A method for ammoximation
By using halogen-containing titanium silicon molecular sieve to react with carbonyl compounds, hydrogen peroxide and ammonia, the problem of short life of titanium silicon molecular sieve in alkaline amoximetization reaction is solved, and efficient catalytic performance and a long life catalyst are achieved.
Patent Information
- Application Number
- CN202111004204.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-08-30
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-08-30
AI Technical Summary
Titanium silicon molecular sieve has a short life in alkaline amoxixilation reaction, resulting in a decrease in activity and selectivity.
Halogen-containing titanium silicon molecular sieve is used as a catalyst to optimize the reaction conditions to improve catalytic performance by contacting carbonyl compounds, hydrogen peroxide, ammonia and solvents.
Gentle reaction conditions, high conversion of carbonyl compounds, high oxime selectivity, and significantly prolong the catalyst life.
Smart Images

Figure BDA0003236625380000121 
Figure BDA0003236625380000131
Abstract
Description
Technical Field
[0001] The present invention relates to a method for preparing oxime, and further relates to a method for preparing oxime by ammoximation using molecular sieve as catalyst. Background Art
[0002] Oxime refers to a compound containing the structure R1R2C=N-OH, where R1 is an organic group and R2 is an H atom (aldehyde oxime) or an organic group (ketone oxime). Oxime compounds contain both nitrogen and oxygen elements in their molecules, and nitrogen and oxygen elements can be introduced simultaneously in organic synthesis. Oxime has two nucleophilic centers (nitrogen and oxygen atoms), one electrophilic center (sp 2 Hybridized carbon atom), and an easy leaving group (hydroxyl group). Therefore, oxime can react with suitable electrophiles or nucleophiles, can act as a 1,3-dipole to undergo a 1,3-dipolar cycloaddition reaction with suitable alkenes or alkynes, can undergo oxime hydroxyl departure, undergo intramolecular dehydration to form a ring, and can undergo a Beckmann rearrangement reaction to obtain amide compounds. Starting from oxime, complex organic compounds such as amides, nitriles, amines, ketones (aldehydes), oxime ethers, oxime esters and isoxazoles (lines) can be synthesized through the above-mentioned different reactions. Therefore, oxime compounds are often used as important intermediates in organic synthesis.
[0003] Cyclohexanone oxime is the most widely used oxime chemical, mainly used to produce ε-caprolactam. ε-caprolactam is one of the monomers for producing nylon-6 fiber and engineering plastics. At present, the main preparation method of cyclohexanone oxime is to use titanium silicalite TS-1 to catalyze cyclohexanone, ammonia and hydrogen peroxide to produce cyclohexanone oxime in a one-step ammoximation reaction. USP 4410501 discloses titanium silicalite, which can use a safe low-concentration H2O2 aqueous solution as an oxygen source to form a "clean" chemical reaction process with oxygen and water as byproducts. Titanium silicalite has high thermal stability. European patent EP0208311 first disclosed a method for the oximation reaction of titanium silicalite with cyclohexanone, hydrogen peroxide and ammonia. CN1260241A discloses a new type of titanium silicalite HTS with a unique hollow structure, which has excellent activity and selectivity in the ammoximation reaction.
[0004] However, in the ammoximation reaction, one of the problems that needs to be solved urgently is the life of the molecular sieve. Since the ammoximation reaction is an alkaline system, the titanium silicon molecular sieve will gradually undergo skeleton desiliconization during use, resulting in the loss of skeleton titanium, and ultimately reduced activity and selectivity. Summary of the invention
[0005] The purpose of the present invention is to provide an ammoximation method using an improved titanium silicon molecular sieve as a catalyst in order to solve the problem that the titanium silicon molecular sieve has a short life in an alkaline reaction system.
[0006] To achieve the above object, the present invention provides an ammoximation method, characterized in that a carbonyl compound, hydrogen peroxide, ammonia, a solvent, and a halogen-containing titanium silicon molecular sieve are contacted to obtain a liquid product containing oxime.
[0007] In the method, the halogen-containing titanium silicon molecular sieve contains 0.5%-5% and 0.5%-4% of halogen and carbon respectively, accounting for the total weight of the molecular sieve. The halogen is one of fluorine, chlorine, bromine and iodine.
[0008] In the method, in the halogen-containing titanium silicon molecular sieve, R XRF / R XPS The value is greater than 2, preferably 2.5-4, R XRF is the atomic ratio of halogen to silicon in the molecular sieve bulk phase analyzed by XRF, R XPS is the atomic ratio of halogen to silicon on the molecular sieve surface analyzed by XPS. Characterized by infrared spectroscopy, the ratio of its characteristic peak intensity I 3740 / I 3530 is 4-10, among which I 3740 The infrared hydroxyl group of molecular sieve is 3740 cm -1 The absorption peak intensity at I 3530 3530cm in the infrared spectrum of molecular sieve -1 The absorption peak intensity at .
[0009] In the method, the halogen-containing titanium silicon molecular sieve has a titanium silicon molar ratio of (0.001-0.05):1. The skeleton structure is preferably an MFI structure. The micropore specific surface area is preferably 350-420 m 2 / g, and the micropore volume is preferably 0.130-0.170 mL / g.
[0010] In the method, the carbonyl-containing compound is preferably an aldehyde, ketone, acid, ester, or carboxylate having a carbon number of C2-C20 and containing at least one carbonyl group.
[0011] In the method, the ammonia is preferably aqueous ammonia or liquid ammonia.
[0012] In the method, the solution comprises water, C6-C12 alkanes, and C2-C10 alcohols.
[0013] In the method, the molar ratio of hydrogen peroxide to the carbonyl compound is preferably (0.3-3):1, the molar ratio of ammonia to the carbonyl compound is preferably (0.3-5):1, and the molar ratio of the solvent to the carbonyl compound is preferably (2-50):1.
[0014] In the method, the weight hourly space velocity of the carbonyl-containing compound based on the halogen-containing titanium silicon molecular sieve is preferably 0.1-3h -1.
