[0066] In a preferred embodiment, the resin composition may further include a photosensitizer.
[0067] In a preferred embodiment, the photosensitizer is preferably a photoacid generator (also called a photoacid generator), for example, a quinonediazide compound, a sulfonium salt compound, a phosphonium salt compound, a diazonium salt compound, an iodonium salt compound, or a combination of at least one or more thereof, and a quinonediazide compound is particularly preferred.
[0068] Preferred quinonediazide compounds include compounds obtained by ester-bonding quinonediazidesulfonic acid to polyhydroxy compounds, compounds obtained by sulfonamide-bonding quinonediazidesulfonic acid to polyamino compounds, compounds obtained by ester-bonding and / or sulfonamide-bonding quinonediazidesulfonic acid to polyhydroxypolyamino compounds, and the like. More preferred are compounds in which more than 50 mol% of all functional groups of polyhydroxy compounds or polyamino compounds are substituted by quinonediazide groups; the quinonediazide groups are preferably selected from at least one or more of naphthoquinonediazide-5-sulfonyl and naphthoquinonediazide-4-sulfonyl. The term "multi" in "polyhydroxy" and "polyamino" as used herein refers to at least 2.
[0069] In a preferred embodiment, the photosensitizer is preferably a photopolymerization initiator (also called a photoinitiator), which can specifically include a combination of at least one or more of a free radical initiator, a cationic initiator, an anionic initiator, and a zwitterionic initiator. Preferably, an oxime ester free radical initiator is used, which can specifically include 1-phenyl-1,2-propanedione-2-(o-methoxycarbonyl)oxime, 1-phenyl-1,2-butanedione-2-(o-methoxycarbonyl)oxime, OXE01 (manufactured by BASF), N-1818, N1919, NCI-831, etc.
[0070] In a preferred embodiment, in the composition of the present application, the photopolymerization initiator is preferably used in combination with a photopolymerizable compound, such as dipentaerythritol hexaacrylate.
[0071] In a preferred embodiment, the photoacid generator accounts for ≤50% by weight of the resin composition, preferably 0.5-30% by weight, and more preferably 2-20% by weight.
[0072] In a preferred embodiment, the photopolymerization initiator accounts for ≤50% by weight of the resin composition, preferably 0.5-30% by weight, and more preferably 2-20% by weight.
[0073] In a preferred embodiment, the resin composition may further include a sensitizer, which may be a free radical photoinitiator or a cationic photoinitiator, such as aromatic diazonium salts, diaryl iodide compounds, triaryl sulfide compounds, benzoin and its derivatives (such as benzoin ether), acetophenone derivatives (such as dialkoxyacetophenone, chlorinated acetophenone derivatives), aromatic ketone compounds (such as benzophenone, 4,4'-dimethylaminobenzophenone, thioxanthone compounds).
[0074] In a preferred embodiment, the resin composition may further include a thermal crosslinking agent. The available thermal crosslinking agent may be a methylol compound, a methoxymethylol compound, a urea compound, an epoxy compound, an oxetane compound, etc. Specifically, the available thermal crosslinking agent may be ML-236TMP, 4-Methylol3M6C, ML-MC, ML-TBC, 2,6-dimethoxymethyl-4-tert-butylphenol, 2,6-dimethoxymethyl-p-cresol, 2,6-diacetoxymethyl-p-cresol, TriML-P, TriML-35XL, TriML-TrisCR-HAP, TML-BP, TML-HQ, TML-pp-BPF, TML-BPA, TMOM-BP, HML-TPPHBA, HML-TPHAP, HMOM-TPPHBA, HMOM-TPHAP, NIKALAC MX-290, NIKALAC MX-280, NIKALAC MX-270, NIKALAC MW-390, NIKALAC MW-100LM, Epolight 400P, Epolight 1500NP, Epolight80MF, Epolight 4000, Epolight 3002, etc.
[0075] In a preferred embodiment, the thermal crosslinking agent accounts for 0.5-50% by weight of the resin composition, and more preferably 3-40% by weight.
[0076] In a preferred embodiment, the resin composition may further include a surface modifier for improving the wettability of the polymer or resin composition with the substrate, which may also be referred to as a wettability surface modifier. Examples of the surface modifier include fluorine-based surfactants such as Fluorad, MEGAFAC, and Surflon, organosiloxane surfactants such as KP341, DBE, GLANOL, and BYK, and acrylic polymer surfactants such as POLYFLOW.
[0077] The amount of the surface modifier used is preferably 0.01-50% by weight of the resin composition.
[0078] In a preferred embodiment, the resin composition may further include a capping agent. For example, the capping agent may be a compound such as phenol, alcohol, or alkyne, and may specifically be, but not limited to, 2-aminophenol, 3-aminophenol, 4-aminophenol, acetylene, methanol, and the like.
[0079] The amount of the end-capping agent used is preferably 0.01-50% by weight of the resin composition.
[0080] In a preferred embodiment, the resin composition may further include filler particles, particularly preferably inorganic particles, which may specifically be, but are not limited to, silicon dioxide, titanium dioxide, aluminum oxide, zirconium oxide, calcium carbonate, talc, tungsten nitride, zirconium nitride, boron nitride, mica powder, kaolin, montmorillonite, palygorskite, etc.
[0081] The amount of filler particles used is preferably 0.01-50% by weight of the resin composition.
[0082] In a preferred embodiment, the resin composition may further include a solvent, especially preferably a polar aprotic solvent, which may be, but is not limited to, γ-butyrolactone, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol mono-n-propyl ether, ethylene glycol mono-n-butyl ether, diethylene glycol monomethyl ether and diethylene glycol, monoethyl ether, diethylene glycol mono-n-propyl ether, diethylene glycol mono-n-butyl ether, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol mono-n-propyl ether, propylene glycol mono-n-butyl ether. n-Butyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol mono-n-propyl ether, dipropylene glycol mono-n-butyl ether, tripropylene glycol monomethyl ether, tripropylene ether, ethylene glycol monoethyl ether, tetrahydrofuran, dioxane, acetone, methyl ethyl ketone, diisobutyl ketone, cyclohexanone, 2-heptanone, 3-heptanone, diacetone alcohol, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether ethyl ester, propylene glycol monoethyl ether acetate Esters, ethyl lactate and other esters, ethyl 2-hydroxy-2-methylpropionate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, ethyl ethoxyacetate, ethyl glycolate, methyl 2-hydroxy-3-methylbutyrate, 3-methoxybutyl acetate, 3-methyl-3-methoxybutyl acetate, 3-methyl-3-methoxybutyl propionate, ethyl acetate, n-propyl acetate, isopropyl acetate, n-butyl acetate, Isobutyl acetate, n-amyl formate, isoamyl acetate, n-butyl propyl valerate, ethyl butyrate, n-propyl butyrate, isobutyric butyrate, n-butyl butyrate, methyl pyruvate, ethyl pyruvate, n-propyl pyruvate, methyl acetoacetate, ethyl acetoacetate, ethyl 2-oxobutyrate, aromatic compounds, for example, toluene, xylene, amides, and any one or more of solvents such as N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, etc.
[0083] The amount of the solvent used is preferably 50-98% by weight of the resin composition.
[0084] In a preferred embodiment, the viscosity of the resin composition is preferably 0.1 cP to 10000 cP.
[0085] The third aspect of the present application is to provide a resin film, which contains the polymer described in the first aspect of the present application, or contains the resin composition described in the second aspect of the present application.
[0086] More preferably, the resin film is prepared from the polymer described in the first aspect of the present application, or is prepared from the resin composition described in the second aspect of the present application.
[0087] The fourth aspect of the present application is to provide a semiconductor device, which includes the resin film described in the third aspect of the present application.
[0088] More preferably, in the semiconductor device, the resin film is applied to an interlayer insulating layer and / or a surface protective layer in a semiconductor device having electrodes, metal wirings, an interlayer insulating layer and / or a surface protective layer on a substrate.
[0089] The fifth aspect of the present application is to provide a light-emitting device, which includes the resin film described in the third aspect of the present application.
[0090] More preferably, in the light-emitting device, the resin film is applied to a planarization layer and / or an insulating layer in an organic light-emitting device having a driving circuit, a planarization layer, a first electrode, an insulating layer, a light-emitting layer and a second electrode on a substrate.
[0091] In a preferred embodiment, the thickness of the resin film is preferably 1.0-20 μm, more preferably 2.0-10 μm.
[0092] The sixth aspect of the present application is to provide a method for preparing the polymer, comprising subjecting the monomer represented by formula (1-1), -HN2 of the monomer represented by formula (2-1), and the carboxyl group of a monomer containing at least two carboxyl groups, or the acyl halide of a monomer containing at least two acyl halide groups, or the anhydride group of a monomer containing at least one anhydride group to a condensation reaction to obtain the polymer.
[0093]
[0094]
[0095] In a preferred embodiment, the monomer structure containing at least one anhydride group is preferably as follows:
[0096]
[0097] In a preferred embodiment, the acyl halide is any one of acyl chloride and acyl bromide.
[0098] In a preferred embodiment, the monomer containing at least two acyl halides or the monomer containing at least two carboxyl groups is as shown in formula (8):
[0099]
[0100] Wherein, E can be a hydroxyl group, a halogen atom (such as Cl or Br); R 10 It can be any one or more of a C1-C30 linear hydrocarbon group, an aromatic group, and an aromatic group containing heteroatoms. More preferably, the heteroatom can be any one or more of O, S, and N. In a preferred embodiment, the aromatic hydrocarbon group or the aromatic group containing heteroatoms is a cyclic structure, and can be preferably one cyclic structure or more cyclic structures. Preferably, the more cyclic structures can be any one or more of a parallel ring, a chain ring, and a spiro ring structure.
[0101] More preferably, the R 10 It may preferably contain any one or more of phenyl, biphenyl, anthracenyl, naphthyl, pyrenyl, pyridyl, bipyridyl, pyrrolyl, pyranyl, benzothiophenyl, thienyl, indolyl, isoindolyl, imidazolyl, benzimidazolyl, carbazolyl, oxazolyl, thiazolyl, isothiazolyl, pyridazinyl, pyrazolyl, acridinyl, benzopyrenyl, quinolyl, triazolyl, or a connected structure of any two or more of the above groups.
[0102] For example, the R 10 It may preferably contain:
[0103]
[0104] Any one of the structures, where A is any one of O, N, and S.
[0105] This application has the following beneficial effects:
[0106] 1) The present application obtains a resin composition containing the structure shown in formula (1) and formula (2) through structural component design, which is easy to form intramolecular and / or intermolecular alignment to obtain a rigid structure, and at the same time, the formed film structure is more compact, which has a good effect on reducing the linear thermal expansion coefficient and has excellent drug resistance; ② It contains fluorine atoms, which can break the intramolecular conjugation balance and has good water repellency, so that the absorbance is good and the drug resistance is excellent; therefore, when the resin composition is prepared into a resin film and / or a photosensitive resin film, it has the performance characteristics of good linear thermal expansion coefficient, drug resistance and absorbance; therefore, in the preparation process of semiconductor devices or display devices, due to the good expansion coefficient, the stress caused by the packaging material can be relieved and the damage of the low-k layer can be suppressed; at the same time, due to the good drug resistance and absorbance, a semiconductor device or display device with high reliability is provided.
[0107] 2) The present application adopts structural component design, and when the obtained resin composition is prepared into a resin film or a photosensitive resin film, it is easy to form intramolecular and / or intermolecular alignment, obtain a rigid structure, and impart a lower water absorption rate. The compact film structure formed also reduces the amount of gas overflow during use; therefore, in the preparation process of semiconductor devices or display devices, due to the low water absorption rate and small amount of gas exhaust, a semiconductor device or display device with high reliability can be provided.
