A calcined three-in-one mica tape and its manufacturing process

By composite glass fiber cloth and modified BOPP film in mica tape, the bidirectional tensile properties of high viscosity glue and modified BOPP film are solved, and the weakness of single-sided calcined mica tape under high-temperature flame conditions is significantly improved. Refractory breakdown resistance and production efficiency.

CN115691859BActive Publication Date: 2024-11-19PAMICA IND (HUBEI) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211278458.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-19
Publication Date
2024-11-19
Estimated Expiration
2042-10-19

AI Technical Summary

Technical Problem

The single-sided calcined mica belt has unstable fire resistance under high temperature flame conditions, which is prone to cable breakdown. The weak points are caused by the random distribution of mica scales and insufficient glue penetration, which affects the fire resistance insulation level.

Method used

Using a calcined three-in-one mica tape, the two-way tensile properties of high viscosity glue and modified BOPP film are used to ensure uniform coverage and penetration of glue by compositeing fiberglass cloth, silicone glue water and modified BOPP film on both sides of the mica paper. Fill in weaknesses and improve overall performance.

Benefits of technology

The refractory and breakdown level of mica belt was improved. In 20 refractory tests, all passed 750℃90min, and 17 passed 950℃180min detection 17 times, overcoming the weaknesses of single-sided calcined mica belt, adhesion conductors and powder loss problems, improving The refractory performance and production efficiency of the cable are provided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003897552120000061
    Figure BDA0003897552120000061
  • Figure BDA0003897552120000081
    Figure BDA0003897552120000081
  • Figure BDA0003897552120000091
    Figure BDA0003897552120000091
Patent Text Reader

Abstract

The present invention provides a calcined three-in-one mica tape and a manufacturing process thereof, belonging to the technical field of mica tape. From one side of the calcined three-in-one mica tape to the other side, glass fiber cloth, organic silica gel water, calcined mica paper, high-viscosity coating glue, and modified BOPP film are compounded in sequence, and the thickness of the mica tape is 0.13-0.15 mm; high-quality mica material is selected and calcined to obtain calcined mica material, the calcined mica material is crushed by a water wet method, and calcined mica slurry is obtained by preferential grading, and the calcined mica slurry is made, pressed, dried, and rolled to obtain calcined mica paper; the machine is turned on for gluing: glass fiber cloth is put into a glue tank for evenly gluing, and the glue is organic silica gel water; the composite surface of the modified BOPP film is glued, and the glue is high-viscosity glue; compounding: glass fiber cloth and modified BOPP film are compounded on both sides of mica paper simultaneously, and the semi-finished mica tape is obtained by drying and curing in a drying tunnel; the calcined refractory mica tape is obtained by rolling, slitting, and winding. The invention has the advantages of high fire resistance and breakdown resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of mica tapes and relates to a calcined three-in-one mica tape and a manufacturing process thereof. Background Art

[0002] As the main fire-resistant insulation layer in fire-resistant cables, the mica tape wrapping layer is the key component to ensure cable insulation under continuous flame temperature. The performance of the mica tape needs to be tested based on the fire-resistant cable, that is, when the fire-resistant insulated cable is energized (with a certain voltage and current) and the flame continues to burn at a high temperature, the damage, breakdown, and changes in power-on parameters during the duration of the flame are tested.

[0003] The general consensus in the industry is that single-sided calcined mica tape should have the best fire-resistant stability, but the test data shows that its fire-resistant data is not very ideal. Among the 20 test data, the single-sided calcined mica tape (with insulated cables as the test subject) only passed 6 times. The test conditions are: power-on voltage 1000V, flame combustion temperature 750℃, and duration 90min; and when the flame combustion temperature is increased to 950℃ and the duration is extended to 180min, the pass rate is even lower. Of course, its fire-resistant insulation performance fluctuates under the influence of factors such as the quality of mica ore, some details in the papermaking process, and the combination of mica flakes and glue content, but the impact on it is limited and it is difficult to make a breakthrough. After analysis, the reasons are as follows: 1. The insulation, moisture resistance, mechanical strength and other properties of mica tape are the result of the combined influence of mica flakes, adhesive, glass fiber cloth and other materials. Since the mica material of the single-sided calcined mica tape is calcined at high temperature and then crushed, its diameter-to-thickness ratio is greatly increased, resulting in a significant extension of the penetration time of organic silica gel into the mica paper during the sizing process of the calcined mica paper. In addition, calcination makes the mica paper denser (this is the main reason why the refractory insulation performance of the calcined mica tape is significantly improved compared to the uncalcined mica tape), the randomness of the flake distribution and other factors make it impossible to ensure that the glue completely penetrates the mica paper. 1. The unpenetrated position of the mother paper forms the weak points of the fire-resistant insulated cable under the test conditions (i.e. a certain power-on voltage, a certain flame burning temperature and a certain duration). Under the test conditions, the comprehensive performance of these weak points forms the point breakdown areas of the cable from low to high; 2. The mica tape forms new weak points due to slight deformation of the mica tape due to stretching and other reasons during the cable processing. Therefore, tensile strength is also an important reference for the mica tape used in fire-resistant insulated cables; 3. In addition, the adhesive-exposed side of the single-sided mica tape adheres to the conductor, and the powder (mica powder) falls off, which will also affect the fire-resistant insulation grade of the fire-resistant insulated cable. Summary of the invention