[0015] In the method, the contacting is preferably carried out at 40-100°C.
[0016] The ammoximation method provided by the invention has the characteristics of mild reaction conditions, high carbonyl compound conversion rate, high oxime selectivity and long catalyst life. DETAILED DESCRIPTION
[0017] The invention provides an ammoximation method, characterized in that a carbonyl compound, hydrogen peroxide, ammonia, a solvent and a halogen-containing titanium silicon molecular sieve are contacted to obtain a liquid product containing oxime.
[0018] In the present invention, the halogen-containing titanium silicon molecular sieve has the following characteristics:
[0019] (1) XRF characterization shows that the molecular sieve contains silicon, titanium, oxygen, carbon and halogen elements, wherein the halogen atoms account for 0.5%-5%, preferably 1%-3% of the total weight of the molecular sieve, and the carbon atoms account for 0.5%-4%, 0.8%-2.5% of the total weight of the molecular sieve. The halogen is one of fluorine, chlorine, bromine and iodine, preferably chlorine;
[0020] (2) XRF analysis of the bulk halogen / silicon atomic ratio is R XRF The surface halogen / silicon atomic ratio is R XPS , R XRF / R XPS The value is greater than 2, indicating that the halogen atoms are mainly distributed on the inner surface of the molecular sieve, i.e., in the pores, and is preferably 2.5-4; characterized by infrared spectroscopy, the ratio of its characteristic peak intensity I 3740 / I 3530 4 to 10, preferably 5 to 8, I 3740 The infrared hydroxyl spectrum of the molecular sieve is 3740 cm -1 The absorption peak intensity near represents the content of terminal hydroxyl groups of the molecular sieve. 3530 The infrared hydroxyl spectrum of the molecular sieve is 3530 cm -1 The absorption peak intensity near represents the content of nested hydroxyl groups. The higher the ratio, the less defect sites in the molecular sieve (Catalysis Today, 1997, 37(4): 353-366). The halogen-containing titanium silicon molecular sieve in the present invention has a higher I value because the halogen atoms are mainly distributed in the molecular sieve pores and combine with the defect sites of the molecular sieve through groups, thereby reducing the defect sites. 3740 / I 3530 ratio.
[0021] (3) Halogen-containing titanium-silicon molecular sieves do not limit the titanium-silicon molar ratio. Among them, the molecular sieve titanium-silicon molar ratio is (0.001-0.05):1, and more preferably (0.01-0.03):1. There is no limitation on the skeleton structure of the molecular sieve, which can be MFI, BEA, MEL, MWW, SVR, MOR, EWT and other topological structures. The skeleton structure of the molecular sieve is preferably MFI structure. The specific surface area and pore volume of the molecular sieve were measured by low-temperature nitrogen adsorption and desorption method, and the micropore specific surface area was 350-420m 2 / g, preferably 360-400m 2 / g, and the micropore volume is 0.130-0.170mL / g, preferably 0.140-0.160mL / g. The BET specific surface area and micropore volume of the halogen-containing titanium silicate molecular sieve of the present invention are lower than those of conventional titanium silicate molecular sieves, indicating that the halogen-containing groups enter the pores of the molecular sieve, resulting in a decrease in both values.
[0022] The halogen-containing titanium silicon molecular sieve described in the present invention can be obtained by the following preparation method: the titanium silicon molecular sieve from which the template is removed by calcination is contacted with an organic amine solution having a carbon number of C1-C3 at 40-100°C, and the separated solid product is washed and dried; then the solid product is contacted with a solution containing a small molecule silanization agent at 50-120°C, and then separated and dried.
[0023] In the preparation method of the halogen-containing titanium silicon molecular sieve, the titanium silicon molecular sieve can be synthesized by a traditional hydrothermal method, a dry gel method, a post-insertion method, or a rearrangement method. In the titanium silicon molecular sieve that is calcined to remove the template, the organic content is less than 0.01% of the weight of the molecular sieve. The calcination to remove the template can be carried out at a temperature greater than 300°C in an oxygen-rich or oxygen-poor atmosphere, or in a water vapor, ammonia atmosphere, alcoholamine atmosphere, or alcohol atmosphere, as long as the organic content in the titanium silicon molecular sieve is reduced to less than 0.01% of the weight of the molecular sieve. The preferred calcination temperature is 350-800°C, more preferably 400-600°C, and the time is 0.5-6h.
[0024] In the preparation method of the halogen-containing titanium silicon molecular sieve, the titanium silicon molecular sieve that has been calcined to remove the template agent is contacted with an organic amine solution with a carbon number of C1-C3 at 40-100°C to clean the channels of the titanium silicon molecular sieve, and this operation has a good effect on activating the titanium silicon molecular sieve framework. The organic amine with a carbon number of C1-C3 includes primary amines, secondary amines, tertiary amines, alcohol amines, and diamines; preferably, the organic amine with a carbon number of C1-C3 is selected from one or more of methylamine, ethylamine, propylamine, dimethylamine, trimethylamine, ethanolamine, propanolamine, ethylenediamine, and propylenediamine.
[0025] In the preparation method of the halogen-containing titanium silicon molecular sieve, in the organic amine solution with a carbon number of C1-C3, the solvent is selected from water, C1-C10 alcohol, C2-C10 ester or C3-C8 ketone. For example, it can be methanol, ethanol, n-propanol, isopropanol, n-butanol, 2-butanol, isobutanol, tert-butanol, n-pentanol, isopentanol, cyclopentanol, n-hexanol, cyclohexanol, n-octanol, methyl formate, ethyl acetate, isopropyl acetate, n-butyl acetate, acetone, butanone, cyclopentanone, cyclohexanone, cycloheptanone, cyclooctanone. Preferably, the organic amine solution with a carbon number of C1-C3 is an aqueous solution of an organic amine with a carbon number of C1-C3.