[0108] 3) At the same time, after the structure of the present application is combined with photosensitivity, a photosensitive resin composition with excellent dissolution rate can be obtained, and the prepared photosensitive resin film can be given a low linear thermal expansion coefficient, excellent drug resistance, and good absorbance. Especially when a photosensitive resin film containing a pattern is made, a high precision of pattern concave and convex is obtained, or a semiconductor device or display device with high reliability is further obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0109] Figure 1 It is a schematic cross-sectional view of a semiconductor device having a bump.
[0110] Figure 2 A schematic cross-sectional view of the main parts of an organic light-emitting device.
[0111] In the figure, serial number 1 is a silicon wafer, 2 is an Al pad, 3 is a passivation layer, 4 is a third insulating layer, 5 is a first metal film, 6 is a second metal film, 7 is a fourth insulating layer, 8 is a barrier metal, 9 is a scribe groove, 10 is a solder bump, 11 is a substrate, 12 is a TFT, 13 is a first insulating layer (planarization layer), 14 is an anode, 15 is a through hole, 16 is a second insulating layer (isolation wall), 17 is a recess, 18 is an organic light-emitting layer, and 19 is a cathode. DETAILED DESCRIPTION
[0112] In order to make the purpose and advantages of the present application clearer, the present application is further described in detail below in conjunction with the embodiments, which will help those skilled in the art to further understand the present application, but do not limit the present application in any form. It should be noted that for those of ordinary skill in the art, several modifications and improvements can be made without departing from the concept of the present application. These all belong to the protection scope of the present application.
[0113] The present application provides a polymer, characterized in that it contains a structural unit represented by formula (1) and a structural unit represented by formula (2):
[0114]
[0115]
[0116] Among them, R 1 An organic group having 2 to 20 carbon atoms in the main chain, and R 1 With 1-4 carboxyl groups.
[0117] Among them, R 3 An organic group having 2 to 20 carbon atoms in the main chain, and R 3 With 1-8 F atoms and 1-4 hydroxyl groups.
[0118] Wherein, Y1, Y2, Z1, Z2 are organic groups, and: one of Y1 and Z1 is H, and the other forms an amide structure with N, or Y1 and Z1 are connected by a chemical bond, and at least one of Y1 and Z1 forms an amide structure with N, or Y1 and Z1 form an imide structure with N, or Y1 and Z1 form a double bond structure connected to N; one of Y2 and Z2 is H, and the other forms an amide structure with N, or Y2 and Z2 are connected by a chemical bond, and at least one of Y2 and Z2 forms an amide structure with N, or Y2 and Z2 form an imide structure with N, or Y2 and Z2 form a double bond structure connected to N.
[0119] The polymer may be a polymer and / or a polymer precursor, such as polyimide, polyamide, polybenzoxazole, polyimide precursor, polybenzoxazole precursor, or copolymers thereof. In terms of heat resistance, at least one of polyimide, polybenzoxazole, polyimide precursor, polybenzoxazole precursor, or copolymers thereof is preferred; in terms of lowering the curing temperature during the film-making process, at least one of polyimide, imide precursor, or copolymers thereof is further preferred.
[0120] In terms of the dissolution rate in alkaline solution, the weight average molecular weight of the polymer or polymer precursor resin is preferably 3,000 to 1,000,000. In terms of the concave-convex pattern shape, drug resistance, solubility and heat resistance, it is further preferably 5,000 to 500,000, and further preferably 8,000 to 200,000.
[0121] In terms of dissolution rate, in a preferred embodiment, the structure represented by formula (1) accounts for 0.01-50% of the total number of monomer units of the polymer, and more preferably 0.02-30%. For example, when the polymer chain synthesized by the monomer contains 100 moles of monomer units in total, the molar number of the structure represented by formula (1) is 0.01-50 moles for solubility considerations, and is more preferably 0.02-30 moles, more preferably 0.05-20 moles, and more preferably 0.1-10 moles for drug resistance considerations.
[0122] In a preferred embodiment, the R 1 It can also have one or more R 2 Group, R 2 The group is preferably H, a halogen atom, or a monovalent organic group containing 1 to 20 carbon atoms. More preferably, the monovalent organic group containing 1 to 20 carbon atoms is 1 The main chain has at least 6 carbon atoms, preferably at least 4 carbon atoms, and does not contain tertiary carbon atoms or cyclic structures. 2 The smaller the spatial position of the group, the better, which helps to improve the heat resistance and linear expansion coefficient of the polymer.
[0123] For ease of understanding, the structural unit shown in formula (1) of the present application can be represented by the following structure of formula (1-2):
[0124]
[0125] Among them, R 11 For R 1 The main chain structure of o1 is the substituent R 2 The number of o2 is R 11 The number of carboxyl groups connected thereto, o2 is preferably an integer of 1-4.
[0126] For ease of understanding, the structural unit shown in formula (2) of the present application can be represented by the structure of the following formula (2-2):
[0127]
[0128] Among them, R 31 For R 3 The main chain structure of q1 is directly connected to R by a covalent bond 31The number of F, q2 is R 31 The number of hydroxyl groups connected to the above, q1 is preferably an integer of 1-8, and q2 is preferably an integer of 1-4.
[0129] Among them, from the perspective of the heat resistance of the obtained resin, the R 1 Main chain R 11 Preferably, it is any one or more of an aromatic hydrocarbon group and an aromatic group containing heteroatoms; wherein, more preferably, the heteroatom may be any one or more of O, S, and N; preferably, the aromatic hydrocarbon group or the aromatic group containing heteroatoms is a cyclic structure, and may be preferably one cyclic structure or more cyclic structures; preferably, the more cyclic structures may be any one or more of a parallel ring, a linked ring, and a spiro ring structure.
[0130] From the perspective of reducing the linear thermal expansion coefficient of the obtained resin, it is more preferred that the R 1 Main chain structure R 11 It may preferably contain any one or more of the following groups: phenyl, biphenyl, anthracenyl, naphthyl, pyrenyl, pyridyl, pyridyl, pyrrolyl, pyranyl, benzothiophenyl, thienyl, indolyl, isoindolyl, imidazolyl, benzimidazolyl, carbazolyl, oxazole, thiazolyl, isothiazolyl, pyridazinyl, pyrazolyl, acridinyl, benzopyrenyl, quinolyl, or a connected structure of any two or more of the above groups.
[0131] For example, the R 1 Main chain structure R 11 It may preferably contain:
[0132]
[0133]
[0134] Any one of the structures, where A is any one of O, N, and S.
[0135] Among them, the R 1 The carboxyl group contained is directly connected to R by the carbon atom of the carboxyl group through a CC covalent bond. 1 The main chain structure may also contain a branched HOOC-V1-T1-structure.
[0136] For example, R 1Part of the H on the main chain structure is replaced by carboxyl, or part of the H is replaced by HOOC-V1-T1-, wherein x is an integer of 1-3, V1 does not exist or is an alkyl group, and preferably a C1-C10 alkyl group, and T1 does not exist or is any one or more of -O-, -CO-O-, -NH-, -CO-NH-, -S-, -N=CH-. Among them, -V1-T1- is not recommended to have a large steric hindrance, for example, it is not recommended to contain tertiary carbon atoms or groups, or it is not recommended to have a cyclic structure, etc. For example, V1 is preferably a straight-chain alkyl group, or an alkyl group with a side chain length of no more than 3 carbon atoms, or a side chain carbon atom totaling no more than 10% of the number of main chain carbon atoms.
[0137] Among them, from the perspective of the heat resistance and linear thermal expansion coefficient of the obtained resin, R 2 The group is not recommended to have large steric hindrance, such as tertiary carbon atoms or groups, and does not contain a ring structure. 2 The group may be independently selected from any one or more of H, halogen atoms, hydroxyl, mercapto, normal hydrocarbon group, isoalkyl group, alkoxy, alkylthio, alkylamino, and alkyl acyloxy. 2 The group may be one or more independently selected from H, a halogen atom, a hydroxyl group, a mercapto group, a methyl group, a methoxy group, a methylamino group, a formyloxy group, an ethyl group, an ethoxy group, an ethylamino group, an acetoxy group, a propyl group, a propoxy group, a propylamino group, and a propionyloxy group. 2 The group is preferably H, a halogen atom, a monovalent organic group containing 1 to 20 carbon atoms, or a hydroxyl group.
[0138] For example, the structure represented by formula (1) or formula (1-2) can be derived from the following compounds:
[0139]
[0140] However, it should be understood that the structure represented by formula (1) or formula (1-2) may also be derived from other diamino compounds.
[0141] From the perspective of heat resistance of the obtained resin, the R 3 Main chain R 31 Preferably, it is any one or more of an aromatic hydrocarbon group and an aromatic group containing heteroatoms. More preferably, the heteroatom may be any one or more of O, S, and N. In a preferred embodiment, the aromatic hydrocarbon group or the aromatic group containing heteroatoms is a cyclic structure, and may be preferably one cyclic structure or more cyclic structures. Preferably, the more cyclic structures may be any one or more of a parallel ring, a chain ring, and a spiro ring structure.
[0142] In order to reduce the linear thermal expansion coefficient of the obtained resin, more preferably, the R 3 Main chain structure R 31 It may preferably contain any one or more of phenyl, biphenyl, anthracenyl, naphthyl, pyrenyl, pyridyl, bipyridyl, pyrrolyl, pyranyl, benzothiophenyl, thienyl, indolyl, isoindolyl, imidazolyl, benzimidazolyl, carbazolyl, oxazolyl, thiazolyl, isothiazolyl, pyridazinyl, pyrazolyl, acridinyl, benzopyrenyl, quinolyl, triazolyl, or a connected structure of any two or more of the above groups.
[0143] For example, the R 3 The main chain structure may preferably contain:
[0144]
[0145]
[0146] Any of the structures, where AA selects any of O, N, and S.
[0147] In a preferred embodiment, the R 3 Main chain structure R 31 In addition to the above structure, it may also preferably contain -MQ-, wherein M is selected from any one or more of aliphatic hydrocarbons, aromatic hydrocarbons, and aromatic compounds containing heteroatoms; N is connected to M; wherein, more preferably, the heteroatom may be any one or more of O, S, and N; Q may be any one or more of -O-, -CO-O-, -NH-, -CO-NH-, -S-, and -N=CH-. In a preferred embodiment, the aromatic hydrocarbon or aromatic compound containing heteroatoms is a cyclic structure, and may be preferably one cyclic structure or more cyclic structures. Preferably, the more cyclic structures may be any one or more of a cyclic, a chain, and a spirocyclic structure.
[0148] More preferably, M can be any one or more of phenyl, biphenyl, anthracenyl, naphthyl, pyrenyl, pyridyl, bipyridyl, pyrrolyl, pyranyl, benzothiophenyl, thienyl, indolyl, isoindolyl, imidazolyl, benzimidazolyl, carbazolyl, oxazolyl, thiazolyl, isothiazolyl, pyridazinyl, pyrazolyl, acridinyl, benzopyrenyl, quinolyl, triazolyl, or a connected structure of any two or more of the above groups.
[0149] For example, the M may be preferably:
[0150]
[0151] Any one of the structures, where A is any one of O, N, and S.
[0152] In a preferred embodiment, R 3 The fluorine atoms contained are directly connected to R by covalent bonds 3 The main chain R 31 In a preferred embodiment, R 31 Some of the H on the C of is replaced by F. From the perspective of reducing the absorbance of the obtained resin, R 31 The C of the x H 3-x C-V2-T2-substituted, wherein x is an integer of 1-3, V2 does not exist or is an alkyl group, and preferably a C1-C10 alkyl group, T2 does not exist or is any one or more of -O-, -CO-O-, -NH-, -CO-NH-, -S-, -N=CH-. x H 3-x It is recommended that C-V2-T2- is a group with less steric hindrance, which can be specifically listed as F, CHF2, CH2F, CF3, C2H4F, C2H3F2, C2H2F3, C2HF4, C2F5, trifluoromethoxy, pentafluoroethoxy, etc.
