A dyeing and finishing process for washable cotton grey fabric

By adding enzyme treatment agents to the pure cotton grey cloth dyeing and finishing process, and adding alkaline reagents and liquid ammonia multiple times to finish, the problems of low color fastness after dyeing and excessive water use in the prior art are solved, and higher resistance is achieved Washing and color fastness, and reduce water consumption and shrinkage.

CN115679721BActive Publication Date: 2024-11-15NANTONG FREYA TEXTILE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211461442.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-16
Publication Date
2024-11-15
Estimated Expiration
2042-11-16

AI Technical Summary

Technical Problem

The existing pure cotton grey cloth dyeing and finishing process cannot meet more than 30 water washing tests after dyeing, the color fastness does not meet the requirements, and the water consumption is large, and the process steps are independent, resulting in low efficiency.

Method used

A dyeing and finishing process of washing-resistant cotton grey cloth is adopted, including pretreatment, dyeing and liquid ammonia finishing steps. In the pretreatment, the enzyme treatment agent is added to remove hair and hydrogen peroxide, and the bath ratio is limited to reduce waste of water resources; alkaline reagents are added multiple times to improve color fastness; liquid ammonia finishing changes the fiber structure, improves softness and reduces friction.

Benefits of technology

It improves the water resistance and color fastness of pure cotton grey fabrics, reduces water resource consumption, and makes the fabric soft and smooth, reducing shrinkage.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a dyeing and finishing process for washable pure cotton grey cloth, which adopts pre-treatment, dyeing, mechanical finishing and liquid ammonia finishing processes for dyeing and finishing, and mainly improves the overall color fastness of the pure cotton grey cloth by enhancing the interaction between the dye solution and the cotton fiber. The advantages of the invention are that the water washing resistance of the pure cotton grey cloth is enhanced, the color fastness is increased, the processing efficiency is improved, and the consumption of water resources is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of textile printing and dyeing, in particular to a dyeing and finishing process for washable pure cotton grey cloth. Background Art

[0002] As a pure textile fabric, pure cotton grey cloth is woven only by using a single cotton fiber. After weaving, the pure cotton grey cloth needs to be dyed and finished. For the dyeing and finishing of pure cotton grey cloth, a long-machine continuous padding process is mostly used. The process steps are: turning the seams, then singeing, one front and one back, followed by desizing, washing, drying, mercerizing, then rolling and drying, and then alkali fixing, soaping, washing, drying, stretching, finishing and packaging to obtain the product.

[0003] However, fabrics treated with this process usually cannot meet the washing test after dyeing. It is difficult to withstand more than 30 industrial washes without fading, and its color fastness does not meet the requirements at all. At the same time, since each step is relatively independent, the amount of water used each time is also quite large. Summary of the invention

[0004] The purpose of the present invention is to provide a dyeing and finishing process for washable pure cotton grey fabric, which can enhance the water washing resistance of the pure cotton grey fabric, increase the color fastness, improve the processing efficiency and reduce the consumption of water resources.

[0005] The above technical objectives of the present invention are achieved through the following technical solutions:

[0006] A dyeing and finishing process for washable pure cotton grey fabric, characterized by comprising the following steps:

[0007] Pretreatment: immerse the cotton grey cloth in water, stop adding water when the bath ratio reaches 10, heat the water to 50℃, add hydrogen peroxide, caustic soda, penetrant and degreaser in the same bath, stir evenly, heat to 98℃ and wash for 30-60min, cool to 80℃ and drain the water after washing, add water for the second time when the bath ratio reaches 10, stop adding water when the bath ratio reaches 10, heat the water to 50℃ and add acid neutralizer for neutralization treatment for 10-20min, drain the water after treatment, add water for the third time when the bath ratio reaches 10, add enzyme treatment agent to the water for 10-20min, drain all the water after treatment;

[0008] Dyeing: Immerse the pre-treated cotton grey fabric in water, stop adding water when the bath ratio reaches 4, heat the water to 40°C and add the auxiliaries, add the dye after 10-20 minutes, add a large amount of sodium sulfate after dyeing for 10-20 minutes, heat to 60°C after 10 minutes, add alkaline reagent several times for color fixation reaction, drain the water after 50-60 minutes, and then perform soap boiling and water washing to remove floating color;

[0009] Mechanical finishing: After dyeing, the cotton grey fabric is overfed by the overfeeding device and expanded by the heat setting machine. After completion, it enters the drying room for drying and then cools to room temperature.

