A polypropylene nonwoven fabric finished with a silver ion-loaded sepiolite fiber carbon nanotube composite antibacterial material
Through the finishing process of sepiolite fiber carbon nanotube composite material and polypropylene nonwoven fabrics loaded with silver ions, the problem of insufficient antibacterial performance of medical polypropylene nonwoven fabrics is solved, and efficient inhibition of Staphylococcus aureus and E. coli is achieved. and improve water absorption, suitable for the antibacterial needs of medical gauze.
Patent Information
- Application Number
- CN202211438129.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-16
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-11-16
AI Technical Summary
The existing medical polypropylene nonwovens have insufficient heat resistance and durability in terms of antibacterial properties, which are easy to decompose, and have a narrow antibacterial range, making it difficult to effectively inhibit the spread of viral mutants such as new coronary pneumonia.
Using the finishing process of silver ions-loaded sepiolite fiber carbon nanotube composite material and polypropylene nonwoven fabric, high-efficiency and antibacterial sepiolite fibers are prepared by plasma activated carbon nanotubes and acid activated sepiolite fibers, combined with AgNO3 reactions, high-efficiency antibacterial sepiolite Fiber carbon nanotube composite material and improves its antibacterial properties in medical gauze through a dual-pad process.
It has achieved efficient inhibition of Staphylococcus aureus and E. coli, improved the water absorption and antibacterial properties of the material, and has a simple process and low cost, which is suitable for industrial production and application.
Smart Images

Figure BDA0003945841970000061 
Figure BDA0003945841970000062 
Figure BDA0003945841970000063
Abstract
Description
Technical Field
[0001] The invention relates to the field of medical materials, and in particular to a polypropylene non-woven fabric finished with a silver ion-loaded sepiolite fiber and carbon nanotube composite antibacterial material. Background Art
[0002] Sepiolite has a certain bactericidal effect and is an antibacterial mineral material. It is a hydrated magnesium-rich porous layered chain silicate with a basic chemical formula of Mg8(H2O)4[Si6O 16 ]2(OH)4·8H2O.
[0003] Sepiolite fiber is a natural mineral fiber, a fibrous variant of the sepiolite mineral, called α-sepiolite. In the structure, a layer of magnesium-oxygen octahedron is sandwiched between two layers of silicon-oxygen tetrahedron, forming a 2:1 layered structural unit. The tetrahedral layer is continuous, and the direction of active oxygen in the layer is reversed periodically. The octahedral layer forms a channel with alternating upper and lower layers. The orientation of the channel is consistent with the fiber axis, allowing water molecules, metal cations, small organic molecules, etc. to enter it.
[0004] Plasma surface activation of carbon nanotubes is a process in which the polymer functional groups on the surface of carbon nanotubes are replaced by atoms of different ions in the plasma to increase the surface energy, thereby increasing the adsorption of silver ions by carbon nanotubes.
[0005] At present, antimicrobial agents can be divided into two categories: organic and inorganic. Organic antimicrobial agents are mainly synthetic organic substances, which have strong initial bactericidal power and obvious antibacterial and sterilization effects, but have average heat resistance and durability, are easy to decompose, migrate quickly, have a narrow antimicrobial range, and are prone to drug resistance after long-term use; inorganic antimicrobial agents are mainly antimicrobial materials made of metallic silver, zinc, copper ions and porous inorganic non-metallic materials as carriers, which have the advantages of strong bactericidal efficiency, good durability, and no impact on the environment and human body.
[0006] Polypropylene (PP) is a colorless, translucent thermoplastic synthetic resin with the advantages of chemical resistance, heat resistance, electrical insulation and good mechanical properties. It is widely used in textile fibers, medical devices, food packaging, agriculture, forestry and fishery, construction, automobiles and other fields. Non-woven fabrics made of polypropylene have the advantages of high strength, strong protection, breathable and comfortable, non-toxic and odorless, and are maturely used in the medical and health fields such as medical masks, surgical gowns, sterilizing bandages, and protective clothing. Since the global outbreak of COVID-19 in 2020 and the subsequent emergence of Delta and Omicron mutant strains, the market has put forward higher requirements on the antibacterial properties of medical polypropylene non-woven fabrics under the normalization of the epidemic. Summary of the invention
[0007] The present invention provides a polypropylene non-woven fabric finished with a silver ion-loaded sepiolite fiber and carbon nanotube composite antibacterial material, and preparation and application thereof. The finished polypropylene non-woven fabric has the advantages of high antibacterial rate, strong water absorption, simple process, low cost and the like.