[0026] In the preparation method of the halogen-containing titanium silicon molecular sieve, the mass fraction of the organic amine in the organic amine solution with a carbon number of C1-C3 is preferably 0.1%-1.5%, preferably 0.2%-1%.
[0027] In the preparation method of the halogen-containing titanium silicon molecular sieve, the step of "contacting the titanium silicon molecular sieve after calcination to remove the template with an organic amine solution with a carbon number of C1-C3 at 40-100°C, and washing and drying the separated solid product" is preferably carried out at 60-80°C for 30-120 minutes, and the separation process can be centrifugation, evaporation, membrane separation, filtration, etc.; the washing is preferably carried out with water or alcohol solution, and the washing is carried out until the liquid pH value is less than 8, and then drying is carried out. The preferred drying temperature is 80-200°C and the time is 0.5-12h.
[0028] In the preparation method of the halogen-containing titanium silicon molecular sieve, the small molecule silanization agent has the following structure: R 1(m) -Si-OR 2(n) , or R 1(m) -Si-X (n) , where the general formula of R1 is C x H y X z, R2 is methyl or ethyl, m and n are positive integers, and m+n=4, y+z=2x+1, and x is a positive integer from 1 to 3, and X is at least one of fluorine, chlorine, bromine, and iodine. Preferably, m=1, R2 is methyl, z=1 or 2, more preferably 1, and the halogen is chlorine. More specifically but not limited thereto, the small molecule silylating agent is selected from chloromethyltrimethoxysilane, bromomethyltrimethoxysilane, chloromethyltriethoxysilane, chloroethyltrimethoxysilane, chloroethyltriethoxysilane, chloropropyltrimethoxysilane, chloropropyltriethoxysilane, dichloromethyldimethoxysilane, dichloromethyldiethoxysilane, 1,2-dichloroethyltrimethoxysilane, 1,2-dichloroethyltriethoxysilane, 1,2-dichloropropyltrimethoxysilane, 1,2-dichloropropyltriethoxysilane, chloromethyltrichlorosilane, dichloromethyldichlorosilane, chloroethyltrichlorosilane, dichloromethyldimethoxysilane, dichloromethyldiethoxysilane, 1,2-dichloroethyltrimethoxysilane, 1,2-dichloroethyltriethoxysilane, 1,2-dichloropropyltrimethoxysilane, 1,2-dichloropropyltriethoxysilane, chloromethyltrichlorosilane, dichloromethyldichlorosilane, chloroethyltrichlorosilane, dichloromethyldimethoxysilane, dichloromethyldiethoxysilane, dichloromethyldimeth ... Ethyldichlorosilane, chloropropyltrichlorosilane, dichloropropyldichlorosilane, 1,2-dichloroethyltrichlorosilane, 1,2-dichloroethyltrichlorosilane, di(1,2-dichloropropyl)dichlorosilane, di(1,2-dichloropropyl)dichlorosilane; preferred small molecule silanization agents are chloromethyltrimethoxysilane, chloroethyltrimethoxysilane, chloropropyltrimethoxysilane, 1,2-dichloroethyltrimethoxysilane, 1,2-dichloropropyltrimethoxysilane, chloromethyltrichlorosilane, chloroethyltrichlorosilane, chloropropyltrichlorosilane, 1,2-dichloroethyltrichlorosilane, and 1,2-dichloropropyltrichlorosilane.
[0029] In the preparation method of the halogen-containing titanium silicon molecular sieve, the solvent in the solution containing the small molecule silanization agent is selected from C3-C8 ketones, C2-C10 esters or C6-C12 alkanes. For example: acetone, butanone, cyclopentanone, cyclohexanone, acetylacetone, cycloheptanone, cyclooctanone, acetophenone, methyl formate, ethyl acetate, isopropyl acetate, butyl acetate, n-hexane, cyclohexane, n-heptane, n-octane, n-decane, benzene, toluene, ethylbenzene, isopropylbenzene, xylene, trimethylbenzene. Ketone is preferably used as the solvent, and more preferably the solvent is one or more of acetone, butanone, cyclopentanone and acetylacetone.
[0030] In the preparation method of the halogen-containing titanium silicalite, the molar ratio of the small molecule silanization agent to the titanium silicalite is preferably (0.001-0.05):1, preferably (0.005-0.03):1; the molar ratio of the solvent containing the small molecule silanization agent to the titanium silicalite is preferably (5-100):1, preferably (20-60:1), the silanization agent is calculated as Si, and the titanium silicalite is calculated as SiO2.
[0031] In the preparation method of the halogen-containing titanium silicon molecular sieve, the contact between the titanium silicon molecular sieve and the organic amine solution with a carbon number of C1-C3 is preferably treated at 60-90°C for 2-8h; the calcination is preferably at a temperature of 350-800°C, more preferably 400-600°C, for 0.5-6h; and the drying is preferably at a temperature of 80-200°C for 0.5-12h.
[0032] In the method of the present invention, the halogen-containing titanium silicon molecular sieve can be used directly as a catalyst, or can be mixed with other catalysts, co-catalysts, carriers, etc., and can be used after being formed. The mass content of the halogen-containing titanium silicon molecular sieve in the formed catalyst is preferably greater than 5%.
[0033] In the method of the present invention, the titanium silicate molecular sieve having halogen atoms and organic groups in the pores is used as a catalyst, which can effectively improve the compatibility of the titanium silicate molecular sieve with the organic substrate, thereby showing excellent performance in catalytic reaction or adsorption separation.