[0153] In a preferred embodiment, R 3 The hydroxyl groups contained may be directly connected to R 3 The main chain R 31 superior.
[0154] In a preferred embodiment, R 31 Part of the H on C is replaced by hydroxyl, or part of the H is replaced by HO-V3-T3-, wherein V3 does not exist or is an alkyl group, and preferably a C1-C10 alkyl group, and T3 does not exist or is any one or more of -O-, -CO-O-, -NH-, -CO-NH-, -S-, -N=CH-. Among them, -V3-T3- is not recommended to have a large steric hindrance, for example, it is not recommended to contain tertiary carbon atoms or groups or cyclic structures. For example, V3 is preferably a straight-chain alkyl group, or an alkyl group with a side chain length of no more than 3 carbon atoms, or a side chain carbon atom totaling no more than 10% of the number of main chain carbon atoms.
[0155] For example, R 3 It can be:
[0156] Thus, the structure represented by formula (2) or formula (2-2) may be derived from the following compounds:
[0157]
[0158] However, it should be understood that the structure represented by formula (2) or formula (2-2) may be derived from other diamino compounds.
[0159] In the above structure of the present application, the reaction of the hydroxyl group on the benzene ring and F replacing H can be carried out by existing technologies, including but not limited to TBAF, NFSI, PhenoFluor TM The reaction of fluorinating agents such as chlorine and bromine, and the substitution reaction from chlorine or bromine atoms to fluorine.
[0160] In a preferred embodiment, the polymer described in the present application further contains an acyl group connected to -NH-, or an acyl group connected to N, forming an amide or imide group.
[0161] For example, formula (1) may be a structural unit formed as follows: A1 is a compound residue providing an acyl group, and as a repeating unit, it can be expressed as
[0162]
[0163] For example, formula (2) may be a structural unit formed as follows: A2 is a compound residue providing an acyl group, and as a repeating unit, it can be expressed as
[0164]
[0165] Among them, A1 and A2 are preferably any one or more of C4-C20 cycloalkanes, aromatic hydrocarbons, and aromatic compounds containing heteroatoms, and are particularly preferably any one or more of phenyl, biphenyl, anthracene, naphthyl, pyrenyl, pyridyl, bipyridyl, pyrrolyl, pyranyl, benzothiophenyl, thienyl, indolyl, isoindolyl, imidazolyl, benzimidazolyl, carbazolyl, oxazolyl, thiazolyl, isothiazolyl, pyridazinyl, pyrazolyl, acridinyl, benzopyrenyl, quinolyl, and triazolyl, or a connected structure of any two or more of the above groups.
[0166] For example, A1 and A2 are preferably independently:
[0167]
[0168] Any one of the structures, where A is any one of O, N, and S.
[0169] Alternatively, in a preferred embodiment, the structural unit represented by formula (2) is an imide structure represented by formula (3) or an amide structure represented by formula (4):
[0170]
[0171] The structures of formula (3) and formula (4) can exist continuously as repeating units in the molecular chain of the polymer, or exist intermittently in the molecular chain of the polymer. For example, the structures shown in formula (3-2) and formula (4-2)
[0172]
[0173] Among them, n1, n2, n3, and n4 are the numbers of corresponding repeating units on the polymer molecular chain.
[0174] Wherein, X is a tetravalent organic group containing 6 to 30 carbon atoms; R 4 and R 5 Each independently selected from H, alkali metal ions, Si1-Si20 silyl, C1-C10 hydrocarbon, C1-C10 hydrocarbon amine, C1-C20 hydrocarbon substituted imidazolyl, C1-C20 hydrocarbon substituted pyridyl, C1-C20 hydrocarbon substituted pyrrolyl, C1-C20 hydrocarbon substituted pyranyl, C1-C20 hydrocarbon substituted benzothiophenyl, C1-C20 hydrocarbon substituted thienyl, C1-C20 hydrocarbon substituted indolyl , C1-C20 alkyl-substituted isoindolyl, C1-C20 alkyl-substituted benzimidazolyl, C1-C20 alkyl-substituted carbazolyl, C1-C20 alkyl-substituted oxazolyl, C1-C20 alkyl-substituted thiazolyl, C1-C20 alkyl-substituted isothiazolyl, C1-C20 alkyl-substituted pyridazinyl, C1-C20 alkyl-substituted pyrazolyl, C1-C20 alkyl-substituted acridinyl, C1-C20 alkyl-substituted quinolyl.
[0175] In a preferred embodiment, the hydrocarbon group is preferably any one or more of an alkyl group, an aromatic hydrocarbon group, an alkyl-substituted aromatic hydrocarbon group, an aromatic hydrocarbon-substituted alkane hydrocarbon group, or any two or more of the hydrocarbon groups are connected by covalent bonds to form a hydrocarbon group.
[0176] From the perspective of reducing the linear thermal expansion coefficient and absorbance of the obtained resin, X is preferably a tetracarboxyl compound residue (the portion after the carboxyl group is removed) or a tetracarboxylic dianhydride compound residue (the portion after the anhydride group is removed). In a preferred embodiment, X is preferably a structure represented by formula (5):
[0177]
[0178] Wherein, the ring in formula (5) is a linear alkyl group, an aliphatic ring, an aromatic ring, or an organic group containing a cycloalkyl group or an organic group containing an aromatic ring. For example, the ring in formula (5) can be preferably selected from: a tetravalent butane group, a cyclopentane group, a cyclobutane group, a biphenyl group, or any one or more of the groups shown in formula (6):
[0179]
[0180] In a preferred embodiment, the ring in formula (6) can be an aromatic ring or an aliphatic ring.
[0181] In a preferred embodiment, R 6 It can be preferably a C1-C10 linear hydrocarbon group, a C3-C30 cyclic hydrocarbon group, a C5-C30 aromatic group containing a heteroatom, -W1-R 7 -W2-, any one or more of -HN-, -CO-O-, -O-, -CO-NH-, -CO-, -N=CH-, or any two or more of the above groups connected by covalent bonds; wherein W1 and W2 are independently selected from any one or more of -HN-, -CO-O-, -O-, -CO-NH-, -CO-, -S-, -N=CH-, and R 7 selected from C5-C30 aromatic groups, C5-C30 aromatic groups containing heteroatoms, Si1-Si20 silyl groups, C1-C10 linear hydrocarbon groups, C1-C20 hydrocarbon-substituted imidazolyl groups, C1-C20 hydrocarbon-substituted pyridyl groups, C1-C20 hydrocarbon-substituted pyrrolyl groups, C1-C20 hydrocarbon-substituted pyranyl groups, C1-C20 hydrocarbon-substituted benzothiophenyl groups, C1-C20 hydrocarbon-substituted thienyl groups, C1-C20 hydrocarbon-substituted indolyl groups, C1-C20 hydrocarbon-substituted any one or more of a C1-C20 alkyl-substituted isoindolyl, a C1-C20 alkyl-substituted benzimidazolyl, a C1-C20 alkyl-substituted carbazolyl, a C1-C20 alkyl-substituted oxazolyl, a C1-C20 alkyl-substituted thiazolyl, a C1-C20 alkyl-substituted isothiazolyl, a C1-C20 alkyl-substituted pyridazinyl, a C1-C20 alkyl-substituted pyrazolyl, a C1-C20 alkyl-substituted acridinyl, and a C1-C20 alkyl-substituted quinolyl.
[0182] For example, X can be a structure shown in formula (7):
[0183]
[0184] Among them, formula (7) can be derived from:
[0185]
[0186] For example, X could be:
[0187]
[0188] One or more of .
[0189] Where n is R 8 The number of groups, m is R 9 The number of groups, R 8 , R 9 Each of the following groups is independently selected from H, a C1-C10 linear alkyl group, a C3-C20 cycloalkyl group, and a C5-C30 aromatic group, such as any one or more of a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a tert-butyl group, an n-pentyl group, a cyclopentyl group, a phenyl group, a biphenyl group, an anthracenyl group, a naphthyl group, a pyrenyl group, a pyridyl group, a bipyridyl group, a pyrrolyl group, a pyranyl group, a benzothiophenyl group, a thienyl group, an indolyl group, an isoindolyl group, an imidazolyl group, a benzimidazolyl group, a carbazolyl group, an oxazolyl group, a thiazolyl group, an isothiazolyl group, a pyridazinyl group, a pyrazolyl group, an acridinyl group, a benzopyrenyl group, a quinolyl group, and a triazolyl group, or a connected structure of any two or more of the above groups.
[0190] Considering the linear thermal expansion coefficient, the available R 6 Examples include:
[0191] The acid anhydride can be selected from existing products, or can be prepared by a known method. For example, the reaction of a hydroquinone derivative and chlorinated trimellitic anhydride includes but is not limited to the reaction using a deacidifying agent such as pyridine.
[0192] Resin composition
[0193] <Polymer>
[0194] The resin composition of the present application comprises at least one or more of polyamide, polyimide, polyimide precursor, polybenzoxazole, polybenzoxazole precursor, or copolymers thereof.
[0195] For example, the resin composition of the present application may include the above-mentioned polymer, or include a first polymer including the structural unit represented by the above-mentioned formula (1) and a second polymer including the structural unit represented by the above-mentioned formula (2).
[0196] Wherein, the first polymer and the second polymer can be independently selected from at least one or more of polyamide, polyimide, polyimide precursor, polybenzoxazole, polybenzoxazole precursor, or copolymers thereof. For example, the second polymer can be a composition containing a polymer of the above structural formula (3) and / or a polymer of the above structural formula (4).
[0197] The polymer (as well as the first polymer and the second polymer) is a main film-forming substance.
[0198] <Photosensitive agent>
[0199] The resin composition of the present application may further include a photosensitizer to form a photosensitive resin composition.
[0200] The photosensitive agent can be specifically selected from a photoacid generator. When a photoacid generator is selected as the photosensitive agent, it can give the resin composition positive photosensitivity, and the composed resin composition is a positive photosensitive resin (positive photosensitive resin) composition. In the case of using a positive photosensitive resin composition, an acidic group is generated in the light-irradiated part resin, thereby increasing the solubility of the light-irradiated part resin in the alkaline solution, and a positive concave-convex pattern in which the light-irradiated part is dissolved can be obtained.
[0201] The photosensitive agent can also be specifically selected from a photopolymerization initiator, and the photopolymerization initiator is preferably used in combination with a photopolymerizable compound, such as dipentaerythritol hexaacrylate (CAS No.: 29570-58-9). When a photopolymerization initiator is selected as the photosensitive agent, it can give the resin composition negative (negative) photosensitivity, and the composed resin composition is a negative photosensitive resin (negative photosensitive resin) composition. In the case of using a negative photosensitive resin composition, the resin in the light irradiation part undergoes a polymerization reaction, thereby reducing the solubility of the resin in the light irradiation part in the alkaline solution, and a negative concave-convex pattern in which the light irradiation part is insoluble can be obtained. The photopolymerization initiator is further preferably used in combination with a photopolymerizable compound containing an unsaturated bond.
[0202] In the present application, the photoacid generator may specifically include quinonediazide compounds, sulfonium salt compounds, phosphonium salt compounds, diazonium salt compounds, iodonium salt compounds, etc. In terms of photosensitivity, it is further preferred to be quinonediazide compounds; the quinonediazide compounds may specifically include compounds obtained by ester-bonding quinonediazidesulfonic acid to polyhydroxy compounds, compounds obtained by sulfonamide-bonding quinonediazidesulfonic acid to polyamino compounds, compounds obtained by ester-bonding and / or sulfonamide-bonding quinonediazidesulfonic acid to polyhydroxypolyamino compounds, etc., and it is further preferred that 50 mol% or more of all functional groups of polyhydroxy compounds or polyamino compounds are substituted by quinonediazide groups; the quinonediazide groups are preferably selected from at least one of naphthoquinonediazide-5-sulfonyl and naphthoquinonediazide-4-sulfonyl, and may also be used in combination.