[0008] Specifically, the present invention provides a method for preparing a polypropylene non-woven fabric finished with a silver ion-loaded sepiolite fiber and carbon nanotube composite antibacterial material, comprising the following steps:
[0009] 1) Plasma activation of carbon nanotubes: Placing carbon nanotubes in a chamber and bombarding the carbon nanotubes with plasma to obtain surface-activated carbon nanotubes;
[0010] 2) acid activation and thermal modification of sepiolite fibers;
[0011] 3) wet-mixing the activated carbon nanotubes with acid-activated sepiolite fibers to prepare a sepiolite fiber-carbon nanotube composite material;
[0012] 4) reacting the sepiolite fiber-carbon nanotube composite material with a AgNO3 solution to prepare a sepiolite fiber-carbon nanotube composite antibacterial material loaded with silver ions;
[0013] 5) Wetting the polypropylene non-woven fabric with clean water, dipping it in a finishing solution containing the sepiolite fiber carbon nanotube composite antibacterial material loaded with silver ions, taking it out and performing a first dipping using a padding machine, then dipping it in the finishing solution containing the sepiolite fiber carbon nanotube composite antibacterial material loaded with silver ions, taking it out and performing a second dipping using a padding machine, and drying it to obtain a polypropylene non-woven fabric finished with the sepiolite fiber carbon nanotube composite antibacterial material loaded with silver ions. The acid activation in step 1) is preferably to activate the sepiolite fiber using hydrochloric acid;
[0014] The diameter of the sepiolite fiber is 20-300 nm;
[0015] During the acid activation, one or more operations of stirring, aging at room temperature, washing, filtering, drying, etc. are optionally performed;
[0016] The aging time is preferably 24h;
[0017] The thermal modification in step 1) is preferably thermal modification at a high temperature, and the high temperature is preferably 300-800° C., more preferably 600° C.;
[0018] The thermal modification time is preferably 10-180 min, more preferably 60 min;
[0019] The reaction temperature of the AgNO3 solution is 30-90°C, preferably 60°C, and the reaction time is 30-60min, preferably 60min;
[0020] The concentration of AgNO3 is preferably 5 mol·L -1 ;
[0021] After the reaction, one or more operations of washing, dehydration, drying, etc. are optionally performed;
[0022] In the step 2), the concentration of the finishing solution containing the sepiolite fiber carbon nanotube composite antibacterial material loaded with silver ions used in the two immersions is 1-10 g·L -1 , preferably 5 g·L -1 ;
[0023] The immersion temperature is preferably 25-75°C, more preferably 50°C;
[0024] The rolling ratio in the first and second rolling is preferably 70%;
[0025] The dipping time is preferably 15 min;
[0026] The present invention also provides a polypropylene non-woven fabric finished with a silver ion-loaded sepiolite fiber and carbon nanotube composite antibacterial material, which is prepared by the above-mentioned preparation method of the present invention;
[0027] The present invention also provides an application of a polypropylene non-woven fabric finished with a silver ion-loaded sepiolite fiber carbon nanotube composite antibacterial material, wherein the polypropylene non-woven fabric finished with a silver ion-loaded sepiolite fiber carbon nanotube composite antibacterial material is used to prepare antibacterial articles;
[0028] The antibacterial articles are preferably medical masks, surgical gowns, sterilizing bandages or protective clothing, etc.;
[0029] The bacteria are preferably Staphylococcus aureus or Escherichia coli.