[0010] Liquid ammonia finishing: The cotton grey fabric after mechanical finishing is first tension adjusted and steamed, then cooled and immersed in anhydrous liquid ammonia in a sealed box. The surface of the cotton grey fabric is evenly covered with anhydrous liquid ammonia by rollers, and then the ammonia gas is removed in a steamer, and then the fabric is washed three times and dried.

[0011] Preferably, the mass ratio of hydrogen peroxide, caustic soda, penetrant, one-bath degreaser to cotton grey fabric in (1) is (15-18):(3-4):(2-3):1:(200-250), the penetrant is selected from one of alkali-resistant penetrant OEP-70, alkali-resistant penetrant AEP or fatty alcohol polyoxyethylene ether phosphate, and the one-bath degreaser is selected from one of one of one-bath degreaser TF-128E or one-bath degreaser BF-302.

[0012] Preferably, the neutral acid neutralizer (1) is glacial acetic acid, and the mass ratio of the acid neutralizer to the pure cotton grey fabric is 1:(200-250).

[0013] Preferably, the mass ratio of the enzyme treatment agent to the pure cotton grey cloth in (1) is 1: (1000-1200), the enzyme treatment agent includes a neutral polishing enzyme and a high-concentration deoxygenase, wherein the neutral polishing enzyme accounts for 35%-40%, the neutral polishing enzyme is selected from one of the neutral polishing enzyme MCH-122, the neutral polishing enzyme TY-C5B or the neutral polishing enzyme JN-156, and the high-concentration deoxygenase is selected from one of the high-concentration deoxygenase QTQ-101 or the high-concentration deoxygenase DM-8697.

[0014] Preferably, the cooling and heating rates in (1) are both 2-2.5°C / min, and the heating and heating rates in (2) are both 1.5-2.0°C / min.

[0015] Preferably, the auxiliary agent in (2) comprises soda ash and a chelating dispersant, and the mass ratio of the soda ash, the chelating dispersant, sodium sulfate and the pure cotton grey cloth is (5-8):1:(35-40):(250-300).

[0016] Preferably, the alkaline agent in (2) is selected from one of the substitute alkali RG-JD100 and the substitute alkali DH-801, the mass ratio of the alkaline agent to the pure cotton grey cloth is 1: (80-90), and the alkaline agent is added three times, the addition amounts are 1 / 10, 2 / 10 and 7 / 10 respectively, and the three addition times are all separated by 10 minutes.

[0017] Preferably, the overfeeding amount of the pure cotton grey fabric in (3) is 3%-7%, the expansion amount is 7%-11%, and the drying temperature in the drying room is 150-180°C.

[0018] Preferably, the tension adjustment range in (4) is 20-40N, the steam drying temperature is 90-95°C, and the anhydrous liquid ammonia temperature is -33 to -35°C.

[0019] In summary, the present invention has the following beneficial effects:

[0020] 1. The present invention adds an enzyme treatment agent during the pretreatment process to achieve corrosion and removal of the outer hairiness of the pure cotton grey cloth, while eliminating the internal hydrogen peroxide, preventing subsequent dyeing color spots, and improving the dyeing color fastness of the pure cotton grey cloth in the later stage. At the same time, the bath ratio is limited during the treatment process to reduce unnecessary waste of water resources.

[0021] 2. In the dyeing process, the present invention adds alkaline reagents for many times to improve the color fastness of the fabric, because the dye first moves from the dye solution to the surface of the cotton fiber, and then is adsorbed on the surface of the cotton fiber under the action of hydrogen bonds and van der Waals attraction, and then diffuses into the interior of the cotton fiber, and reacts with the cotton fiber under the condition of the alkaline reagent to form covalent bonds for fixation. Subsequently, the pure cotton grey cloth is soaped. After the dye is dyed and fixed, there will be a lot of floating dyes, excess alkali agents, and fixed dyes in the cotton fiber. The floating dye is composed of dyes that have not reacted with it on the surface of the cotton fiber and hydrolyzed dyes, and is the main factor affecting the color fastness of the fabric. After the fixation reaction, the pure cotton grey cloth is soaped and washed to remove the floating color, thereby improving the color fastness.