[0034] In the method of the present invention, the carbonyl-containing compound is preferably an aldehyde, ketone, acid, ester, carboxylate with a carbon number of C2-C20, and contains at least one carbonyl group. The aldehyde contains at least one aldehyde group and may also contain other groups, such as alkyl, cycloalkyl, aryl, halogen, double bond, triple bond, N, S, O, P, ether bond, ester group, ketone group, hydroxyl, carboxyl group. The aldehyde may be one or more of acetaldehyde, propionaldehyde, butyraldehyde, valeraldehyde, hexanal, heptaldehyde, acrolein, crotonaldehyde, pentenealdehyde, hexenealdehyde, benzaldehyde, phenylacetaldehyde, malondialdehyde, succinaldehyde, glutaraldehyde, adipaldehyde, furandicarboxaldehyde, preferably one or more of acetaldehyde, butyraldehyde, succinaldehyde, glutaraldehyde, adipaldehyde, furandicarboxaldehyde. The ketone contains at least one ketone group and may also contain other groups, such as alkyl, cycloalkyl, aryl, halogen, double bond, triple bond, N, S, O, ether bond, ester group, aldehyde group, hydroxyl, carboxyl group. The ketone can be one or more of acetone, butanone, pentanone, hexanone, heptanone, dodecanone, cyclopentanone, cyclohexanone, cyclooctanone, cyclododecanone, acetophenone, propiophenone, cyclopentanedione, cyclohexanedione, cyclohexenone, and anthraquinone. Preferably, one or more of acetone, butanone, cyclopentanone, cyclohexanone, cyclooctanone, cyclododecanone, and acetophenone are used. The acid contains at least one carboxyl group and can also contain other groups, such as alkyl, cycloalkyl, aryl, halogen, double bond, triple bond, N, S, O, ether bond, ester group, ketone group, hydroxyl, and aldehyde group. The acid can be one or more of acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, aminocaproic acid, mercaptocaproic acid, stearic acid, oleic acid, ricinoleic acid, malonic acid, succinic acid, glutaric acid, adipic acid, furandicarboxylic acid, benzoic acid, phthalic acid, terephthalic acid, and isophthalic acid. Preferably, one or more of malonic acid, succinic acid, glutaric acid, adipic acid, and furandicarboxylic acid. The ester contains at least one ester group and may also contain other groups, such as alkyl, cycloalkyl, aryl, halogen, double bond, triple bond, N, S, O, ether bond, aldehyde group, ketone group, hydroxyl, and carboxyl. The ester may be one or more of methyl formate, methyl acetate, ethyl acetate, ethyl formate, butyl acetate, propyl acetate, dimethyl malonate, dimethyl succinate, dimethyl glutarate, dimethyl adipate, diethyl adipate, and dimethyl furandicarboxylic acid. Preferably, one or more of ethyl acetate, butyl acetate, dimethyl succinate, dimethyl glutarate, dimethyl adipate, and dimethyl furandicarboxylic acid. The carboxylate contains at least one carboxyl group and may also contain other groups, such as alkyl, cycloalkyl, aryl, halogen, double bond, triple bond, N, S, O, ether bond, ester group, ketone group, hydroxyl group, and aldehyde group.The carboxylate can be one or more of ammonium acetate, ammonium propionate, ammonium butyrate, ammonium valerate, ammonium caproate, ammonium benzoate, ammonium malonate, ammonium succinate, ammonium glutarate, ammonium adipate, ammonium furandicarboxylate, acetamide, propionamide, butanamide, valeramide, caproamide, acrylamide, crotonamide, pentaneamide, hexeneamide, malonyl diamine, succinyl diamine, glutaramide, adipic diamine, benzamide, furandicarboxylate, phthalamide, terephthalamide, and m-phthalamide. Preferably, one or more of ammonium acetate, ammonium adipate, ammonium furandicarboxylate, acetamide, succinyl diamine, and adipic diamine.
[0035] In the method of the present invention, the ammonia is preferably aqueous ammonia or liquid ammonia. The aqueous ammonia may be an aqueous ammonia solution with a mass concentration of 1% or more, preferably with a mass concentration of 5% to 20%. The liquid ammonia may be fed as a liquid or as a gas.
[0036] In the method of the present invention, the solvent includes water, C6-C12 alkanes, and C2-C10 alcohols. The alkanes may be one or more of hexane, heptane, octane, decane, cyclohexane, cyclooctane, benzene, toluene, xylene, ethylbenzene, and isopropylbenzene. The alcohol may be one or more of ethanol, propanol, butanol, pentanol, hexanol, octanol, cyclopentanol, cyclohexanol, cyclohexanediol, benzyl alcohol, and phenylethyl alcohol.
[0037] In the method of the present invention, the molar ratio of hydrogen peroxide to the carbonyl-containing compound is preferably (0.3-3): 1, and more preferably (1-1.8): 1. The molar ratio of ammonia to the carbonyl-containing compound is preferably (0.3-5): 1, and more preferably (1-3): 1. The molar ratio of the solvent to the carbonyl-containing compound is preferably (2-50): 1, and more preferably (5-20): 1.
[0038] In the method of the present invention, the weight hourly space velocity of the carbonyl-containing compound based on the halogen-containing titanium silicon molecular sieve is preferably 0.1-3h -1 , further preferably 0.2-1.5h -1 The contacting is preferably carried out at 40-100°C.
[0039] The method of the present invention can be carried out in a slurry bed reactor, a fixed bed reactor, a microchannel reactor, or a fluidized bed reactor, and the present invention has no particular limitation. When the ammoximation method is carried out in a non-fixed bed reactor, the catalyst can be recycled by centrifugal separation, filtration separation, membrane separation, sedimentation separation, and the like.
[0040] The present invention will be further described below by way of examples, but the present invention is not limited thereto.
[0041] In the preparation example, the X-ray powder diffraction (XRD) spectrum of the titanium silicalite was measured on a Siemens D5005 X-ray diffractometer. XRF was measured using a 3013 X-ray fluorescence spectrometer produced by Rigaku Corporation. XPS was measured using an ESCALab250 X-ray photoelectron spectrometer produced by ThermoFisher Scientific. The infrared hydroxyl spectrum of the titanium silicalite was measured on a Nicolet 870 Fourier transform infrared spectrometer. The sample was pressed into a self-supporting sheet, placed in an infrared cell, and heated at 1×10 -3 The samples were treated at 450 °C for 3 h under Pa conditions, and the infrared hydroxyl spectrum of the samples was measured.