[0203] In the present application, the photopolymerization initiator can specifically include at least one of the free radical generating type (free radical initiator), the photocation generating type (cationic initiator), and the photobase generating type (anionic initiator), and can also be used in combination; from the perspective of obtaining higher sensitivity for pattern processing, it is preferred to use free radical generating type oxime esters, which can specifically include 1-phenyl-1,2-propanedione-2-(o-methoxycarbonyl) oxime, 1-phenyl-1,2-butanedione-2-(o-methoxycarbonyl) oxime, OXE01 (manufactured by BASF), N-1818, N1919, NCI-831 (manufactured by EDICO), etc.
[0204] In the present application, the content of the photoacid generator is preferably 0.5 weight ratio (0.5wt%) or more, more preferably 2 weight ratio (2wt%) or more, and preferably 30 weight ratio (30wt%) or less, more preferably 20 weight ratio (20wt%) or less, based on 100 weight ratio of the resin composition; when the content of the photoacid generator is 0.5 weight ratio (0.5wt%) or more, the exposure effect is better and a finer pattern can be obtained; when the content of the photoacid generator is 50 weight ratio (50wt%) or less, a resin film with excellent heat resistance can be obtained. In order to obtain a better exposure effect, a sensitizer can also be contained.
[0205] In the present application, the content of the photopolymerization initiator is preferably 0.5 weight ratio (0.5wt%) or more, more preferably 2 weight ratio (2wt%) or more, and preferably 30 weight ratio (30wt%) or less, more preferably 20 weight ratio (20wt%) or less, based on 100 weight ratio of the resin composition; when the content of the photopolymerization initiator is 0.5 weight ratio (0.5wt%) or more, the developability of the exposed part during development can be reduced to obtain a finer pattern, and when the content is 50 weight ratio (50wt%) or less, a resin film with excellent heat resistance can be obtained. In order to obtain a better exposure effect, a sensitizer can also be contained.
[0206] <Thermal cross-linking agent>
[0207] The resin composition of the present application may further contain a thermal crosslinking agent. Examples of the crosslinking agent include methylol compounds, methoxymethylol compounds, urea compounds, epoxy compounds, and oxetane compounds, and any of these compounds can be preferably used.
[0208] In particular, from the perspective of storage stability after exposure, it is further preferred to use a methoxymethylol compound. When the resin composition involved in the present application contains these thermal crosslinking agents, a resin film with low shrinkage, stable dimensions and high reproducibility can be obtained after curing. In addition, in the case where the composition is the photosensitive resin composition, the present application further has the following advantages: it is almost insoluble in alkaline developer before exposure, but easily soluble in alkaline developer after exposure, so the film loss caused by development is small, and development can be performed in a short time, and finally a finer pattern can be obtained.
[0209] Examples of the thermal crosslinking agent include ML-236TMP, 4-Methylol 3M6C, ML-MC, and ML-TBC (these are trade names, manufactured by Honshu Chemical Industry Co., Ltd.), 2,6-dimethoxymethyl-4-tert-butylphenol, 2,6-dimethoxymethyl-p-cresol, 2,6-diacetoxymethyl-p-cresol, TriML-P, TriML-35XL, TriML-TrisCR-HAP, TML-BP, TML-HQ, TML-pp-BPF, TML-BPA, TMOM-BP, HML-TPPHBA, HML-TPHAP, HMOM-TPPHBA, and HMOM-TPHAP (these are trade names, manufactured by Honshu Chemical Industry Co., Ltd.), MX-290, NIKALAC MX-280, NIKALAC MX-270, NIKALAC MW-390, NIKALAC MW-100LM (trade names, manufactured by Sanwa Chemical Co., Ltd.), Epolight 400P, Epolight 1500NP, Epolight 80MF, Epolight 4000, Epolight 3002 (the above are trade names, manufactured by Kyoeisha Chemical Co., Ltd.). The content of the thermal crosslinking agent is preferably 0.5 parts by weight (0.5wt%) or more, more preferably 3 parts by weight (3wt%) or more, based on 100 parts by weight of the resin composition, and is preferably 50 parts by weight (50wt%) or less, more preferably 40 parts by weight (40wt%) or less. When it is within the above range, it is possible to obtain a fine pattern while also providing an advantage of excellent chemical resistance.
[0210] <Surface Modifier>
[0211] The resin composition involved in the present application may also contain a surface modifier to improve the wettability between the resin composition and the substrate. Therefore, the surface modifier is also called a wettability surface modifier. Examples of the surface modifier include: (trade name, manufactured by DIC Corporation), (trade name, manufactured by Asahi Glass Co., Ltd.), etc. fluorine-based surfactants (fluorocarbon surfactants), KP341 (trade name, manufactured by Shin-Etsu Chemical Co., Ltd.), DBE (trade name, manufactured by CHISSO CORPORATION), GLANOL (trade name, manufactured by Kyoeisha Chemical Co., Ltd.), BYK (manufactured by BYK Chemie) and other organosiloxane surfactants, POLYFLOW (trade name, manufactured by Kyoeisha Chemical Co., Ltd.) and other acrylic polymer surfactants, etc.
[0212] <Capping agent>
[0213] The resin composition involved in the present application may also contain an end-capping agent, thereby improving the adhesion of the resin film and the heat-resistant film after the heat treatment. As the end-capping agent, 2-aminophenol, 3-aminophenol, 4-aminophenol, etc. are preferred, but not limited to these; as the end-capping agent, ethynyl, hydroxymethyl, alkoxymethyl and other functional groups are further preferably listed, which can give excellent polymerization performance to the end of the resin.
[0214] <Inorganic particles>
[0215] The resin composition involved in the present application may also contain inorganic particles according to the application requirements, thereby giving the resin film and its heat-resistant film after heat treatment strong and high elasticity, etc.; as preferred inorganic particles, silicon dioxide, titanium dioxide, aluminum oxide, zirconium oxide, etc. can be listed, but are not limited to these.
[0216] <Solvent>
[0217] The resin composition of the present application may further contain a solvent. The coating performance can be improved by making the slurry contain a solvent.
[0218] As the solvent, there can be: gamma-butyrolactone, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol mono-n-propyl ether, ethylene glycol mono-n-butyl ether, diethylene glycol monomethyl ether and diethylene glycol, monoethyl ether, diethylene glycol mono-n-propyl ether, diethylene glycol mono-n-butyl ether, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol mono-n-propyl ether, propylene glycol mono-n-butyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol mono-n-propyl ...-n-butyl ether, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, propylene glycol mono-n-propyl ether, dipropylene glycol mono-n-butyl ether, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, propylene glycol mono-n-propyl ether, dipropylene glycol mono-n-butyl ether, triethylene glycol monomethyl butyl alcohol, tripropylene glycol monomethyl ether, tripropylene glycol monomethyl ether, ethylene glycol monoethyl ether, tetrahydrofuran, dioxane, acetone, methyl ethyl ketone, diisobutyl ketone, cyclohexanone, 2-heptanone, 3-heptanone, diacetone alcohol, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether ethyl ester, propylene glycol monoethyl ether acetate, ethyl lactate and other esters, 2-hydroxy-2-methylpropionic acid ethyl Esters, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, ethyl ethoxyacetate, ethyl hydroxyacetate, methyl 2-hydroxy-3-methylbutyrate, 3-methoxybutyl acetate, 3-methyl-3-methoxybutyl acetate, 3-methyl-3-methoxybutyl propionate, ethyl acetate, n-propyl acetate, isopropyl acetate, n-butyl acetate, isobutyl acetate, n-pentyl formate, isopentyl acetate, n-butyl propyl valerate, ethyl butyrate, n-propyl butyrate, isobutyric acid, n-butyl butyrate, methyl pyruvate, ethyl pyruvate, n-propyl pyruvate, methyl acetoacetate, ethyl acetoacetate, ethyl 2-oxobutyrate, aromatic compounds, for example, toluene, xylene, amides, as well as N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, etc.; it can also contain two or more types of solvents.
[0219] In order to give the resin composition other functional characteristics, other organic and / or inorganic functional reagent materials such as pigments, dyes, and conductive agents may also be added.
[0220] <Method for preparing resin composition>
[0221] The resin composition involved in the present application can be prepared by the following method: (1) subjecting the monomer compound required in the present application to polymerization reaction to obtain the resin required in the present application; (2) placing the required resin in a glass flask or a stainless steel container, and adding a solvent and / or other required additives as required; (3) mixing by dissolving using a mechanical stirrer, ultrasonic wave, stirring degassing machine, etc. to obtain the resin composition involved in the present application. If the photosensitizer described in the present application is added in the preparation method, the photosensitive resin composition described in the present application can be obtained.
[0222] The viscosity of the resin composition involved in the present application is preferably 0.1cP to 10000cP; when the viscosity is above 0.1cP and above 10,000cP, by adjusting the appropriate solid content, a resin film of target thickness can be obtained, the uniformity of film performance can be controlled, and good coating efficiency can be obtained. The viscosity test can be performed using an E-type viscometer. In addition, in order to remove foreign matter in the resin composition, the resin composition can be filtered with a filter with a pore size of 0.01-5μm. The materials used as the main filter components in the filter include polypropylene (PP), polyethylene (PE), nylon (NY), polytetrafluoroethylene (PTFE), etc.; when the resin composition contains fluorine-based surfactants and / or surface modifiers, polyethylene (PE) is preferably used as the material of the main filter components in the filter.
[0223] <Method for preparing resin film>
[0224] The resin film involved in the present application can be prepared by the following method: coating the resin composition involved in the present application on a substrate, and then performing drying, heat treatment and curing processes to obtain the resin film, which can also be called a cured film.
[0225] The substrate may be made of silicon wafer, ceramics, gallium arsenide, metal, glass, metal oxide insulating film, silicon nitride, ITO, IZO, amorphous silicon, microcrystalline silicon, polycrystalline silicon, IGZO, etc., but is not limited to these.
[0226] The coating method may be one of spin coating, spray coating, slit coating, inkjet coating and / or a combination of multiple methods; in terms of the uniformity of the thickness of the resulting resin film, it is preferred to use a coating method that uses slit coating, a combination of slit coating and spin coating, etc.
[0227] The drying method may be one of oven, heating plate, infrared ray and / or a combination of multiple methods; in terms of production stability, the drying conditions are preferably a drying temperature in the range of 50°C to 150°C and a drying time in the range of 2 minutes to 3 hours; in terms of film stability, the drying temperature is preferably 80°C to 130°C. In addition, the drying method may be a drying method that is carried out in one stage, two stages or more stages.
[0228] The heat treatment curing method may use one of an oven, a heating plate, infrared rays and / or a combination of multiple methods; from the perspective of production stability, the heat treatment conditions preferably have a heat treatment temperature in the range of 150°C to 500°C as the curing temperature, and a heat treatment time in the range of 2 minutes to 5 hours. In addition, the heat treatment method may be a heat treatment method that is carried out in one stage, two stages or more stages; from the perspective of warping of the resin film, a heat treatment method that is carried out in multiple stages is preferred.
[0229] <Method for preparing photosensitive resin film>
[0230] The photosensitive resin film involved in the present application can be prepared by the following method: coating the resin composition involved in the present application on a substrate, and then obtaining the photosensitive resin film through processes such as drying, exposure, development, and heat treatment curing, which can also be called a cured film.