[0030] The present invention prepares a sepiolite fiber-carbon nanotube composite antibacterial material loaded with silver ions by mixing carbon nanotubes with sepiolite fibers and loading silver ions, and by controlling key processes such as reaction temperature and time, and by controlling the impregnation process in a finishing liquid, obtains a polypropylene non-woven fabric with the advantages of high antibacterial rate and strong water absorption, and in particular has a good inhibitory effect on Staphylococcus aureus and Escherichia coli. The present invention has a simple process, low cost, and is easy to industrialize and apply. DETAILED DESCRIPTION
[0031] The present invention uses the following main reagents / materials:
[0032] AgNO3 (Hunan Huihong Reagent Co., Ltd.);
[0033] Staphylococcus aureus (ATCC6538), Escherichia coli (ATCC11229) (Shanghai Fuxiang Biotechnology Co., Ltd.);
[0034] Agar powder, peptone, beef extract (Sinopharm Chemical Reagent Co., Ltd.);
[0035] Penetrant DM-1232 (Guangdong Demei Fine Chemical Group Co., Ltd.);
[0036] Polypropylene meltblown nonwoven fabric (Dongguan Baoxinghui Industrial Co., Ltd., weight: 65g / ㎡);
[0037] Sepiolite fiber (Xiangtan Sepiolite Technology Co., Ltd., diameter 80 nm);
[0038] Carbon nanotubes.
[0039] The present invention uses the following main instruments:
[0040] Plasma treatment equipment;
[0041] DH3600 constant temperature incubator (Guangzhou Dexinduo Scientific Instrument Co., Ltd.);
[0042] XPB10-01 pulsator washing machine (Ningbo Kemei Electric Appliance Co., Ltd.);
[0043] LP-400 vertical padder (Foshan Nanhai Hongxin Machinery Equipment Co., Ltd.);
[0044] SX2-8-16NP muffle furnace (Zhejiang Saide Instrument Co., Ltd.);
[0045] JGW-360 contact angle meter (Dataphysics, Germany);
[0046] SHB-III circulating water multi-purpose vacuum pump (Zhengzhou Great Wall Science and Technology Trading Co., Ltd.).
[0047] Example 1
[0048] 1g of carbon nanotubes were placed in a stainless steel tray, connected to the cathode of a glow ion bombardment furnace, and low-pressure Ar, Ar / O2, Ar / H2, Ar / H2 / O2, and NH3 glow discharge plasma were used to bombard CNTs for 5min to obtain surface-activated carbon nanotubes.
[0049] Take 100 mL of water and place it in a 250 mL beaker, add 1 g of sepiolite fiber, add the above surface-activated carbon nanotubes, and then stir evenly at 50-150 speed for 60 min, then age at room temperature for 24 h, then wash with water, filter, dry at 75 ° C, cool to room temperature, put into a beaker, and add 5 mol·L -1The AgNO3 solution was reacted at 30°C for 60 minutes; finally, it was washed with water, dehydrated, and dried at 75°C to obtain a sepiolite fiber carbon nanotube composite antibacterial material loaded with silver ions.
[0050] Take a 5 cm × 25 cm polypropylene nonwoven fabric and put it into clean water to wet it. Then, immerse it in 5 g·L -1 The sepiolite fiber carbon nanotube composite antibacterial material and silver ion finishing liquid were placed in the solution for 15 minutes, and the polypropylene non-woven fabric was taken out and flatly pasted on the surface of the padding roller of the padding machine. The padding machine was started for the first padding (rolling rate 70%). After the first padding was completed, the fabric was taken out and then immersed in 5g·L -1 The non-woven fabric was soaked in the sepiolite antibacterial finishing liquid for 15 minutes, and the polypropylene non-woven fabric was taken out and flatly attached to the surface of the roller of the impregnation mill. The impregnation mill was started for the second impregnation (the residual rate was 70%). After the second impregnation was completed, the polypropylene non-woven fabric was taken out and put into an oven and dried at 50°C to obtain a polypropylene non-woven fabric finished with sepiolite antibacterial material loaded with silver ions.
[0051] Example 2
[0052] Take 100mL of water and place it in a 250mL beaker, add 1g of sepiolite fiber, and then stir evenly at 50-150 speed for 60min, then age it at room temperature for 24h, then wash it with water, filter it, dry it at 75℃, cool it to room temperature, put it in a beaker, and add 5mol·L -1 The AgNO3 solution was reacted at 30°C for 60 minutes; finally, the material was washed with water, dehydrated and dried at 75°C to obtain a sepiolite fiber composite antibacterial material loaded with silver ions.