[0042] In the preparation example, the carbon content of the titanium silicon molecular sieve is measured using a CS-844 high-frequency infrared carbon-sulfur analyzer (LECO Analytical Instruments Co., Ltd., USA). The specific process is to put the weighed sample to be tested together with the flux into a high-frequency induction furnace, and burn it at high temperature after passing oxygen. The CO2 gas generated by carbon flows through an infrared detector for detection, and the carbon content of the titanium silicon molecular sieve is calculated. (Reference: Shen Shanwen, et al. Determination of carbon and sulfur in precious metal catalysts by high-frequency infrared absorption method, precious metals, 2001).
[0043] The raw materials used in the examples and comparative examples are all commercially available and analytically pure.
[0044] Gas chromatography was used to analyze the product composition.
[0045] Conversion rate of carbonyl compound = (molar amount of carbonyl compound in raw material - molar amount of carbonyl compound remaining in product) / molar amount of carbonyl compound in raw material × 100%
[0046] Oxime selectivity = molar amount of oxime generated in the product / (molar amount of carbonyl compound in the raw material - molar amount of carbonyl compound remaining in the product) × 100%
[0047] Preparation Example 1
[0048] TS-1 molecular sieve was prepared according to the method of Zeolites, 1992, Vol. 12, pp. 943-950.
[0049] At room temperature, the above substances are mixed under stirring according to the molar ratio of 1:0.03:0.2:25 of tetraethyl orthosilicate (in terms of SiO2): tetrabutyl titanate (in terms of TiO2): tetrapropylammonium hydroxide (in terms of N): deionized water, and then transferred to a pressure-resistant stainless steel reactor, crystallized at 170°C and autogenous pressure for 72 hours, and then filtered, washed and recovered The solid product is dried in an oven at 120°C for 12 hours, and then calcined at 550°C in an air atmosphere for 6 hours. The organic matter content is less than 0.01% of the weight of the molecular sieve, and a titanium silicon molecular sieve numbered TS-1-A is obtained.
[0050] XRF, XPS, low temperature nitrogen adsorption and desorption characterization results, infrared spectrum characterization characteristic peak intensity ratio I 3740 / I 3530 See Table 1.
[0051] Preparation Example 2
[0052] TS-1 molecular sieve was prepared according to the method of Zeolites, 1992, Vol. 12, pp. 943-950.
[0053] At room temperature, the above substances are mixed under stirring according to the molar ratio of 1:0.01:0.2:25 of tetraethyl orthosilicate (in terms of SiO2): tetrabutyl titanate (in terms of TiO2): tetrapropylammonium hydroxide (in terms of N): deionized water, and then transferred to a pressure-resistant stainless steel reactor, crystallized at 170°C and autogenous pressure for 72 hours, and then filtered, washed and recovered The solid product is dried in an oven at 120°C for 12 hours, and then calcined at 550°C in an air atmosphere for 6 hours. The organic matter content is less than 0.01% of the weight of the molecular sieve, and a titanium silicon molecular sieve numbered TS-1-B is obtained.
[0054] XRF, XPS, low temperature nitrogen adsorption and desorption characterization results, infrared spectrum characterization characteristic peak intensity ratio I 3740 / I 3530 See Table 1.
[0055] Preparation Example 3
[0056] This preparation example illustrates the treatment of titanium silicalite molecular sieve with a commonly used silanization agent.
[0057] Titanium silicate molecular sieve TS-1-A was mixed with a toluene solution containing 3-(phenylamino)propyltrimethoxysilane and treated at 80°C for 6 hours, wherein the silanization agent (calculated as Si): titanium silicate molecular sieve (calculated as SiO2) = 0.02:1 (molar ratio), solvent: titanium silicate molecular sieve (calculated as SiO2) = 60:1 (molar ratio), and then the molecular sieve was separated and dried at 120°C for 12 hours to obtain the titanium silicate molecular sieve with surface silanization treatment.
[0058] XRF, XPS, low temperature nitrogen adsorption and desorption characterization results, infrared spectrum characterization characteristic peak intensity ratio I 3740 / I 3530 See Table 1.
[0059] Preparation Example 4
[0060] (1) Mix titanium silicalite TS-1-A with an aqueous solution of methylamine, with the mass fraction of organic amine being 0.5%, and then treat at 80°C for 120 minutes, separate the TS-1-A molecular sieve, wash it with deionized water until the pH is less than 8, and dry it at 120°C for 12 hours.
[0061] (2) The titanium silicalite obtained in step (1) is mixed with a butanone solution containing chloromethyltrimethoxysilane, and treated at 80°C for 6 hours, wherein the silanization agent (calculated as Si): titanium silicalite (calculated as SiO2) = 0.02:1 (molar ratio), and the solvent: titanium silicalite (calculated as SiO2) = 60:1 (molar ratio). The molecular sieve is then separated and dried at 120°C for 12 hours to obtain a halogen-containing titanium silicalite.
[0062] XRF, XPS, low temperature nitrogen adsorption and desorption characterization results, infrared spectrum characterization characteristic peak intensity ratio I 3740 / I 3530 See Table 1.
[0063] Preparation Example 5
[0064] (1) Mix titanium silicalite TS-1-A with an aqueous solution of ethylamine, with the mass fraction of organic amine being 1.0%, and then treat at 80°C for 90 minutes, separate the TS-1-A molecular sieve, wash it with deionized water until the pH is less than 8, and dry it at 120°C for 12 hours.
[0065] (2) The titanium silicalite obtained in step (1) is mixed with a cyclopentanone solution containing chloropropyltrimethoxysilane, and treated at 70°C for 6 hours, wherein the silanization agent (calculated as Si): titanium silicalite (calculated as SiO2) = 0.01:1 (molar ratio), and the solvent: titanium silicalite (calculated as SiO2) = 40:1 (molar ratio). The molecular sieve is then separated and dried at 120°C for 12 hours to obtain the halogen-containing titanium silicalite.
[0066] XRF, XPS, low temperature nitrogen adsorption and desorption characterization results, infrared spectrum characterization characteristic peak intensity ratio I 3740 / I 3530 See Table 1.