[0231] The substrate may be made of silicon wafer, ceramics, gallium arsenide, metal, glass, metal oxide insulating film, silicon nitride, ITO, IZO, amorphous silicon, microcrystalline silicon, polycrystalline silicon, IGZO, etc., but is not limited to these.
[0232] The coating method may be one of spin coating, spray coating, slit coating, inkjet coating and / or a combination of multiple methods; from the perspective of uniformity of thickness of the resulting photosensitive resin film, it is preferred to use a coating method that uses slit coating or a combination of slit coating and spin coating.
[0233] The drying method may be one of oven, heating plate, infrared and / or a combination of multiple methods; in view of the stability of the obtained photosensitive resin film, the drying conditions are preferably a drying temperature in the range of 50°C to 150°C and a drying time in the range of 2 minutes to 3 hours; in view of the film stability, the drying temperature is preferably 80°C to 130°C. In addition, the drying method may be a drying method carried out in one stage, two stages or more stages.
[0234] The exposure method can be to place a mask having a desired shape on the dried resin composition film, and then irradiate the film with radiation from a desired light source. The radiation for the exposure can be ultraviolet visible light, electron beam, or X-ray; in terms of exposure effect, ultraviolet visible light is preferably used, and i-line (365nm), h-line (405nm), and g-line (436nm) from a mercury lamp are more preferably used.
[0235] The development method may be one or more of the following methods: direct spraying of the developer, immersion in the developer, immersion and simultaneous use of ultrasonic waves and ultrasound, and / or a combination thereof. In terms of development efficiency, the preferred development time is 10 seconds to 3 hours. For the developer used in the present method, in order to improve the resolution of the graphics and obtain a refined graphics, it is preferred to use an aqueous solution or organic solution prepared by a single substance or a combination of multiple substances such as N-methyl-2-pyrrolidone, N-acetyl-2-pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, hexamethylphosphoric triamide, tetramethylammonium hydroxide (TMAH), diethanolamine, diethylaminoethanol, sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, triethylamine, diethylamine, methylamine, dimethylamine, dimethylaminoethyl acetate, dimethylaminoethanol, dimethylaminoethyl methacrylate, cyclohexylamine, ethylenediamine, hexamethylenediamine, γ-butyrolactone, dimethylacrylamide, alcohols such as methanol, ethanol, and isopropanol, esters such as ethyl lactate and propylene glycol monomethyl ether acetate, ketones such as cyclopentanone, cyclohexanone, isobutyl ketone, and methyl isobutyl ketone, which have excellent solubility in the resin composition.
[0236] The heat treatment curing method can use one of the methods selected from the group consisting of an oven, a heating plate, and infrared rays, and / or a combination of multiple methods; considering the heat resistance of the obtained photosensitive resin film, the maximum curing temperature of the heat treatment stage is below 400°C, and the curing time is between 5 minutes and 5 hours; considering the stability of the obtained photosensitive resin film, it is preferred that the maximum curing temperature of the heat treatment stage is below 350°C, and the heating method for the heat treatment is a multi-stage heating method.
[0237] The resin film and photosensitive resin film involved in the present application can be applied to electronic components such as semiconductor devices and multilayer wiring boards; specifically, they can be suitably applied to passivation films in semiconductor devices, surface protection films of semiconductor elements, interlayer insulating layers, interlayer insulating films of multilayer wiring for high-density installation, substrates of organic light-emitting elements, insulating layers, planar layers of thin-film transistors, interlayer insulating films of thin-film transistors, etc.; in addition, when the resin composition contains conductive fillers, it can also be used as a wiring material, but various structures can be adopted and are not limited to this.
[0238] <Semiconductor electronic devices>
[0239] Reference Figure 1The present application also provides a semiconductor device, comprising a resin film and / or a photosensitive resin film obtained from the resin composition of the present application; the resin film and / or the photosensitive resin film can be appropriately applied to semiconductor electronic components and semiconductor devices having electrodes, metal wiring, interlayer insulating layers and / or surface protective layers on substrates. Since the resin film and the photosensitive resin film of the present application also have excellent mechanical properties, the stress from the packaging material can be relieved in the packaging process, the damage to the low-k layer can be suppressed, and a highly reliable semiconductor device can be provided.
[0240] <Organic Light Emitting Device>
[0241] Reference Figure 2 The present application also provides a light-emitting device, comprising a resin film and / or a photosensitive resin film obtained from the resin composition involved in the present application; the planarization layer and / or the insulating layer can be appropriately applied to an organic light-emitting device having a driving circuit, a planarization layer, a first electrode (such as an anode), a second insulating layer (isolation layer), an organic light-emitting layer and a second electrode (such as a cathode) on a substrate.
[0242] Since organic light-emitting materials are easily affected by moisture in the environment and deteriorate, adverse effects may occur, such as a decrease in the area ratio of the light-emitting part and the area ratio of its light-emitting pixels. Since the resin film and photosensitive resin film involved in the present application have low water absorption, it is not easy to cause the problem of a decrease in the area ratio of the light-emitting part and the area ratio of its light-emitting pixels, and thus stable driving and good light-emitting characteristics can be maintained for a long time.
[0243] An active matrix display device is taken as an example of a light-emitting device: the display device has a TFT and wiring located on the side of the TFT, and is connected to the TFT on a substrate such as glass or plastic; in addition, a planarization layer is provided on the TFT to cover uneven areas; and a display element is also provided on the planarization layer; the display element and the wiring located on the side of the TFT are connected via contact holes prepared in the planarization layer. When the resin film and / or photosensitive resin film involved in the present application is used as the planarization layer, not only can high-precision graphics be obtained in the manufactured device, and the planarity and dense wiring of the TFT can be improved, but also because the resin film and photosensitive resin film involved in the present application have a small amount of gas exhaust (gas overflow during use), the luminescence reliability of the organic light-emitting device can be improved; therefore, the thickness of the resin film and / or photosensitive resin film is preferably 1.0-20μm, more preferably 2.0-10μm; in addition, from the perspective that the TFT and the wiring located on the side of the TFT can be arranged with high clarity in the thickness direction of the resin film and / or photosensitive resin film, the resin film and / or photosensitive resin film of the planarization layer is preferably a multilayer film structure.
[0244] Evaluation methods involved in this application
[0245] The testing method involved in this application is described below, but is not limited thereto.
[0246] (1) Molecular weight determination method
[0247] The weight average molecular weight (Mw) and molecular weight distribution (Mw / Mn) of the resin were measured using HLC-8020 manufactured by Tosoh.
[0248] (2) Film thickness measurement method
[0249] The test was conducted using VM-1020 equipment manufactured by Dainippon Scrren Mfg Co., Ltd. For the film thickness test of the resin film and the photosensitive resin film, the refractive index involved was measured at 1.629. (3) Method for measuring the linear thermal expansion coefficient
[0250] Sample preparation: Spin the solution of the resin composition onto an 8-inch silicon wafer, and then pre-bake it for 3 minutes on a 120°C hot plate (using a coating and developing device Act-8 manufactured by Tokyo Electric) to make a pre-baked film. Then use an inert gas oven (device CLH-21CD(V)-CCC manufactured by Koyo Thermo Systems Co., Ltd.) to bake, and make the oxygen concentration below 20 ppm, raise the temperature to 250°C at a rate of 5°C / min, heat treat at 250°C for 1 hour, and then cool to 50°C at a rate of 5°C / min to make a baked film. Next, immerse the baked film in a hydrofluoric acid solution for 1-4 minutes, peel off the baked film from the substrate, and air-dry it to obtain a film after heat treatment. During spin coating, the rotation speed is adjusted so that the thickness of the film after heat treatment is controlled to about 10μm.
[0251] Test: The obtained heat-treated film was made into a sample of the required size for the test, and measured using a mechanical analyzer (TMA4000 manufactured by Perkin Elmer) under a nitrogen flow. The heating method during the test was carried out under the following conditions: Step 1, heating to 200°C at a heating rate of 5°C / min at room temperature to remove the water adsorbed by the sample; Step 2, cooling from 200°C to room temperature in an air atmosphere at a cooling rate of 5°C / min; Step 3, starting from room temperature, the measurement was carried out at a heating rate of 5°C / min, and then the average value of the linear thermal expansion coefficient of 50-200°C was obtained.
[0252] (4) Absorbance measurement method
[0253] Sample preparation: Using a spin coater MS-B150 manufactured by MIKASA CO., LTD., the solution of the resin composition was spin-coated on a 50 mm × 50 mm × 0.7 mm thick glass substrate (EAGLE Slim); Next, bake it for 3 minutes on a 120°C hot plate (using a NEO HOTPLATE HI-1000 hot plate manufactured by ASONE) to obtain a resin film. The resin film is then baked using an inert gas oven (apparatus CLH-21CD(V)-CCC manufactured by Koyo Thermo Systems Co., Ltd.), and the oxygen concentration is made less than 20 ppm, and the temperature is raised to 250°C at a rate of 5°C / min, and heat-treated at 250°C for 1 hour, and then cooled to 50°C at a rate of 5°C / min to form a baked resin film. Next, the baked resin film is immersed in hydrofluoric acid for 1-4 minutes, and then the baked resin film is peeled off from the glass substrate and air-dried to obtain a film after heat treatment. During spin coating, the rotation speed is adjusted so that the thickness of the film after heat treatment is about 3 μm.
[0254] Test: The obtained heat-treated film was measured using an ultraviolet-visible spectrophotometer (UV-2600i manufactured by SHIMADZU) to obtain the absorbance value at a wavelength of 400 nm.
[0255] (5) Photosensitivity evaluation method
[0256] Sample preparation: The solution of the resin composition was spin-coated on an 8-inch silicon wafer, and then baked for 3 minutes on a 120°C hot plate (using a coating and developing device Act-8 manufactured by Tokyo Electron Limited.) to obtain a pre-baked film, and the coating process was adjusted to obtain a pre-baked film with a thickness of about 6 μm. The pre-baked film was then exposed to light using an i-line stepper (NIKON NSRi14) at 0-1000 mJ / cm 2 Exposure, 10mJ / cm 2 After exposure, the film was developed with a 2.38 wt % tetramethylammonium hydroxide (TMAH) aqueous solution (Chinese medicine) for 90 seconds and then washed with pure water.
[0257] Test: After exposure and development, the exposure amount (i.e. the minimum exposure amount, expressed as Eth) at which the exposed part completely dissolves and disappears or the unexposed part completely dissolves and disappears is taken as the sensitivity. 2 Below 500 mJ / cm, the sensitivity is considered good. 2 When it is less than , it can be judged that the sensitivity is excellent.
[0258] (6) Drug resistance evaluation method
[0259] Sample preparation: The solution of the resin composition was spin-coated on an 8-inch silicon wafer, and then baked for 3 minutes on a 120°C hot plate (using a coating and developing device Act-8 manufactured by Toshiba Electronics) to obtain a pre-baked film, and the coating process was adjusted to obtain a pre-baked film with a thickness of about 10 μm. The pre-baked film was then baked using an inert gas oven (Koyo Thermo Systems Co., Ltd. device CLH-21CD(V)-CCC) to keep the oxygen concentration below 20 ppm, and the temperature was raised to 250°C at a rate of 5°C / min, and heated at 250°C for 1 hour, and then cooled to 50°C at a rate of 5°C / min to obtain a baked film.
[0260] Test: First, test the baked film and its film thickness is H1. Next, immerse the baked film in an organic solution (dimethyl sulfoxide: 25% water tetramethyl ammonium hydroxide aqueous solution = 90: 8) at 65°C for 60 minutes, and then wash the film with pure water and test its film thickness as H2. Then calculate the film thickness change rate by formula (1). When the film thickness change rate is greater than 20% or the film peeling off from the silicon wafer is observed to be poor, the chemical resistance can be evaluated as very poor, represented by grade D; when the film thickness change rate is between 20% and 10%, the chemical resistance level can be evaluated as generally poor, represented by grade C; when the film thickness change rate is between 10% and 5%, the chemical resistance level can be evaluated as good, represented by grade B; when the film thickness change rate is below 5%, the chemical resistance can be evaluated as excellent, represented by grade A.