[0022] 3. The present invention changes the transverse and longitudinal structures of the cotton fibers and improves the performance of the cotton fibers by subjecting the cotton fibers to liquid ammonia finishing, so that the pure cotton grey cloth can have a soft and smooth feel without adding a softener. At the same time, the liquid ammonia finishing process is optimized, which can effectively improve the treatment effect of liquid ammonia on the fibers, effectively reduce friction, and at the same time give the fabric a certain tension effect, thereby preventing the shrinkage of the fabric and reducing the shrinkage rate. DETAILED DESCRIPTION

[0023] The specific implementation modes of the present invention are further described below, and these embodiments do not constitute a limitation of the present invention. Example 1

[0024] A dyeing and finishing process for washable all-cotton grey fabric, comprising the following steps:

[0025] Pretreatment: immerse the cotton grey fabric in water, stop adding water when the bath ratio reaches 10, heat the water to 50℃, add hydrogen peroxide, caustic soda, penetrant and same-bath degreaser, the mass ratio of hydrogen peroxide, caustic soda, penetrant, same-bath degreaser to cotton grey fabric is 15:3:2:1:200, the penetrant is alkali-resistant penetrant OEP-70, the same-bath degreaser is same-bath degreaser TF-128E, stir evenly, heat to 98℃ at 2℃ / min, and then boil and wash for 30min, after boiling and washing, cool to 80℃ at 2℃ / min, and drain the water, after drainage, add water for the second time, when the bath ratio reaches After the bath ratio reaches 10, stop adding water, heat the water to 50°C, add acidic neutralizer glacial acetic acid for neutralization treatment for 10 minutes, the mass ratio of acidic neutralizer to pure cotton grey cloth is 1:200, drain the water after the treatment is completed, add water for the third time, stop adding water when the bath ratio reaches 10, add enzyme treatment agent to the water for treatment for 10 minutes, drain all the water after the treatment is completed, the mass ratio of enzyme treatment agent to pure cotton grey cloth is 1:1000, the enzyme treatment agent includes neutral polishing enzyme MCH-122 and high concentration deoxygenation enzyme QTQ-101, of which neutral polishing enzyme MCH-122 accounts for 35%.

[0026] Dyeing: immerse the cotton grey fabric after pretreatment in water, stop adding water when the bath ratio reaches 4, heat the water to 40°C at a rate of 1.5°C / min, and then add auxiliaries, including soda ash and chelating dispersants. Add dyes after 10 minutes for dyeing. After dyeing for 10 minutes, add a large amount of sodium sulfate. After reacting for 10 minutes, heat to 60°C, and then add alkaline reagents for fixation reaction several times. The alkaline reagent is the substitute alkali RG-JD100. The mass ratio of alkaline reagent to pure cotton grey fabric is 1:80. The alkaline reagent is added three times, and the addition amounts are 1 / 10, 2 / 10 and 7 / 10 respectively. The three addition times are 10 minutes apart. After a total of 50 minutes, the water is discharged, and then soap boiling and water washing are performed to remove floating color. The mass ratio of soda ash, chelating dispersant, sodium sulfate and pure cotton grey fabric is 5:1:35:250.

[0027] Mechanical finishing: After dyeing, the cotton grey cloth is overfed by an overfeeding device and expanded by a heat setting machine. The overfeeding amount is 3% and the expansion amount is 7%. After completion, it enters the drying room for drying at a drying temperature of 150°C and then cools to room temperature.

[0028] Liquid ammonia finishing: The cotton grey fabric after mechanical finishing is first tension adjusted and steamed. The tension adjustment range is 20N and the steaming temperature is 90℃. After cooling, it is immersed in -33℃ anhydrous liquid ammonia in a sealed box. The surface of the cotton grey fabric is evenly covered with anhydrous liquid ammonia by a roller. Subsequently, the ammonia involved is removed in a steamer, and then the fabric is washed three times and dried. Example 2

[0029] A dyeing and finishing process for washable all-cotton grey fabric, comprising the following steps:

[0030] Pretreatment: immerse the cotton grey fabric in water, stop adding water when the bath ratio reaches 10, heat the water to 50℃, add hydrogen peroxide, caustic soda, penetrant and same-bath degreaser, the mass ratio of hydrogen peroxide, caustic soda, penetrant, same-bath degreaser to cotton grey fabric is 16:4:2:1:220, the penetrant is alkali-resistant penetrant AEP, the same-bath degreaser is same-bath degreaser BF-302, stir evenly, heat to 98℃ at 2℃ / min, and then boil and wash for 50min, after boiling and washing, cool to 80℃ at 2℃ / min, and drain the water, after drainage, add water for the second time, when the bath ratio reaches After 10, stop adding water, heat the water to 50℃, add acidic neutralizer glacial acetic acid for neutralization treatment for 15 minutes, the mass ratio of acidic neutralizer to pure cotton grey cloth is 1:230, drain the water after the treatment is completed, add water for the third time, stop adding water when the bath ratio reaches 10, add enzyme treatment agent to the water for treatment for 15 minutes, drain all the water after the treatment is completed, the mass ratio of enzyme treatment agent to pure cotton grey cloth is 1:1100, the enzyme treatment agent includes neutral polishing enzyme TY-C5B and high concentration deoxygenation enzyme QTQ-101, of which neutral polishing enzyme TY-C5B accounts for 37%.