[0067] Preparation Example 6
[0068] (1) Mix titanium silicalite TS-1-A with an aqueous solution of ethanolamine, with the mass fraction of organic amine being 0.5%, and then treat at 80°C for 60 minutes, separate the TS-1-A molecular sieve, wash it with deionized water until the pH is less than 8, and dry it at 120°C for 12 hours.
[0069] (2) Mix the titanium silicalite obtained in step (1) with an acetylacetone solution containing chloroethyltrichlorosilane, and treat at 90°C for 4 hours, wherein the silanization agent (calculated as Si): titanium silicalite (calculated as SiO2) = 0.005:1 (molar ratio), and the solvent: titanium silicalite (calculated as SiO2) = 20:1 (molar ratio). Then separate the molecular sieve and dry it at 120°C for 12 hours to obtain the halogen-containing titanium silicalite.
[0070] XRF, XPS, low temperature nitrogen adsorption and desorption characterization results, infrared spectrum characterization characteristic peak intensity ratio I 3740 / I 3530 See Table 1.
[0071] Preparation Example 7
[0072] (1) Mix titanium silicalite TS-1-A with an aqueous solution of ethylenediamine, with the mass fraction of organic amine being 0.2%, and then treat at 80°C for 120 minutes, separate the TS-1-A molecular sieve, wash it with deionized water until the pH is less than 8, and dry it at 120°C for 12 hours.
[0073] (2) The titanium silicalite obtained in step (1) is mixed with a butanone solution containing chloroethyltrimethoxysilane, and treated at 70°C for 2 hours, wherein the silanization agent (calculated as Si): titanium silicalite (calculated as SiO2) = 0.03:1 (molar ratio), and the solvent: titanium silicalite (calculated as SiO2) = 40:1 (molar ratio). The molecular sieve is then separated and dried at 120°C for 12 hours to obtain a halogen-containing titanium silicalite.
[0074] XRF, XPS, low temperature nitrogen adsorption and desorption characterization results, infrared spectrum characterization characteristic peak intensity ratio I 3740 / I 3530 See Table 1.
[0075] Preparation Example 8
[0076] (1) Mix titanium silicalite TS-1-A with an aqueous solution of dimethylamine, with the mass fraction of organic amine being 1.0%, and then treat at 60°C for 120 minutes, separate the TS-1-A molecular sieve, wash it with deionized water until the pH is less than 8, and dry it at 120°C for 12 hours.
[0077] (2) Mix the titanium silicalite obtained in step (1) with an acetone solution containing 1,2-dichloropropyltrichlorosilane, and treat at 60°C for 8 hours, wherein the silanization agent (calculated as Si): titanium silicalite (calculated as SiO2) = 0.025:1 (molar ratio), and the solvent: titanium silicalite (calculated as SiO2) = 20:1 (molar ratio). Then separate the molecular sieve and dry it at 120°C for 12 hours to obtain the halogen-containing titanium silicalite.
[0078] XRF, XPS, low temperature nitrogen adsorption and desorption characterization results, infrared spectrum characterization characteristic peak intensity ratio I 3740 / I 3530 See Table 1.
[0079] Preparation Example 9
[0080] (1) Mix titanium silicalite TS-1-B with an aqueous solution of propylamine, with the mass fraction of organic amine being 1.0%, and then treat at 80°C for 90 minutes, separate the TS-1-B molecular sieve, wash it with deionized water until the pH is less than 8, and dry it at 120°C for 12 hours.
[0081] (2) The titanium silicalite obtained in step (1) is mixed with a cyclopentanone solution containing chloromethyltrichlorosilane, and treated at 80°C for 4 hours, wherein the silanization agent (calculated as Si): titanium silicalite (calculated as SiO2) = 0.02:1 (molar ratio), and the solvent: titanium silicalite (calculated as SiO2) = 60:1 (molar ratio). The molecular sieve is then separated and dried at 120°C for 12 hours to obtain the halogen-containing titanium silicalite.
[0082] XRF, XPS, low temperature nitrogen adsorption and desorption characterization results, infrared spectrum characterization characteristic peak intensity ratio I 3740 / I 3530 Table 1.
[0083] Preparation Example 10
[0084] (1) Mix titanium silicalite TS-1-B with a methanol solution of methylamine, with the mass fraction of the organic amine being 0.1%, and then treat at 50°C for 180 minutes, separate the TS-1-B molecular sieve, wash it with deionized water until the pH is less than 8, and dry it at 120°C for 12 hours.
[0085] (2) The titanium silicalite obtained in step (1) is mixed with an ethyl acetate solution containing dichloromethyldimethoxysilane, and treated at 50°C for 12 hours, wherein the silanization agent (calculated as Si): titanium silicalite (calculated as SiO2) = 0.05:1 (molar ratio), and the solvent: titanium silicalite (calculated as SiO2) = 100:1 (molar ratio). The molecular sieve is then separated and dried at 120°C for 12 hours to obtain the halogen-containing titanium silicalite.
[0086] XRF, XPS, low temperature nitrogen adsorption and desorption characterization results, infrared spectrum characterization characteristic peak intensity ratio I 3740 / I 3530 See Table 1.
[0087] Preparation Example 11
[0088] (1) Mix titanium silicalite TS-1-B with an ethanol solution of trimethylamine, with the mass fraction of the organic amine being 1.5%, and then treat at 40°C for 180 minutes, separate the TS-1-B molecular sieve, wash it with deionized water until the pH is less than 8, and dry it at 120°C for 12 hours.
[0089] (2) Mix the titanium silicalite obtained in step (1) with an isopropyl acetate solution containing dichloromethyldichlorosilane, and treat at 100°C for 24 hours, wherein the silanization agent (calculated as Si): titanium silicalite (calculated as SiO2) = 0.001:1 (molar ratio), and the solvent: titanium silicalite (calculated as SiO2) = 10:1 (molar ratio), then separate the molecular sieve, and dry at 120°C for 12 hours to obtain the halogen-containing titanium silicalite.