[0261] Film thickness change rate (%) = (H1-H2) / H1×100% Formula (1)
[0262] Example
[0263] The present application is described in more detail below based on the examples, but the present application is not limited to these examples. In the examples and comparative examples, the specific compounds and their names or abbreviations used are as follows:
[0264] 1. TCL: terephthaloyl chloride (CAS No.: 100-20-9)
[0265]
[0266] 2. DABA: 3,5-diaminobenzoic acid (CAS No.: 535-87-5)
[0267]
[0268] 3. SiDA: 1,1,3,3-tetramethyl-1,3-bis(3-aminopropyl)disiloxane (CAS No.: 2469-55-8)
[0269]
[0270] 4. DHB: 3,3'-dihydroxy-4,4'-biphenylenediamine (CAS No.: 2373-98-0)
[0271]
[0272] 5. TFMB: 2,2'-bis(trifluoromethyl)benzidine (CAS No.: 341-58-2)
[0273]
[0274] 6. Photopolymerization initiator [a]: NCI-831 manufactured by Aidico Corporation
[0275] 7. Photopolymerizable compound [b]: dipentaerythritol hexaacrylate (CAS No.: 29570-58-9)
[0276] 8. Photoacid generator [c]:
[0277]
[0278] Q is
[0279]
[0280] Synthesis of Photoacid Generator [c]
[0281] Under a nitrogen atmosphere, 29.7 g (0.07 mol) of TrisP-PA (trade name, manufactured by Honshu Chemical Industry Co., Ltd., α,α,α'-tri(4-hydroxyphenyl)-1-ethyl-4-isopropylbenzene) and 50.8 g (0.19 mol, CAS No. 1001756-09-7) of 1,2-naphthoquinone-2-diazide-5-sulfonyl chloride were added to a reactor and dissolved in 600 g of 1,4-dioxane, and 70 g of a 1,4-dioxane solution mixed with 21.3 g of triethylamine (CAS No. 121-44-8) was added dropwise; after stirring at 30°C for 2 hours, the reaction solution was added to water, the precipitated solid was collected, and vacuum dried to obtain a photoacid generator [c].
[0282] 9. OPDA: 4,4'-oxydiphthalic anhydride (CAS No.: 1823-59-2)
[0283]
[0284] 10. NMP: N-methyl-2-pyrrolidone (CAS No.: 872-50-4)
[0285]
[0286] 11. GBL: γ-butyrolactone (CAS No.: 96-48-0)
[0287] 12. Compound [1]: 3,5-Diaminosalicylic acid (CAS No.: 112725-89-0)
[0288]
[0289] Compound [1] is commercially available.
[0290] 13. Compound [2]: 2,2'-bis(trifluoromethyl)-5,5'-dihydroxy-4,4'-diaminobiphenyl
[0291]
[0292] Synthesis of compound [2]:
[0293] Under nitrogen atmosphere, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl (80.0 g, 0.25 mol, CAS No.: 341-58-2) and ethyl acetate (800 mL) were added to the reactor. After replacing with nitrogen three times, the reaction flask was placed in an ice bath at -20°C and stirred; then liquid bromine (26.2 mL, 0.51 mol) was slowly dripped into the reaction flask, and the reaction temperature was controlled below 20°C. The reaction was monitored by high performance liquid chromatography. When the content of the raw material was less than 3%, stirring was stopped, and a saturated sodium carbonate solution was slowly added to the reaction flask to adjust the pH value to neutral. The organic phase was then separated and washed with water (500 mL × 2 times), then anhydrous sodium sulfate was added to dry and filter, and then the organic solvent was removed to obtain a crude product as a yellow solid. Next, petroleum ether / ethyl acetate (150 ml / 5 ml) was added to the crude yellow solid, stirred at room temperature for 30 minutes, and then filtered to obtain a white solid of 2,2'-bis(trifluoromethyl)-5,5'-dibromo-4,4'-diaminobiphenyl, weighing 106.5 g (yield 90%, purity 96%).
[0294] Then, under a nitrogen atmosphere, 2,2'-bis(trifluoromethyl)-5,5'-dibromo-4,4'-diaminobiphenyl (95.6 g, 0.2 mol) and dichloromethane (500 mL) obtained by the above manufacturing method were added to the reactor, and acetic anhydride (51.0 g, 0.5 mol) was added, and the reaction flask was placed in a constant temperature ethanol bath at 10°C and stirred. After standing overnight, the reaction was monitored by a high performance liquid chromatograph. When the content of the raw material was less than 3%, stirring was stopped to obtain a white suspension solution. The reaction solution was filtered, and the filtered solid was washed twice with 50 ml of dichloromethane, and then washed twice with 100 ml of water, and then placed in a vacuum dryer for drying to obtain a white solid of 2,2'-bis(trifluoromethyl)-5,5'-dibromo-4,4'-diacetamidobiphenyl, weighing 106.2 g (yield 94.3%, purity 98%).
[0295] Under nitrogen atmosphere, 2,2'-bis(trifluoromethyl)-5,5'-dibromo-4,4'-diacetamidobiphenyl (112.4 g, 0.20 mol) obtained by the above-mentioned manufacturing method, cuprous iodide (3.82 g, 0.02 mol), N,N'-dimethylethylenediamine (3.52 g, 0.04 mol), potassium phosphate (110.4 g, 0.8 mol), and xylene (1200 mL) were added to the reactor, and then replaced with nitrogen three times, and reacted in an oil bath at 140°C. The reaction was monitored by high performance liquid chromatography, and stirring was stopped when the content of the raw material was less than 3%. The reaction was then cooled, 1 L of toluene was added, and activated carbon was used for decolorization. The mixture was then filtered, and the filtrate was concentrated and recrystallized to finally obtain 48.1 g (yield 60%, purity 97%) of a white solid compound 2,2'-dimethyl-5,5'-bis(trifluoromethyl)-[6,6']dibenzoxazole.
[0296] 2,2'-dimethyl-5,5'-bis(trifluoromethyl)-[6,6']dibenzoxazole (80.0 g, 0.2 mol) obtained by the above-mentioned production method, 36.5% hydrochloric acid (250 ml) and ethanol (1.25 L) were added to a conical flask, and stirred in a 60°C constant temperature oil bath. The reaction was monitored by high performance liquid chromatography. When the content of the raw material was less than 3%, stirring was stopped. Water was added to the reaction solution, and ethanol was removed by vacuum distillation. The pH value was adjusted to be greater than 3, and filtered. The solid obtained by filtration was washed with 100 ml of ethyl acetate and dried in a vacuum dryer to obtain a white solid compound [2]: 2,2'-bis(trifluoromethyl)-5,5'-dihydroxy-4,4'-diaminobiphenyl 63.2 g (yield 90%, purity 98%).
[0297] 14. Compound [3]: 3-Hydroxy-3'-fluoro-4,4'-diphenylenediamine
[0298]
[0299] Synthesis of compound [3]:
[0300] Under nitrogen atmosphere, 21.6 g (100 mmol, CAS No.: 2373-98-0) of 3,3'-dihydroxybiphenyl diamine, 45.8 g (210 mmol) of di-tert-butyl dicarbonate and tetrahydrofuran solution (80 ml) were added to the reactor and stirred at 40°C for 2 hours. After the reaction solution was concentrated by half under reduced pressure, petroleum ether was added for recrystallization to obtain 40.6 g of 3,3'-dihydroxy-N,N'-(tert-butyloxycarbonyl)-4,4'-biphenyl diamine.
[0301] Under nitrogen atmosphere, 20.8 g (50 mmol) of 3,3'-dihydroxy-N,N'-(tert-butyloxycarbonyl)-4,4'-biphenylenediamine, 8.1 g (50 mmol) of (diethylamino)sulfur trifluoride and tetrahydrofuran solution (200 ml) were added to the reactor and stirred at 0°C for 4 hours and at room temperature overnight. 1M HCl (10 ml) was added and stirred for 1 hour and then filtered. The filtrate was separated into an organic layer and an aqueous layer, and the organic layer was concentrated under reduced pressure. The obtained solid was washed with ethanol to obtain 9.8 g of compound, namely compound [3]: 3-hydroxy-3'-fluoro-4,4'-biphenylenediamine.
[0302] 15. Compound [4]: 2,2'-bis(trifluoromethyl)-5-hydroxy-5'-fluoro-4,4'-diaminobiphenyl
[0303]
[0304] Synthesis of compound [4]
[0305] 2,2'-bis(trifluoromethyl)-5,5'-dihydroxy-4,4'-diaminobiphenyl was used to replace 3,3'-dihydroxybiphenyl diamine, and the rest was prepared by referring to the method of synthesizing compound [3].
[0306] 16. Compound [5]: 2,2'-bis(trifluoromethyl)-5,5'-difluoro-4,4'-diaminobiphenyl
[0307]
[0308] The method of synthesizing compound [3] was followed except that 2,2'-bis(trifluoromethyl)-5,5'-dihydroxy-4,4'-diaminobiphenyl was used to replace 3,3'-dihydroxybiphenyl diamine and the amount of (diethylamino)sulfur trifluoride was doubled.
[0309] 17. Compound [6]: N,N'-(3,3'-dihydroxy-[1,1'-biphenyl]-4,4'-diyl)bis(4-aminobenzamide)
[0310]
[0311] Synthesis of compound [6]
[0312] Under nitrogen atmosphere, 3,3'-dihydroxybenzenediamine (CAS No.: 2373-98-0) dissolved in 100 ml of acetone and 17.4 g (0.3 mol) of propylene oxide was added to the reactor and cooled to -15°C. A solution obtained by dissolving 20.4 g (0.11 mol, CAS No.: 122-04-3) of 4-nitrobenzoyl chloride in 100 mL of acetone was added dropwise thereto. After the addition was completed, the reaction was carried out at -15°C for 4 hours, then the temperature was restored to room temperature, and the precipitated white solid was obtained by filtration and vacuum drying at 50°C.
[0313] 30 g of the obtained white solid was placed in a 300 mL stainless steel autoclave and dispersed in 250 mL methyl cellosolve, and 2 g of 5% palladium-carbon catalyst was added. Hydrogen was introduced into the system using a balloon, and the reduction reaction was carried out at room temperature. After about 2 hours, the reaction was terminated after confirming that the balloon was no longer soft. After the reaction was completed, the palladium compound used as the catalyst was removed by filtration, and concentrated using a rotary evaporator to obtain a hydroxyl-containing diamine compound, namely compound [6]: N,N'-(3,3'-dihydroxy-[1,1'-biphenyl]-4,4'-diyl)bis(4-aminobenzamide).
[0314] 18. Compound [7]: N,N'-(3-fluoro-3'-hydroxy-[1,1'-biphenyl]-4,4'-diyl)bis(4-aminobenzamide)
[0315]
[0316] Synthesis of compound [7]
[0317] Except for using compound [3] instead of 3,3'-dihydroxybenzenediamine, the remaining steps are the same as those for synthesizing compound [6].
[0318] 19. Compound [8]: N,N'-(5-fluoro-5'-hydroxy-2,2'-bis(trifluoromethyl)-[1,1'-biphenyl]-4,4'-diyl)bis(4-aminobenzamide)
[0319]
[0320] Synthesis of compound [8]
[0321] Except for using compound [4] instead of 3,3'-dihydroxybenzenediamine, the remaining steps are the same as those for synthesizing compound [6].