[0031] Dyeing: immerse the cotton grey fabric after pretreatment in water, stop adding water when the bath ratio reaches 4, heat the water to 40℃ at a rate of 2.0℃ / min, and then add auxiliaries, including soda ash and chelating dispersants. Add dyes after 15 minutes for dyeing. After dyeing for 15 minutes, add a large amount of sodium sulfate. After reacting for 10 minutes, heat to 60℃, and then add alkaline reagents for fixing reaction several times. The alkaline reagent is the substitute alkali DH-801. The mass ratio of alkaline reagent to pure cotton grey fabric is 1:85. The alkaline reagent is added three times, and the addition amounts are 1 / 10, 2 / 10 and 7 / 10 respectively. The three addition times are 10 minutes apart. After a total of 50-60 minutes, the water is discharged, and then soap boiling and water washing are performed to remove floating color. The mass ratio of soda ash, chelating dispersant, sodium sulfate and pure cotton grey fabric is 7:1:40:280.

[0032] Mechanical finishing: After dyeing, the cotton grey cloth is overfed by an overfeeding device and expanded by a heat setting machine. The overfeeding amount is 5% and the expansion amount is 9%. After completion, it enters the drying room for drying at a drying temperature of 170°C and then cools to room temperature.

[0033] Liquid ammonia finishing: The cotton grey fabric after mechanical finishing is first tension adjusted and steamed. The tension adjustment range is 30N and the steaming temperature is 90℃. After cooling, it is immersed in -34℃ anhydrous liquid ammonia in a sealed box. The surface of the cotton grey fabric is evenly covered with anhydrous liquid ammonia by a roller. Subsequently, the ammonia involved is removed in a steamer, and then the fabric is washed three times and dried. Example 3

[0034] A dyeing and finishing process for washable all-cotton grey fabric, comprising the following steps:

[0035] Pretreatment: immerse the cotton grey fabric in water, stop adding water when the bath ratio reaches 10, heat the water to 50℃, add hydrogen peroxide, caustic soda, penetrant and same-bath degreaser, the mass ratio of hydrogen peroxide, caustic soda, penetrant, same-bath degreaser to cotton grey fabric is 18:4:3:1:250, the penetrant is fatty alcohol polyoxyethylene ether phosphate, the same-bath degreaser is same-bath degreaser BF-302, stir evenly, heat to 98℃ at 2.5℃ / min, and then boil and wash for 60min, after boiling and washing, cool to 80℃ at 2.5℃ / min, and drain the water, after drainage, add water for the second time, when Stop adding water after the bath ratio reaches 10, heat the water to 50°C, add acidic neutralizer glacial acetic acid for neutralization treatment for 20 minutes, the mass ratio of acidic neutralizer to pure cotton grey cloth is 1:250, drain the water after the treatment is completed, add water for the third time, stop adding water when the bath ratio reaches 10, add enzyme treatment agent to the water for 20 minutes, drain all the water after the treatment is completed, the mass ratio of enzyme treatment agent to pure cotton grey cloth is 1:1200, the enzyme treatment agent includes neutral polishing enzyme JN-156 and high concentration deoxygenation enzyme QTQ-101, of which neutral polishing enzyme JN-156 accounts for 40%.

[0036] Dyeing: immerse the cotton grey fabric after pretreatment in water, stop adding water when the bath ratio reaches 4, heat the water to 40°C at a rate of 2.0°C / min, and then add auxiliaries, including soda ash and chelating dispersants. Add dyes after 20 minutes for dyeing. After dyeing for 20 minutes, add a large amount of sodium sulfate. After reacting for 10 minutes, heat to 60°C, and then add alkaline reagents for fixation reaction. The alkaline reagent is the substitute alkali RG-JD100. The mass ratio of alkaline reagent to pure cotton grey fabric is 1:90. The alkaline reagent is added three times, and the addition amounts are 1 / 10, 2 / 10 and 7 / 10 respectively. The three addition times are 10 minutes apart. After a total of 60 minutes, the water is discharged, and then soap boiling and water washing are performed to remove floating color. The mass ratio of soda ash, chelating dispersant, sodium sulfate and pure cotton grey fabric is 8:1:40:300.