[0004] The purpose of the present invention is to provide a calcined three-in-one mica tape in view of the above-mentioned problems existing in the prior art. The technical problem to be solved by the present invention is how to compensate for the electrical shock weakness of the single-sided calcined mica tape and improve the fire resistance and breakdown resistance level of the fire-resistant cable.

[0005] The purpose of the present invention can be achieved through the following technical scheme: a calcined three-in-one mica tape, characterized in that glass fiber cloth, organic silica gel water, calcined mica paper, high-viscosity coating glue, and modified BOPP film are compounded in sequence from one side to the other side of the mica tape.

[0006] Furthermore, the mica tape has a thickness of 0.13-0.15 mm.

[0007] A manufacturing process of a calcined three-in-one mica tape, characterized in that it comprises the following steps: 1) selecting high-quality mica material and calcining it to obtain calcined mica material, crushing the calcined mica material by a water wet method, and preferentially grading it to obtain calcined mica slurry, and the calcined mica slurry is paper-made, pressed, dried, and rolled to obtain calcined mica paper;

[0008] 2) Start gluing: put the glass fiber cloth into the glue tank and apply glue evenly. The glue is organic silicone water. Apply glue to the composite surface of the modified BOPP film. The glue is high viscosity glue.

[0009] 3) Compounding: Compound the glass fiber cloth and modified BOPP film on both sides of the mica paper simultaneously, and obtain the semi-finished mica tape after surface treatment, drying in a drying oven and curing;

[0010] 4) After coiling, slitting and winding, the calcined refractory mica tape is obtained.

[0011] Furthermore, the thickness of the modified BOPP film is 0.018-0.020 mm, and its performance is biaxial stretching and high temperature resistance, which can reach 150°C for 5 minutes without deformation of the film surface. The film is more uniform when glued, effectively protecting the mica paper from being broken when folded horizontally or vertically, and improving the overall performance of the mica tape.

[0012] The refinement steps of calcined three-in-one mica tape are as follows:

[0013] 1): a. Select high-quality mica materials, which are muscovite or phlogopite after removing sand, impurities, crystal water, small scales or large scales; the calcination method is kiln calcination, the calcination temperature is 650-850℃; the calcination time is: 0.5-1.5 hours, b. adopt the wet crushing method formed by the combination of hydraulic crushing and ultrasonic crushing.

[0014] 2): a. The glass fiber cloth is alkali-free glass fiber cloth; the adhesive of the glass fiber cloth is oily organic silicone water, and both the glass fiber cloth and the organic silicone water are produced by the company.

[0015] 3): The production speed is controlled at 5-7 meters / minute.

[0016] 4): The laminating temperature is 85-95°C, and the laminating surface of the modified BOPP film is glued by a roller.

[0017] Furthermore, the solid content of the glue between the mica paper and the glass fiber cloth is controlled at 10-20%.

[0018] Furthermore, the solid content of the glue between the mica paper and the modified BOPP film is controlled at 25-30%.

[0019] This solution has the following advantages over existing technologies:

[0020] 1. Use glue with a relatively small solid content as the bonding medium between mica paper and glass fiber cloth. It is the primary penetration glue of mica paper and the main penetration glue of mica paper flakes. The glue between mica paper and PE film is used as compensation glue to fill and compensate for the weak points that were not penetrated during the primary penetration. It can also fill the places with less glue for a second time, so that the existence of the penetration weak points can be ignored, and the click resistance and fire resistance of the weak points can be improved. Since the performance of mica tape needs to be applied to cable products, it is most accurate and practical to test cable products. By applying glue and film on the paper surface of a single-layer mica tape, the random glue penetration weak points that cannot be detected during the production process can be effectively eliminated, thereby improving the fire resistance and breakdown resistance of the cable.