[0322] 20. Compound [9]: N,N'-(5,5'-difluoro-2,2'-bis(trifluoromethyl)-[1,1'-biphenyl]-4,4'-diyl)bis(4-aminobenzamide)
[0323]
[0324] Synthesis of compound [9]
[0325] Except for using compound [5] instead of 3,3'-dihydroxybenzenediamine, the remaining steps are the same as those for synthesizing compound [6].
[0326] 21. Compound
[10] : 1,4-[2,5-bis(tert-butyl)]phenyl-bis(trimethylene)-dianhydride
[0327]
[0328] Synthesis of compound
[10]
[0329] Under nitrogen atmosphere, 22.2 g (100 mmol, CAS No.: 88-58-4) of 2,5-di-tert-butylhydroquinone, 42.1 g (200 mmol, CAS No.: 1204-28-0) of chlorotrimellitic anhydride, pyridine (20 ml) and tetrahydrofuran (150 ml) were added to the reactor and stirred at 0°C for 3 hours and then stirred at room temperature overnight. After filtration, the filtrate was separated into an organic layer and an aqueous layer, and the organic layer was concentrated under reduced pressure. The obtained solid was washed with ethanol to obtain 43.1 g of the compound, namely compound
[10] : 1,4-[2,5-bis(tert-butyl)]phenyl-bis(trimellitate) dianhydride.
[0330] 22. Compound
[11] : 1,4-(2-phenyl)phenyl-diphenyltrimethoxybenzene dianhydride
[0331]
[0332] Synthesis of compound
[11]
[0333] Except for using 2-phenylhydroquinone (CAS No.: 1079-21-6) instead of 2,5-di-tert-butylhydroquinone, the remaining steps are the same as those of the synthetic compound
[10] .
[0334] 23. Compound
[12] : 1,4-(2,2'-phenyl)biphenyl-bis(triphenyl)phthalate dianhydride
[0335]
[0336] Synthesis of compound
[12]
[0337] Except for using 3,3'-diphenylbiphenol (CAS No.: 2401-43-6) instead of 2,5-di-tert-butylhydroquinone, the remaining steps are the same as those for synthesizing compound
[10] .
[0338] 24. Compound
[13] : 4-ethynylaniline (CAS No.: 14235-81-5)
[0339] 25. Compound
[14] : 3-aminophenol (CAS No.: 591-27-5)
[0340] 26. Compound
[15] : 4,4'-Dicarbonyl imidazole diphenyl ether
[0341] 27. Compound
[16] : N,N-dimethylformamide diethyl acetal (CAS No.: 1188-33-6)
[0342]
[0343] Other compounds, chemical reagents, and equipment mentioned in the following examples of this application can all be obtained commercially.
[0344] Example 1 (E1), Synthesis of Resin A
[0345] Under nitrogen atmosphere, compound [3] (3-hydroxy-3'-fluoro-4,4'-diphenylenediamine) 10.08g (0.047mol), DABA (3,5-diaminobenzoic acid) 0.15g (0.001mol) and SiDA 0.75g (0.003mol) were added to the reactor, stirred and dissolved in NMP194ml, and then added to an ice bath. TCL 9.14g (0.045mol) was added 5 times within 30 minutes and reacted for 1 hour. The hydrochloric acid produced in the reaction was neutralized with lithium carbonate 1.43g, added to 2L of water, filtered, washed with water 3 times, and then dried in a vacuum dryer at 50°C for 72 hours to obtain resin A.
[0346] Example 2 (E2), Synthesis of Resin B
[0347] In a nitrogen atmosphere, 16.64 g (0.047 mol) of compound [4] (2,2'-bis(trifluoromethyl)-5-hydroxy-5'-fluoro-4,4'-diaminobiphenyl) and DABA (0.15 g, 0.001 mol of 3,5-diaminobenzoic acid) dissolved in 80 g of NMP were added to the reactor, and 16.13 g (0.045 mol) of compound
[15] was added. After reacting at 70°C for 12 hours, the mixture was added to 2 L of water, filtered, washed with water three times, and then dried in a vacuum dryer at 50°C for 72 hours to obtain resin B.
[0348] Example 3 (E3), Synthesis of Resin C
[0349] In a nitrogen atmosphere, compound [4] (16.65 g) (0.047 mol) of 2,2'-bis(trifluoromethyl)-5-hydroxy-5'-fluoro-4,4'-diaminobiphenyl), 0.15 g (0.001 mol) of DABA (3,5-diaminobenzoic acid) and 0.75 g (0.003 mol) of SiDA were dissolved in 80 g of NMP, and 16.13 g (0.045 mol) of OPDA was added. After reacting at 40°C for 2 hours, 1.17 g (0.01 mol) of compound
[13] was added as a capping agent and reacted for 2 hours. 13.23 g (0.09 mol) of compound
[16] (N,N-dimethylformamide diethyl acetal) was added as an esterifying agent and reacted at 40°C for 2 hours. After the reaction was completed, the liquid temperature was below 30°C, and 30 g of acetic acid was added. After stirring for 1 hour, the mixture was poured into 2 L of water, filtered, washed with water three times, and then dried in a vacuum dryer at 50° C. for 72 hours to obtain a resin C.
[0350] Example 4 (E4), Synthesis of Resin D
[0351] Except that compound [1] (3,5-diaminosalicylic acid, 0.4 mol) was used instead of DABA, the rest was the same as in Example 3. Resin D was obtained.
[0352] Example 5 (E5), Synthesis of Resin E
[0353] Except that compound [8] was used instead of compound [4], the rest was the same as Example 3. Resin E was obtained.
[0354] Example 6 (E6), Synthesis of Resin F
[0355] Except that compound
[14] was used instead of compound
[13] as the end-capping agent, the rest was the same as Example 5. Resin F was obtained.
[0356] Example 7 (E7), Synthesis of Resin G
[0357] Except that compound
[11] was used instead of compound OPDA, the rest was the same as Example 3. Resin G was obtained.
[0358] Example 8 (E8), Synthesis of Resin H
[0359] The same procedure as in Example 7 was followed except that compound
[13] was not used as the end-capping agent. Resin H was obtained.
[0360] Example 9 (E9), Synthesis of Resin I
[0361] The same procedure as in Example 8 was followed except that compound
[16] was not used as the esterification agent. Resin I was obtained.
[0362] Example 10 (E10), Synthesis of Resin J
[0363] Except that compound
[10] was used instead of compound [OPDA], the rest was the same as Example 3. Resin J was obtained.
[0364] Example 11 (E11), Synthesis of Resin K
[0365] Except that compound [8] was used instead of compound [4], the rest was the same as Example 10. Resin K was obtained.
[0366] Example 12 (E12), Synthesis of Resin L
[0367] Except that compound [7] was used instead of compound [4], the rest was the same as in Example 3. Resin L was obtained. Comparative Example 1 (C1), Synthesis of Resin M
[0368] Except that compound [9] was used instead of compound [4], the rest was the same as Example 10. Resin M was obtained. Comparative Example 2 (C2), Synthesis of Resin N
[0369] Except that compound DHB was substituted for compound [4], the rest was the same as in Example 1. Resin N was obtained. Comparative Example 3 (C3), Synthesis of Resin O
[0370] The same procedure as in Example 2 was followed except that compound [2] was substituted for compound [4]. Resin O was obtained. Comparative Example 4 (C4), Synthesis of Resin P
[0371] The same procedure as in Example 3 was followed except that compound [2] was used instead of compound [4]. Resin P was obtained. Comparative Example 5 (C5), Synthesis of Resin Q
[0372] The same procedure as in Example 7 was used except that compound [2] was substituted for compound [4]. Resin Q was obtained. Comparative Example 6 (C6), Synthesis of Resin R
[0373] Except that compound [6] was used instead of compound [4], the rest was the same as Example 7. Resin R was obtained.
[0374] The resin AL described in Examples 1-12 and the resin MR described in Comparative Examples 1-6 were dissolved in GBL to prepare a resin composition with a resin concentration of 30%. Then, the linear thermal expansion coefficient, absorbance, and drug resistance tests described in this application were performed, and the results are shown in Table 1.
[0375] Example 13 (E13)
[0376] 17.5 g of the resin G obtained in Example 7 and 2.3 g of the photoacid generator [c] obtained in Synthesis Example 13 were added to 45 g of GBL to prepare a photosensitive resin composition G1. The obtained photosensitive resin composition G1 was used to perform the linear thermal expansion coefficient, absorbance, drug resistance and photosensitivity tests described in the present application, and the results are shown in Table 2.
[0377] Example 14 (E14)
[0378] 17.5 g of the resin G obtained in Example 7 was weighed, and 0.5 g of the photopolymerization initiator [a] and 2.5 g of the photopolymerizable compound [b] were added to 45 g of GBL to prepare a photosensitive resin composition G2. The obtained photosensitive resin composition G2 was used to perform the linear thermal expansion coefficient, absorbance, drug resistance and photosensitivity tests described in this application, and the results are shown in Table 2.
[0379] Comparative Example 7 (C7)
[0380] 17.5 g of the resin Q obtained in Comparative Example 5 and 2.3 g of the photoacid generator [c] obtained in Synthesis Example 13 were added to 45 g of GBL to prepare a photosensitive resin composition Q1. The obtained photosensitive resin composition Q1 was used to perform the linear thermal expansion coefficient, absorbance, drug resistance and photosensitivity tests described in this application, and the results are shown in Table 2.
[0381] Comparative Example 8 (C9)
[0382] 17.5 g of the resin Q obtained in Comparative Example 5 was weighed, and 0.5 g of the photopolymer initiator [a] and 2.5 g of the photopolymerizable compound [b] were added to 45 g of GBL to prepare a photosensitive resin composition Q2. The obtained photosensitive resin composition Q2 was used to perform the linear thermal expansion coefficient, absorbance, drug resistance and photosensitivity tests described in this application, and the results are shown in Table 2.
[0383] Comparative Example 9 (C9)
[0384] 17.5 g of the resin M obtained in Comparative Example 6 and 2.3 g of the photoacid generator [c] obtained in Synthesis Example 13 were added to 45 g of GBL to prepare a photosensitive resin composition Q1. The obtained photosensitive resin composition M1 was used to perform the linear thermal expansion coefficient, absorbance, drug resistance and photosensitivity tests described in this application, and the results are shown in Table 2.
[0385] Table 1 (1-1 part, mol)
[0386]
[0387] Table 1 (1-2 parts, mol)
[0388]
[0389] Table 2
[0390]
[0391] In summary, the resin composition provided in the present application can obtain a resin film or photosensitive resin film with a linear thermal expansion coefficient of less than 40, an absorbance of less than 0.40, and a drug resistance of good level above Class C. Considering the reliability of forming a semiconductor device or a display device, the resin composition provided preferably can obtain a resin film or photosensitive resin film with a linear thermal expansion coefficient of less than 35, an absorbance of less than 0.35, and a drug resistance of good level above Class B. The semiconductor device, display device, etc. finally prepared have high reliability.
[0392] The specific embodiments of the present application are described in detail above, but they are only examples, and the present application is not limited to the specific embodiments described above. For those skilled in the art, any equivalent modifications and substitutions made to the present application are also within the scope of the present application. Therefore, the equalization changes and modifications made without departing from the spirit and scope of the present application should be included in the scope of the present application.