[0037] Mechanical finishing: After dyeing, the cotton grey cloth is overfed by an overfeeding device and expanded by a heat setting machine. The overfeeding amount is 7% and the expansion amount is 11%. After completion, it enters the drying room for drying at a drying temperature of 180°C and then cools to room temperature.

[0038] Liquid ammonia finishing: The cotton grey fabric after mechanical finishing is first tension adjusted and steamed. The tension adjustment range is 40N and the steaming temperature is 95℃. After cooling, it is immersed in -35℃ anhydrous liquid ammonia in a sealed box. The surface of the cotton grey fabric is evenly covered with anhydrous liquid ammonia by a roller. Subsequently, the ammonia involved is removed in a steamer, and then the fabric is washed three times and dried.

[0039] The dyed cotton grey fabrics obtained in the above-mentioned Examples 1 to 3 were tested for color fastness to washing, color fastness to perspiration, color fastness to rubbing, color fastness to dry heat, and cylinder difference with the cotton grey fabrics prepared by the long-wheel continuous pad dyeing process in the prior art. The cotton grey fabrics prepared by the long-wheel continuous pad dyeing process in the prior art were used as control examples. The test results are shown in Table 1 below:

[0040] Table 1 shows the performance test results of various embodiments and control examples.

[0041] test Example 1 Example 2 Example 3 Comparative Example Color fastness to washing Level 5 Level 5 Level 5 Level 4 and above Color fastness to perspiration Level 5 Level 5 Level 5 Level 4 and above Color fastness to rubbing Level 4 and above Level 5 Level 4 and above Level 4 Color fastness to dry heat Level 5 Level 4 and above Level 5 Level 4 and above Cylinder difference Level 5 Level 4 and above Level 5 Level 4

[0042] Among them, the color fastness standards are divided into 5 levels, with level 5 being the best and level 1 being the worst.

[0043] The above test results show that the pure cotton grey cloth obtained by the dyeing and finishing process provided in Examples 1 to 3 has a natural color and a soft fabric, and its color fastness to washing, color fastness to perspiration, color fastness to friction, color fastness to dry heat and cylinder difference all reach level 4 or above, which is far superior to the pure cotton grey cloth obtained by the normal long-machine continuous pad dyeing process in the prior art.

[0044] The invention adds an enzyme treatment agent in the pre-treatment process to realize the corrosion removal of the outer hairiness of the pure cotton grey cloth, eliminates the hydrogen peroxide inside, prevents the subsequent dyeing color flower, improves the dyeing color fastness of the pure cotton grey cloth in the later stage, and limits the bath ratio in the treatment process to reduce unnecessary waste of water resources. In addition, alkaline reagents are added multiple times in the dyeing process to improve the color fastness of the fabric, because the dye first moves from the dye solution to the cotton fiber surface, then adsorbs on the cotton fiber surface under the action of hydrogen bonds and van der Waals attraction, and then diffuses into the inside of the cotton fiber, and reacts with the cotton fiber under the condition of the alkaline reagent to generate covalent bonds for fixation, and then soaps the pure cotton grey cloth. After the dye is dyed and fixed, there will be a lot of floating dyes, excess alkali agents, and fixed dyes in the cotton fiber. The floating dyes are composed of dyes that do not react with the cotton fiber surface and hydrolyzed dyes, and are the main factors affecting the color fastness of the fabric. After the fixation reaction, the pure cotton grey cloth is soaped and washed to remove the floating color, thereby improving the color fastness. In addition, by treating cotton fibers with liquid ammonia, the transverse and longitudinal structures of the cotton fibers can be changed and the performance of the cotton fibers can be improved. The pure cotton grey cloth can have a soft and smooth feel without adding softener. At the same time, the liquid ammonia finishing process is optimized to effectively improve the treatment effect of liquid ammonia on the fibers, effectively reduce friction, and give the fabric a certain tension, which can prevent the shrinkage of the fabric and reduce the shrinkage rate.

[0045] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Those skilled in the art may make various modifications or equivalent substitutions to the present invention within the essence and protection scope of the present invention, and such modifications or equivalent substitutions should also be deemed to fall within the protection scope of the technical solution of the present invention.