[0021] 2. The presence of modified BOPP film can improve the flatness and smoothness of the corresponding surface of the mica tape, overcoming the defects of single-sided calcined mica tape such as adhesion to the conductor and powder loss (mica powder).

[0022] 3. Since the compounding is carried out at a higher temperature, the glue penetration efficiency is improved, and the laminating speed can be increased accordingly, thereby improving production efficiency.

[0023] 4. Due to the presence of modified BOPP film and the viscosity glue, the weak points of mica tape penetration can be effectively compensated, reducing the penetration requirements of organic silicone water between glass fiber cloth and mica paper, which can further increase vehicle speed and thus improve efficiency.

[0024] 5. The modified BOPP film has tough biaxial stretching and higher smoothness, which can improve the portability of mica tape winding, cable wrapping and other operations. It also improves the mechanical properties of mica tape, especially the tensile resistance. Such advantages indirectly optimize mica tape products and fire-resistant insulated cable products. DETAILED DESCRIPTION

[0025] The following are specific embodiments of the present invention, which further describe the technical solutions of the present invention, but the present invention is not limited to these embodiments.

[0026] The calcined three-in-one mica tape is composed of calcined mica paper, glass fiber cloth and modified BOPP film. The modified BOPP film and mica paper are bonded and compounded by high-viscosity glue, which can be the glue used when laminating release paper; the glass fiber cloth and mica paper are compounded by organic silicone water, which is a low-viscosity glue and its curing depends on the penetration and volatilization of the solvent. In the process of compounding the modified BOPP film, the high-viscosity glue covers the surface of the mica paper, effectively controlling the weak points on the mica paper surface, and the breakdown problem of the mica tape is also controlled.

[0027] The calcined three-in-one mica tape improved by this technology has made a qualitative leap from the original unstable calcined single-sided mica tape in fire resistance. In the fire resistance test, it was tested 20 times at 750℃ for 90min, and all 20 times passed; it was tested 20 times at 950℃ for 180min, and 17 times passed, and 3 times failed.

[0028] As a refinement, high-quality mica materials are selected and calcined to obtain calcined mica materials, the calcined mica materials are crushed by a water-wet method, and calcined mica slurry is obtained by preferential grading. The calcined mica slurry is papered, pressed, dried, and rolled to obtain calcined mica paper.

[0029] Start the glue coating machine, put the glass fiber cloth into the glue tank and evenly apply glue. The glue is: organic silicone water; high-viscosity glue is rolled between the PE film and the mica paper; the three are compounded synchronously, and the semi-finished mica tape is obtained through surface treatment, drying in a drying oven, and curing; and then the calcined three-in-one mica tape is obtained through winding, slitting, and winding.

[0030] The selected high-quality mica material is muscovite or phlogopite after removing sand, impurities, crystal water, small scales or large scales; the calcination method is kiln calcination, the calcination temperature is 650-850℃; the calcination time is: 0.5-1.5 hours, and the wet crushing is a combination of hydraulic crushing and ultrasonic crushing.

[0031] The glass fiber cloth is alkali-free glass fiber cloth; the selected adhesive is oily organic silicone water, and its solid content is: 10%-25%. The glass fiber cloth and organic silicone water are both produced by the company.

[0032] The gluing equipment is self-produced and uses coating to apply glue, and the production speed has been increased from the original 2 meters to 5-7 meters.

[0033] The composite temperature of the modified BOPP film and paper is 90°C. The film is glued by rollers and then passed through a drying tunnel for baking, drying and rolling.

[0034] For any unclear points, please refer to the applicant's prior patent application with application number CN202010865766.1, which is about the production parameters of single-sided calcined mica tape, and the drying temperature is as described in this scheme.

[0035] Embodiment 1:

[0036] High-quality mica materials are selected and calcined to obtain calcined mica materials, the calcined mica materials are crushed by a wet method, and calcined mica slurry is obtained by priority classification. The calcined mica slurry is papered, pressed, dried, and rolled to obtain calcined mica paper.

[0037] Turn on the glue applying machine, put the fiberglass cloth into the glue slot and apply glue evenly. The glue is: organic silicone water.

[0038] Bonding and laminating: the glass fiber cloth and the modified BOPP film are respectively laminated on both sides of the mica paper, and the semi-finished mica tape is obtained through surface treatment, drying in an oven, and curing. The thickness of the modified BOPP film is 0.018-0.020 mm.