Claims
1. A polymer, characterized in that The polymer contains a structural unit represented by formula (1) and a structural unit represented by formula (2): Among them, R 1 An organic group having 2 to 20 carbon atoms in the main chain, and R 1 The main chain carries 1-4 carboxyl groups; the R 1 The carboxyl group contained is directly connected to R by a C-C covalent bond. 1 The main chain structure of R 1 The main chain contains any one or more of an aromatic hydrocarbon group and an aromatic group containing heteroatoms; the aromatic hydrocarbon group or the aromatic group containing heteroatoms is a cyclic structure, and is one cyclic structure or more cyclic structures; Among them, R 3 The structure includes: The structural unit shown in formula (2) is an imide structure shown in formula (3) and / or an amide structure shown in formula (4): Wherein, X is a tetravalent organic group containing 6 to 30 carbon atoms; R 4 and R 5 are independently selected from H, alkali metal ions, Si1-Si 20 Silane groups, C1-C 10 Hydrocarbon, C1-C 10 Hydrocarbylamine, C1-C 20 Hydrocarbyl-substituted imidazolyl, C1-C 20 Hydrocarbyl-substituted pyridyl, C1-C 20 Hydrocarbyl-substituted pyrrolyl, C1-C 20 Hydrocarbon-substituted pyranyl, C1-C 20 Hydrocarbon-substituted benzothiophenyl, C1-C 20 Hydrocarbon-substituted thienyl, C1-C 20 Hydrocarbyl-substituted indolyl, C1-C 20 Hydrocarbyl-substituted isoindolyl, C1-C 20 Hydrocarbon-substituted benzimidazole, C1-C 20 Hydrocarbyl-substituted carbazole, C1-C 20 Hydrocarbon-substituted oxazolyl, C1-C 20 Hydrocarbon-substituted thiazolyl, C1-C 20 Hydrocarbon-substituted isothiazolyl, C1-C 20 Hydrocarbyl-substituted pyridazinyl, C1-C 20 Hydrocarbyl-substituted pyrazolyl, C1-C 20 Hydrocarbyl-substituted acridinyl, C1-C 20 Hydrocarbyl-substituted quinolinyl.
2. The polymer according to claim 1, characterized in that The R 1 The main chain structure contains: any one or more of phenyl, biphenyl, anthracenyl, naphthyl, pyrenyl, pyridyl, pyridyl, pyrrolyl, pyranyl, benzothiophenyl, thienyl, indolyl, isoindolyl, imidazolyl, benzimidazolyl, carbazolyl, oxazole, thiazolyl, isothiazolyl, pyridazinyl, pyrazolyl, acridinyl, benzopyrenyl, quinolyl, or a connected structure of any two or more of the above groups.
3. The polymer according to claim 1 or 2, characterized in that The R 1 Also with one or more R 2 Group, the R 2 The group is H, a halogen atom, a monovalent organic group containing 1 to 20 carbon atoms, or a hydroxyl group.
4. The polymer according to claim 1 or 2, characterized in that The R 3 The main chain structure further contains -MQ-, wherein M is selected from any one or more of aliphatic hydrocarbons, aromatic hydrocarbons, and aromatic compounds containing heteroatoms; N is connected to M; The heteroatom is any one or more of O, S, and N; and Q is any one or more of -O-, -CO-O-, -NH-, -CO-NH-, -S-, and -N=CH-.
5. The polymer according to claim 4, characterized in that The M is any one or more of phenyl, biphenyl, anthracenyl, naphthyl, pyrenyl, pyridyl, bipyridyl, pyrrolyl, pyranyl, benzothiophenyl, thienyl, indolyl, isoindolyl, imidazolyl, benzimidazolyl, carbazolyl, oxazolyl, thiazolyl, isothiazolyl, pyridazinyl, pyrazolyl, acridinyl, benzopyrenyl, quinolyl, triazolyl, or a connected structure of any two or more of the above groups.
6. The polymer according to claim 1, characterized in that X is a tetracarboxyl compound residue or a tetracarboxylic dianhydride compound residue.
7. The polymer according to claim 6, characterized in that The X is a structure shown in formula (5): The ring in formula (5) is a linear alkyl group, an organic group containing a cycloalkyl group, or an organic group containing an aromatic ring.
8. The polymer according to claim 7, characterized in that The ring in formula (5) is an aliphatic ring or an aromatic ring.
9. The polymer according to claim 7, characterized in that The ring in formula (5) is selected from: a tetravalent butane group, a cyclopentane group, a cyclobutane group, a biphenyl group, or any one or more of the groups represented by formula (6): The ring in formula (6) is an aromatic ring or an aliphatic ring; R 6 C1-C 10 Linear hydrocarbon groups, C3-C 30 Cyclic hydrocarbon groups, C5-C 30 Aromatic group, -W1-R 7 -W2-、Si1-Si 20 any one or more of -HN-, -CO-O-, -O-, -CO-NH-, -CO-, -N=CH-, or any two or more of the above groups connected by covalent bonds; wherein W1 and W2 are independently selected from any one or more of -HN-, -CO-O-, -O-, -CO-NH-, -CO-, -S-, -N=CH-, and R 7 Selected from C5-C 30 Aromatic groups, C5-C 30 Aromatic groups, Si1-Si 20 Silane groups, C1-C 10 Linear hydrocarbon groups, C1-C 20 Hydrocarbyl-substituted imidazolyl, C1-C 20 Hydrocarbon-substituted pyridyl, C1-C 20 Hydrocarbyl-substituted pyrrolyl, C1-C 20 Hydrocarbyl-substituted pyranyl, C1-C 20 Hydrocarbon-substituted benzothiophenyl, C1-C 20 Hydrocarbon-substituted thienyl, C1-C 20 Hydrocarbyl-substituted indolyl, C1-C 20 Hydrocarbyl-substituted isoindolyl, C1-C 20 Hydrocarbon-substituted benzimidazole, C1-C 20 Hydrocarbyl-substituted carbazole, C1-C 20 Hydrocarbon-substituted oxazolyl, C1-C 20 Hydrocarbon-substituted thiazolyl, C1-C 20 Hydrocarbon-substituted isothiazolyl, C1-C 20 Hydrocarbyl-substituted pyridazinyl, C1-C 20 Hydrocarbyl-substituted pyrazolyl, C1-C 20 Hydrocarbyl-substituted acridinyl, C1-C 20 Any one or more of quinolyl substituted with a hydrocarbyl group.
10. The polymer according to claim 6, characterized in that X is a structure shown in formula (7-1): R 7 selected from C5-C30 aromatic groups, C5-C30 aromatic groups containing heteroatoms, Si1-Si20 silyl groups, C1-C10 linear hydrocarbon groups, C1-C20 hydrocarbon-substituted imidazolyl groups, C1-C20 hydrocarbon-substituted pyridyl groups, C1-C20 hydrocarbon-substituted pyrrolyl groups, C1-C20 hydrocarbon-substituted pyranyl groups, C1-C20 hydrocarbon-substituted benzothiophenyl groups, C1-C20 hydrocarbon-substituted thienyl groups, C1-C20 hydrocarbon-substituted indolyl groups, C1-C20 hydrocarbon-substituted any one or more of a C1-C20 alkyl-substituted isoindolyl, a C1-C20 alkyl-substituted benzimidazolyl, a C1-C20 alkyl-substituted carbazolyl, a C1-C20 alkyl-substituted oxazolyl, a C1-C20 alkyl-substituted thiazolyl, a C1-C20 alkyl-substituted isothiazolyl, a C1-C20 alkyl-substituted pyridazinyl, a C1-C20 alkyl-substituted pyrazolyl, a C1-C20 alkyl-substituted acridinyl, and a C1-C20 alkyl-substituted quinolyl.
11. The polymer according to claim 1, characterized in that The polymer is polyamide, polyimide, polyimide precursor, polybenzoxazole, polybenzoxazole precursor, or a copolymer thereof.
12. The polymer according to claim 11, characterized in that The weight average molecular weight of the polymer is 3,000-1,000,000.
13. The polymer according to claim 12, characterized in that The average molecular weight of the polymer is 5,000-500,000.
14. The polymer according to claim 13, characterized in that The average molecular weight of the polymer is 8,000-200,000.
15. A resin composition, characterized in that Including the polymer described in claim 1; or, comprising a first polymer containing a structural unit represented by formula (1) and a second polymer containing a structural unit represented by formula (2), wherein the first polymer and the second polymer are selected from at least one or more of polyamide, polyimide, polyimide precursor, polybenzoxazole, polybenzoxazole precursor, or copolymers thereof.
16. The resin composition according to claim 15, characterized in that The resin composition further comprises a photosensitizer; the photosensitizer is a photoacid generator or a photopolymer initiator.
17. The resin composition according to claim 16, characterized in that The photoacid generator is one or more of quinonediazide compounds, sulfonium salt compounds, phosphonium salt compounds, diazonium salt compounds, and iodonium salt compounds.
18. The resin composition according to claim 16, characterized in that The photopolymer initiator is a combination of at least one of a free radical initiator, a cationic initiator, an anionic initiator, and a zwitterionic initiator, or more.
19. The resin composition according to claim 16, characterized in that The photopolymerization initiator is used in combination with a photopolymerizable compound.
20. The resin composition according to claim 16, characterized in that The photoacid generator or photopolymer initiator accounts for ≤50 weight % of the resin composition.
21. The resin composition according to claim 20, characterized in that The photoacid generator or photopolymer initiator accounts for 0.5-30 weight % of the resin composition.
22. The resin composition according to claim 21, characterized in that The photoacid generator or photopolymer initiator accounts for 2-20 wt % of the resin composition.
23. The resin composition according to claim 16, characterized in that The resin composition further includes a sensitizer.
24. The resin composition according to claim 23, characterized in that The sensitizer is a free radical photoinitiator or a cationic photoinitiator.
25. The resin composition according to claim 23, characterized in that The sensitizer is one or more of aromatic diazonium salts, diaryl iodine compounds, triaryl sulfide compounds, benzoin and its derivatives, acetophenone derivatives, and aromatic ketone compounds.
26. The resin composition according to claim 25, characterized in that The benzoin and its derivatives are benzoin ether.
27. The resin composition according to claim 25, characterized in that The acetophenone derivative is a dialkoxyacetophenone or a chlorinated acetophenone derivative.
28. The resin composition according to claim 25, characterized in that The aromatic ketone compound is one or more of 4,4'-dimethylaminobenzophenone and thioxanthone compounds.
29. The resin composition according to claim 16, characterized in that The resin composition further includes a thermal crosslinking agent.
30. The resin composition according to claim 29, characterized in that The thermal crosslinking agent is one or more of a methylol compound, a methoxymethylol compound, a urea compound, an epoxy compound, and an oxetane compound.
31. The resin composition according to claim 29 or 30, characterized in that The thermal crosslinking agent accounts for 0.5-50% by weight of the resin composition.
32. The resin composition according to claim 31, characterized in that The thermal crosslinking agent accounts for 3-40% by weight of the resin composition.
33. The resin composition according to claim 16, characterized in that The resin composition further comprises one or more of a surface modifier, a capping agent, filler particles and a solvent.
34. A resin film, characterized in that Containing the polymer described in any one of claims 1 to 14, or containing the resin composition described in any one of claims 15 to 33; or, prepared from the polymer described in any one of claims 1 to 14, or the resin composition described in any one of claims 15 to 33.
35. A semiconductor device, characterized in that: A composition comprising the polymer according to any one of claims 1 to 14, a resin composition according to any one of claims 15 to 33, or a resin film according to claim 34.
36. A light emitting device, characterized in that: A composition comprising the polymer according to any one of claims 1 to 14, a resin composition according to any one of claims 15 to 33, or a resin film according to claim 34.
37. A method for preparing the polymer according to claim 1 or the resin composition according to claim 15, characterized in that: The method comprises subjecting a monomer represented by formula (1-1) or a monomer represented by formula (2-1) to a condensation polymerization reaction with a carboxyl group of a monomer containing at least two carboxyl groups, a haloacyl group of a monomer containing at least two haloacyl groups, or an anhydride group of a monomer containing at least one anhydride group to obtain the polymer or resin composition: Among them, R 1 and R 3 As defined in claim 1.