Claims

1. A dyeing and finishing process for washable cotton grey fabric, characterized in that: The steps include: (1) Pretreatment: Immerse the cotton grey fabric in water. When the bath ratio reaches 10, stop adding water. Heat the water to 50°C and add hydrogen peroxide, caustic soda, penetrant and degreaser. Stir evenly and heat to 98°C for 30-60 minutes. After boiling and washing, cool to 80°C and drain the water. After drainage, add water for the second time. When the bath ratio reaches 10, stop adding water. Heat the water to 50°C and add acid neutralizer for neutralization for 10-20 minutes. After treatment, drain the water. After drainage, add water for the third time. When the bath ratio reaches 10, stop adding water. Add enzyme treatment agent to the water for 10-20 minutes. After treatment, drain all the water. (2) Dyeing: Immerse the pre-treated cotton grey fabric in water. When the bath ratio reaches 4, stop adding water. Heat the water to 40°C and add the auxiliaries. After 10-20 minutes, add the dye for dyeing. After dyeing for 10-20 minutes, add a large amount of sodium sulfate. After reacting for 10 minutes, heat to 60°C, add alkaline reagent several times for color fixation reaction. After 50-60 minutes, drain the water, and then perform soap boiling and water washing to remove floating color. The auxiliary agent includes soda ash and a chelating dispersant, and the mass ratio of the soda ash, the chelating dispersant, sodium sulfate and the pure cotton grey cloth is (5-8):1:(35-40):(250-300); The alkaline agent is selected from the substitute alkali RG-JD100, the mass ratio of the alkaline agent to the pure cotton grey cloth is 1: (80-90), the alkaline agent is added three times, the addition amounts are 1 / 10, 2 / 10 and 7 / 10 respectively, and the three addition times are all separated by 10 minutes; (3) Mechanical finishing: After dyeing, the cotton grey fabric is overfed through an overfeeding device and expanded using a heat setting machine. After completion, it is dried in a drying room and subsequently cooled to room temperature. (4) Liquid ammonia finishing: The cotton grey fabric after mechanical finishing is first tension-adjusted and steam-dried, then cooled and immersed in anhydrous liquid ammonia in a sealed box. The surface of the cotton grey fabric is evenly covered with anhydrous liquid ammonia by rollers, and then the ammonia gas is removed in a steamer. The fabric is then washed three times and dried.

2. The dyeing and finishing process of a washable cotton grey fabric according to claim 1, characterized in that: The mass ratio of hydrogen peroxide, caustic soda, penetrant, one-bath degreaser to cotton grey fabric in (1) is (15-18):(3-4):(2-3):1:(200-250), the penetrant is selected from one of alkali-resistant penetrant OEP-70, alkali-resistant penetrant AEP or fatty alcohol polyoxyethylene ether phosphate, and the one-bath degreaser is selected from one of one of one-bath degreaser TF-128E or one-bath degreaser BF-302.

3. The dyeing and finishing process of a washable cotton grey fabric according to claim 1, characterized in that: The (1) neutral acid neutralizer is glacial acetic acid, and the mass ratio of the acid neutralizer to the pure cotton grey fabric is 1:(200-250).

4. The dyeing and finishing process of a washable cotton grey fabric according to claim 1, characterized in that: The mass ratio of the enzyme treatment agent in (1) to the pure cotton grey cloth is 1: (1000-1200), the enzyme treatment agent includes a neutral polishing enzyme and a high-concentration deoxygenase, wherein the neutral polishing enzyme accounts for 35%-40%, the neutral polishing enzyme is selected from one of the neutral polishing enzyme MCH-122, the neutral polishing enzyme TY-C5B or the neutral polishing enzyme JN-156, and the high-concentration deoxygenase is selected from one of the high-concentration deoxygenase QTQ-101 or the high-concentration deoxygenase DM-8697.

5. The dyeing and finishing process of a washable cotton grey fabric according to claim 1, characterized in that: The cooling and heating rates in (1) are both 2-2.5°C / min, and the heating and heating rates in (2) are both 1.5-2.0°C / min.

6. The dyeing and finishing process of a washable pure cotton grey fabric according to claim 1, characterized in that: In the above (3), the overfeeding amount of the pure cotton grey cloth is 3%-7%, the expansion amount is 7%-11%, and the drying temperature in the drying room is 150-180°C.

7. The dyeing and finishing process of a washable pure cotton grey fabric according to claim 1, characterized in that: The tension adjustment range of (4) is 20-40N, the steam drying temperature is 90-95°C, and the anhydrous liquid ammonia temperature is -33 to -35°C.