[0053] Take a 5 cm × 25 cm polypropylene nonwoven fabric and put it into clean water to wet it. Then, immerse it in 5 g·L -1 The nonwoven fabric was placed in the sepiolite antibacterial finishing liquid for 15 min, and the nonwoven fabric was flatly attached to the surface of the padding roller. The padding roller was started for the first padding (rolling rate 70%). After the first padding was completed, the fabric was taken out and then immersed in 5 g·L -1 The non-woven fabric was soaked in the sepiolite fiber composite antibacterial finishing liquid for 15 minutes, and the polypropylene non-woven fabric was taken out and flatly attached to the surface of the impregnation mill roller. The impregnation mill was started for the second impregnation (rolling rate 70%). After the second impregnation was completed, the polypropylene non-woven fabric was taken out and put into an oven and dried at 50°C to obtain a polypropylene non-woven fabric finished with a sepiolite fiber composite antibacterial material loaded with silver ions.
[0054] Example 3
[0055] Take 100mL of hydrochloric acid (6mol·L -1) was placed in a 250mL beaker, 1g of 800-mesh sepiolite powder was added, and then stirred evenly at a speed of 50-150 for 60 minutes, and then aged at room temperature for 24 hours, and then washed with water, filtered, and dried at 75°C; the filter cake was placed in a crucible, placed in a muffle furnace, and thermally modified at a high temperature of 600°C for 60 minutes. After the thermal modification was completed, it was cooled to room temperature and placed in a beaker; 5mol·L -1 The AgNO3 solution was reacted at 30°C for 60 minutes; finally, it was washed with water, dehydrated, and dried at 75°C to obtain the sepiolite antibacterial material loaded with silver ions.
[0056] Take a 5 cm × 25 cm polypropylene nonwoven fabric and put it into clean water to wet it. Then, immerse it in 5 g·L -1 The nonwoven fabric was placed in the sepiolite antibacterial finishing liquid for 15 min, and the nonwoven fabric was flatly attached to the surface of the padding roller. The padding roller was started for the first padding (rolling rate 70%). After the first padding was completed, the fabric was taken out and then immersed in 5 g·L -1 The non-woven fabric was soaked in the sepiolite antibacterial finishing liquid for 15 minutes, and the polypropylene non-woven fabric was taken out and flatly attached to the surface of the roller of the impregnation mill. The impregnation mill was started for the second impregnation (the residual rate was 70%). After the second impregnation was completed, the polypropylene non-woven fabric was taken out and put into an oven and dried at 50°C to obtain a polypropylene non-woven fabric finished with sepiolite antibacterial material loaded with silver ions.
[0057] Example 4
[0058] Take a 5 cm × 25 cm polypropylene nonwoven fabric and put it into clean water to wet it. Then, immerse it in 5 mol·L -1 The nonwoven fabric was placed flat on the surface of the padding mill roll and the padding mill was started for the first padding (rolling rate 70%). After the first padding was completed, the fabric was taken out and immersed in 5g·L AgNO3 solution at 25°C. -1 The non-woven fabric was placed in the sepiolite antibacterial finishing liquid for 15 minutes, and the non-woven fabric was taken out and flatly attached to the surface of the roller of the impregnation mill. The impregnation mill was started for the second impregnation (the residual rate was 70%). After the second impregnation was completed, the non-woven fabric was taken out and placed in an oven and dried at 50°C to obtain a polypropylene non-woven fabric finished with an antibacterial material containing silver ions.
[0059] 1. Antibacterial performance test: The polypropylene non-woven fabrics of Examples 1-4 of the present invention were tested with reference to GB / T20944.3-2008 "Evaluation of antibacterial properties of textiles (Part 3): Oscillation method", and the test results were calculated according to the following formula:
[0060]
[0061] Wherein: A represents the colony count of the blank control sample after culturing for 24 hours; B represents the colony count of the antibacterial finishing sample after culturing for 24 hours. The test results are shown in Table 1.
[0062] Table 1 Antibacterial rate against Staphylococcus aureus and Escherichia coli
[0063]
[0064] 2. Hygroscopicity test: The polypropylene non-woven fabrics of Examples 1 to 4 of the present invention and the unfinished polypropylene non-woven fabric (blank) were respectively tested for the water contact angle on the surface of the material using a fully automatic optical contact angle measuring instrument. The test results are shown in Table 2.
[0065] Table 2 Hygroscopicity test results
[0066]
[0067] The above results show that the polypropylene non-woven fabric finished with the silver ion-loaded sepiolite fiber carbon nanotube composite antibacterial material has excellent antibacterial properties, among which the finished polypropylene non-woven fabric obtained in Example 1 has the best inhibition rate against Staphylococcus aureus and Escherichia coli; after finishing, the water contact angle value of the surface of the polypropylene non-woven fabric decreases, indicating that its hygroscopicity is significantly improved.