[0090] XRF, XPS, low temperature nitrogen adsorption and desorption characterization results, infrared spectrum characterization characteristic peak intensity ratio I 3740 / I 3530 See Table 1.
[0091] Table 1
[0092]
[0093]
[0094] As can be seen from Table 1, the titanium silicalite molecular sieves (Preparation Examples 4 to 11) used in the present invention contain halogen atoms and organic groups, and the R XRF / R XPS Greater than 2, I 3740 / I 3530 Greater than 4, micropore specific surface area is 350-420m 2 / g, and the micropore volume is 0.130-0.170mL / g, which is lower than the results of conventional samples. These results indicate that the halogen atoms and organic groups are mainly present in the pores of the molecular sieve.
[0095] Example 1
[0096] Cyclohexanone, water, and the halogen-containing titanium silicon molecular sieve obtained in Preparation Example 4 were mixed and placed in a continuous reaction kettle, and liquid ammonia and hydrogen peroxide (30%) were continuously fed, and the catalyst was separated by a membrane and then continuously discharged. Among them, hydrogen peroxide: cyclohexanone = 1.3:1, ammonia: cyclohexanone = 1.5:1, solvent: cyclohexanone = 15:1, and the weight hourly space velocity of cyclohexanone based on the catalyst was 1h -1 The mixture was reacted continuously at 90°C, and samples were taken regularly to analyze the product composition and determine the catalyst life. The results are shown in Table 2.
[0097] Example 2
[0098] Cyclohexanone, tert-butyl alcohol, and the halogen-containing titanium silicon molecular sieve obtained in Preparation Example 5 were mixed and placed in a continuous reaction kettle, and ammonia water (20%) and hydrogen peroxide (30%) were continuously fed, and the materials were continuously discharged after the catalyst was separated by a membrane. Among them, hydrogen peroxide: cyclohexanone = 1.8:1, ammonia: cyclohexanone = 2:1, solvent: cyclohexanone = 20:1, and the weight hourly space velocity of cyclohexanone based on the catalyst was 1.2h -1 The mixture was reacted continuously at 80°C, and samples were taken regularly to analyze the product composition and determine the catalyst life. The results are shown in Table 2.
[0099] Example 3
[0100] Cyclohexanone, cyclohexane, and the halogen-containing titanium silicon molecular sieve obtained in Preparation Example 6 were mixed and placed in a continuous reaction kettle, and ammonia (10%) and hydrogen peroxide (50%) were continuously fed, and the catalyst was separated by a membrane and then discharged continuously. Among them, hydrogen peroxide: cyclohexanone = 1.5:1, ammonia: cyclohexanone = 2.5:1, solvent: cyclohexanone = 15:1, and the weight hourly space velocity of cyclohexanone based on the catalyst was 1.5h -1 The mixture was reacted continuously at 60°C, and samples were taken regularly to analyze the product composition and determine the catalyst life. The results are shown in Table 2.
[0101] Example 4
[0102] Glutaraldehyde, toluene, and the halogen-containing titanium silicon molecular sieve obtained in Preparation Example 7 were mixed and placed in a continuous reaction kettle, and ammonia water (15%) and hydrogen peroxide (30%) were continuously fed, and the materials were continuously discharged after the catalyst was separated by a membrane. Among them, hydrogen peroxide: glutaraldehyde = 1.2: 1, ammonia: cyclohexanone = 1: 1, solvent: cyclohexanone = 10: 1, and the weight hourly space velocity of glutaraldehyde based on the catalyst was 0.5h -1The mixture was reacted continuously at 70°C, and samples were taken regularly to analyze the product composition and determine the catalyst life. The results are shown in Table 2.
[0103] Example 5
[0104] Acetone, tert-butyl alcohol, and the halogen-containing titanium silicon molecular sieve obtained in Preparation Example 8 were mixed and placed in a continuous reaction kettle, and ammonia water (5%) and hydrogen peroxide (27%) were continuously fed, and the materials were continuously discharged after the catalyst was separated by a membrane. Among them, hydrogen peroxide: acetone = 1: 1, ammonia: cyclohexanone = 3: 1, solvent: cyclohexanone = 5: 1, and the weight hourly space velocity of acetone based on the catalyst was 1.2 h -1 The mixture was reacted continuously at 80°C, and samples were taken regularly to analyze the product composition and determine the catalyst life. The results are shown in Table 2.
[0105] Example 6
[0106] Cyclohexanone, water, and the halogen-containing titanium silicon molecular sieve obtained in Preparation Example 9 were mixed and placed in a continuous reaction kettle, and liquid ammonia and hydrogen peroxide (30%) were continuously fed, and the catalyst was separated by a membrane and then continuously discharged. Among them, hydrogen peroxide: cyclohexanone = 1.3:1, ammonia: cyclohexanone = 1.5:1, solvent: cyclohexanone = 15:1, and the weight hourly space velocity of cyclohexanone based on the catalyst was 1h -1 The mixture was reacted continuously at 90°C, and samples were taken regularly to analyze the product composition and determine the catalyst life. The results are shown in Table 2.
[0107] Example 7
[0108] Cyclohexanone, cyclohexane, and the halogen-containing titanium silicon molecular sieve obtained in Preparation Example 10 were mixed and placed in a continuous reaction kettle, and liquid ammonia and hydrogen peroxide (30%) were continuously fed, and the catalyst was separated by a membrane and then continuously discharged. Among them, hydrogen peroxide: cyclohexanone = 2:1, ammonia: cyclohexanone = 5:1, solvent: cyclohexanone = 50:1, and the weight hourly space velocity of cyclohexanone based on the catalyst was 2h -1 The mixture was reacted continuously at 100°C, and samples were taken regularly to analyze the product composition and determine the catalyst life. The results are shown in Table 2.