[0039] After winding, slitting and coiling, the calcined refractory mica tape is obtained.

[0040] The selected high-quality mica material is muscovite or phlogopite after removing sand, impurities, crystal water, small scales or large scales; the calcination method is kiln calcination, the calcination temperature is 700℃; the calcination time is: 60min, and the wet crushing is a combination of hydraulic crushing and ultrasonic crushing.

[0041] The glass fiber cloth is alkali-free glass fiber cloth; the selected adhesive is oily organic silicone water, and its solid content is: 10%-25%. The glass fiber cloth and organic silicone water are both produced by the company.

[0042] The gluing equipment is self-produced and uses coating to apply glue, and the production speed has been increased from the original 2 meters to 5 meters.

[0043] The temperature of the film and paper composite is 90℃. The film is glued by rollers and then passed through a drying tunnel for baking, drying and rolling.

[0044] The parameters of the calcined three-in-one mica tape are shown in the following table.

[0045]

[0046] Fire resistance test: 750℃90min test 10 times, passed 7 times, failed 3 times

[0047] Embodiment 2:

[0048] High-quality mica materials are selected and calcined to obtain calcined mica materials, the calcined mica materials are crushed by a wet method, and calcined mica slurry is obtained by priority classification. The calcined mica slurry is papered, pressed, dried, and rolled to obtain calcined mica paper.

[0049] Turn on the glue applying machine, put the fiberglass cloth into the glue slot and apply glue evenly. The glue is: organic silicone water.

[0050] Bonding and laminating: the glass fiber cloth and the modified BOPP film are respectively laminated on both sides of the mica paper, and the semi-finished mica tape is obtained through surface treatment, drying in an oven, and curing. The thickness of the modified BOPP film is 0.018-0.020 mm.

[0051] After winding, slitting and coiling, the calcined refractory mica tape is obtained.

[0052] The selected high-quality mica material is muscovite or phlogopite after removing sand, impurities, crystal water, small scales or large scales; the calcination method is kiln calcination, the calcination temperature is 750℃; the calcination time is: 70min, and the wet crushing is a combination of hydraulic crushing and ultrasonic crushing.

[0053] The glass fiber cloth is alkali-free glass fiber cloth; the selected adhesive is oily organic silicone water, and its solid content is: 10%-25%. The glass fiber cloth and organic silicone water are both produced by the company.

[0054] The gluing equipment is self-produced and uses coating to apply glue, and the production speed has been increased from the original 2 meters to 5.5 meters.

[0055] The composite temperature of the modified BOPP film and paper is 90°C. The film is glued by rollers and then passed through a drying tunnel for baking, drying and rolling.

[0056] The parameters of the calcined three-in-one mica tape are shown in the following table.

[0057]

[0058] Fire resistance test: 750℃90min test 10 times passed 9 times, 1 time failed

[0059] Embodiment 3:

[0060] High-quality mica materials are selected and calcined to obtain calcined mica materials, the calcined mica materials are crushed by a wet method, and calcined mica slurry is obtained by priority classification. The calcined mica slurry is papered, pressed, dried, and rolled to obtain calcined mica paper.

[0061] Turn on the glue applying machine, put the fiberglass cloth into the glue slot and apply glue evenly. The glue is: organic silicone water.

[0062] Bonding and laminating: the glass fiber cloth and the modified BOPP film are respectively laminated on both sides of the mica paper, and the semi-finished mica tape is obtained through surface treatment, drying in an oven, and curing. The thickness of the modified BOPP film is 0.018-0.020 mm.

[0063] After winding, slitting and coiling, the calcined refractory mica tape is obtained.

[0064] The selected high-quality mica material is muscovite or phlogopite after removing sand, impurities, crystal water, small scales or large scales; the calcination method is kiln calcination, the calcination temperature is 830℃; the calcination time is: 60min, and the wet crushing is a combination of hydraulic crushing and ultrasonic crushing.

[0065] The glass fiber cloth is alkali-free glass fiber cloth; the selected adhesive is oily organic silicone water, and its solid content is: 10%-25%. The glass fiber cloth and organic silicone water are both produced by the company.

[0066] The gluing equipment is self-produced and uses coating to apply glue, and the production speed has been increased from the original 2 meters to 5.5 meters.

[0067] The composite temperature of the modified BOPP film and paper is 90°C. The film is glued by rollers and then passed through a drying tunnel for baking, drying and rolling.

[0068] The parameters of the calcined three-in-one mica tape are shown in the following table.