[0068] The embodiments described above are only preferred implementations of the present invention. It should be pointed out that a person skilled in the art can make several improvements without departing from the principles of the present invention, and these improvements should also be regarded as within the scope of protection of the present invention.
Claims
1. A method for preparing a polypropylene non-woven fabric finished with a silver ion-loaded sepiolite fiber composite antibacterial material, characterized in that: The preparation method comprises the following steps: 1) Plasma activation of carbon nanotubes: Placing carbon nanotubes in a chamber and bombarding the carbon nanotubes with plasma to obtain surface-activated carbon nanotubes; 2) Acid activation and thermal modification of sepiolite fibers; 3) wet-mixing the activated carbon nanotubes with the acid-activated sepiolite fibers to prepare a sepiolite fiber-carbon nanotube composite material; 4) reacting the sepiolite fiber-carbon nanotube composite material with a AgNO3 solution to prepare a sepiolite fiber-carbon nanotube composite antibacterial material loaded with silver ions; 5) Wetting the polypropylene non-woven fabric with clean water, immersing it in a finishing solution containing the silver ion-loaded sepiolite fiber carbon nanotube composite antibacterial material, taking it out and performing a first immersion using a padding machine, then immersing it in the finishing solution containing the silver ion-loaded sepiolite fiber carbon nanotube composite antibacterial material, taking it out and performing a second immersion using a padding machine, and drying to obtain a polypropylene non-woven fabric finished with the silver ion-loaded sepiolite fiber carbon nanotube composite antibacterial material.
2. The preparation method according to claim 1, characterized in that: The acid activation in step 1) is to activate the sepiolite fiber with hydrochloric acid; and / or, The diameter of the sepiolite fiber is 20-300 nm; and / or, During the acid activation, one or more of stirring, room temperature aging, water washing, suction filtration, and drying are optionally performed.
3. The preparation method according to claim 1, characterized in that: The thermal modification in step 1) is thermal modification at a high temperature, wherein the high temperature is 300-800°C; The thermal modification time is 10-180 minutes.
4. The preparation method according to claim 3, characterized in that: The thermal modification in step 1) is thermal modification at a high temperature, the high temperature is 600° C. and the thermal modification time is 60 minutes.
5. The preparation method according to claim 1, characterized in that: The reaction temperature of the sepiolite fiber carbon nanotube composite material and the AgNO3 solution in step 4) is 30-90°C, and the reaction time is 30-60min; The concentration of the AgNO3 solution is 5 mol·L -1 .
6. The preparation method according to claim 5, characterized in that: The reaction temperature is 60° C., and the reaction time is 60 min.
7. The preparation method according to claim 1, characterized in that: The concentration of the finishing liquid containing the silver ion-loaded sepiolite fiber carbon nanotube composite antibacterial material used in the two immersions is 1-10 g·L -1 .
8. The preparation method according to claim 7, characterized in that: The concentration of the finishing solution containing the sepiolite fiber carbon nanotube composite antibacterial material loaded with silver ions used in the two immersions was 5 g·L -1 .
9. The preparation method according to claim 7, characterized in that: The immersion temperature is 25-75°C.
10. The preparation method according to claim 9, characterized in that: The immersion temperature was 50°C.
11. The preparation method according to any one of claims 7 to 10, characterized in that: The rolling rate in the first and second rolling is 70%; The immersion time is 15 minutes.
12. A polypropylene nonwoven fabric finished with a silver ion-loaded sepiolite fiber and carbon nanotube composite antibacterial material, characterized in that: The polypropylene non-woven fabric finished with the silver ion-loaded sepiolite fiber and carbon nanotube composite antibacterial material is prepared by the preparation method described in any one of claims 1 to 11.
13. An application of polypropylene non-woven fabric finished with the silver ion-loaded sepiolite fiber and carbon nanotube composite antibacterial material according to claim 12, characterized in that: The polypropylene non-woven fabric finished with the silver ion-loaded sepiolite fiber carbon nanotube composite antibacterial material is used for preparing antibacterial articles.
14. The use according to claim 13, characterized in that The antibacterial article is a medical mask, surgical gown, sterilization bandage or protective clothing.