[0069]

[0070] Fire resistance test: 950℃180min test 10 times passed 8 times, 2 times failed

[0071] Embodiment 4:

[0072] High-quality mica materials are selected and calcined to obtain calcined mica materials, the calcined mica materials are crushed by a wet method, and calcined mica slurry is obtained by priority classification. The calcined mica slurry is papered, pressed, dried, and rolled to obtain calcined mica paper.

[0073] Turn on the glue applying machine, put the fiberglass cloth into the glue slot and apply glue evenly. The glue is: organic silicone water.

[0074] Bonding and laminating: the glass fiber cloth and the modified BOPP film are respectively laminated on both sides of the mica paper, and the semi-finished mica tape is obtained through surface treatment, drying in an oven, and curing. The thickness of the modified BOPP film is 0.018-0.020 mm.

[0075] After winding, slitting and coiling, the calcined refractory mica tape is obtained.

[0076] The selected high-quality mica material is muscovite or phlogopite after removing sand, impurities, crystal water, small scales or large scales; the calcination method is kiln calcination, the calcination temperature is 850℃; the calcination time is: 50min, and the wet crushing is a combination of hydraulic crushing and ultrasonic crushing.

[0077] The glass fiber cloth is alkali-free glass fiber cloth; the selected adhesive is oily organic silicone water, and its solid content is: 10%-25%. The glass fiber cloth and organic silicone water are both produced by the company.

[0078] The gluing equipment is self-produced and uses coating to apply glue, and the production speed has been increased from the original 2 meters to 5.8 meters.

[0079] The temperature of the film and paper composite is 90℃. The film is glued by rollers and then passed through a drying tunnel for baking, drying and rolling.

[0080] The parameters of the calcined three-in-one mica tape are shown in the following table.

[0081]

[0082] Fire resistance test: 950℃180min test 10 times, passed 9 times, failed once.

[0083] The specific embodiments described herein are merely examples of the spirit of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in similar ways, but they will not deviate from the spirit of the present invention or exceed the scope defined by the appended claims.

Claims

1. A calcined three-in-one mica tape, characterized in that: From one side of the mica tape to the other side, the multi-layer structure of the mica tape includes glass fiber cloth, organic silica gel water, calcined mica paper, high-viscosity coating glue, and modified BOPP film compounded in sequence; The processing technology of calcining three-in-one mica tape is as follows: 1) Select high-quality mica materials and calcine them to obtain calcined mica materials. The calcined mica materials are crushed by wet method and prioritized to obtain calcined mica slurry. The calcined mica slurry is made, pressed, dried and rolled to obtain calcined mica paper. 2) Start gluing: put the glass fiber cloth into the glue tank and apply glue evenly. The glue is organic silicone water; apply glue to the composite surface of the modified BOPP film. The glue is high viscosity glue; 3) Compounding: Compound the glass fiber cloth and modified BOPP film on both sides of the mica paper simultaneously, and obtain the semi-finished mica tape after surface treatment, drying in a drying oven and curing; 4) After coiling, slitting and winding, the calcined refractory mica tape is obtained; The solid content of the glue between the mica paper and the glass fiber cloth is controlled at 10-20%; The solid content of the glue between the mica paper and the modified BOPP film is controlled at 25-30%; Organic silicone water is a low viscosity glue.

2. The calcined three-in-one mica tape according to claim 1, characterized in that: The mica tape has a thickness of 0.13-0.15 mm.

3. The calcined three-in-one mica tape according to claim 1, characterized in that: The thickness of the modified BOPP film is 0.018-0.020 mm.

4. The manufacturing process of calcined three-in-one mica tape according to claim 1, characterized in that: In the step 1), the selected high-quality mica material is muscovite or phlogopite after removing sand, impurities, crystal water, small scales or large scales; the calcination method is kiln calcination, the calcination temperature is 650-850°C; the calcination time is: 0.5-1.5 hours, and the wet crushing method formed by combining hydraulic crushing and ultrasonic crushing is adopted.

5. The manufacturing process of calcined three-in-one mica tape according to claim 1, characterized in that: The glass fiber cloth is alkali-free glass fiber cloth; the glue between the glass fiber cloth and the mica paper is oily organic silicone water.

6. The manufacturing process of calcined three-in-one mica tape according to claim 1, characterized in that: The production speed in step 3) is controlled at 5-7 m / min.

7. The manufacturing process of calcined three-in-one mica tape according to claim 1, characterized in that: The lamination temperature in step 3) is 85-95° C., and the lamination surface of the modified BOPP film is glued by a roller.