[0109] Example 8
[0110] Cyclohexanone, tert-butyl alcohol, and the halogen-containing titanium silicon molecular sieve obtained in Preparation Example 11 were mixed and placed in a continuous reaction kettle, and liquid ammonia and hydrogen peroxide (30%) were continuously fed, and the catalyst was separated by a membrane and then continuously discharged. Among them, hydrogen peroxide: cyclohexanone = 3:1, ammonia: cyclohexanone = 3.5:1, solvent: cyclohexanone = 30:1, and the weight hourly space velocity of cyclohexanone based on the catalyst was 3h -1 The mixture was reacted continuously at 40°C, and samples were taken regularly to analyze the product composition and determine the catalyst life. The results are shown in Table 2.
[0111] Example 9
[0112] Cyclododecanone, tert-butyl alcohol, and the halogen-containing titanium silicon molecular sieve obtained in Preparation Example 4 were mixed and placed in a continuous reaction kettle, and liquid ammonia and hydrogen peroxide (30%) were continuously fed, and the catalyst was separated by a membrane and then continuously discharged. Among them, hydrogen peroxide: cyclododecanone = 1.5:1, ammonia: cyclododecanone = 1:1, solvent: cyclododecanone = 10:1, and the weight hourly space velocity of cyclododecanone based on the catalyst was 1h -1 The mixture was reacted continuously at 80°C, and samples were taken regularly to analyze the product composition and determine the catalyst life. The results are shown in Table 2.
[0113] Example 10
[0114] Furandicarboxylic acid, cyclohexane, and the halogen-containing titanium silicon molecular sieve obtained in Preparation Example 4 were mixed and placed in a continuous reaction kettle, and ammonia water (15%) and hydrogen peroxide (30%) were continuously fed, and the catalyst was separated by a membrane and then continuously discharged. Among them, hydrogen peroxide: furandicarboxylic acid = 1.2:1, ammonia: furandicarboxylic acid = 1.5:1, solvent: furandicarboxylic acid = 5:1, and the weight hourly space velocity of furandicarboxylic acid based on the catalyst was 0.5h -1 The mixture was reacted continuously at 60°C, and samples were taken regularly to analyze the product composition and determine the catalyst life. The results are shown in Table 2.
[0115] Embodiment 11
[0116] Acetaldehyde, tert-butyl alcohol, and the halogen-containing titanium silicon molecular sieve obtained in Preparation Example 4 were mixed and placed in a continuous reaction kettle, and ammonia water (10%) and hydrogen peroxide (30%) were continuously fed, and the materials were continuously discharged after the catalyst was separated by a membrane. Among them, hydrogen peroxide: acetaldehyde = 1:1, ammonia: acetaldehyde = 1.3:1, solvent: acetaldehyde = 10:1, and the weight hourly space velocity of acetaldehyde based on the catalyst was 0.2h -1 The mixture was reacted continuously at 50°C, and samples were taken regularly to analyze the product composition and determine the catalyst life. The results are shown in Table 2.
[0117] Comparative Example 1
[0118] The difference from Example 1 is that the halogen-free titanium silicon molecular sieve obtained in Preparation Example 1 is used as a catalyst. The results are shown in Table 2.
[0119] Comparative Example 2
[0120] The difference from Example 1 is that the halogen-free titanium silicon molecular sieve obtained in Preparation Example 2 is used as a catalyst. The results are shown in Table 2.
[0121] Comparative Example 3
[0122] The difference from Example 1 is that the halogen-free titanium silicon molecular sieve obtained in Preparation Example 3 is used as a catalyst. The results are shown in Table 2.
[0123] Table 2
[0124] Reaction time / h Hydrogen peroxide conversion rate / % Oxime selectivity / % Example 1 650 99 99 Example 2 680 99 99 Example 3 630 99 99 Example 4 660 99 99 Example 5 690 99 99 Example 6 410 96 99 Example 7 350 92 99 Example 8 320 92 99 Example 9 630 99 99 Example 10 640 99 99 Embodiment 11 695 99 99 Comparative Example 1 180 87 96 Comparative Example 2 150 84 95 Comparative Example 3 230 90 97
[0125] As can be seen from Table 2, the ammoximation method of the present invention has a simple operation process and significantly improves the catalyst life while ensuring a high carbonyl compound conversion rate and oxime selectivity.
Claims
1. A method for ammoximation, characterized in that: A carbonyl compound, hydrogen peroxide, ammonia, a solvent, and a halogen-containing titanium silicon molecular sieve are contacted to obtain a liquid product containing oxime, wherein the halogen-containing titanium silicon molecular sieve is obtained by the following preparation method: the titanium silicon molecular sieve from which the template is removed by calcination is contacted with an organic amine solution having a carbon number of C1-C3 at 40-100° C., the separated solid product is washed and dried, and then contacted with a solution containing a small molecule silanization agent at 50-120° C., and then separated and dried; the small molecule silanization agent has the following structure: R 1(m) -Si-OR 2(n) , or R 1(m) -Si-X (n) , where the general formula of R1 is C x H y X z , R2 is methyl or ethyl, m and n are positive integers, and m+n=4, y+z=2x+1, and x is a positive integer from 1 to 3, and X is at least one of fluorine, chlorine, bromine, and iodine; the halogen-containing titanium silicon molecular sieve contains 0.5%-5% halogen and 0.5%-4% carbon by weight of the total molecular sieve; in the halogen-containing titanium silicon molecular sieve, R XRF / R XPS Value greater than 2, R XRF is the atomic ratio of halogen to silicon in the molecular sieve bulk phase analyzed by XRF, R XPS is the atomic ratio of halogen to silicon on the molecular sieve surface analyzed by XPS; the halogen-containing titanium silicon molecular sieve is characterized by infrared spectroscopy, and the ratio of its characteristic peak intensity I 3740 / I 3530 For 4-10, I 3740 The infrared spectrum of the hydroxyl group of the molecular sieve is 3740 cm -1 The absorption peak intensity at I 3530 3530cm in the infrared spectrum of molecular sieve -1 The absorption peak intensity at .
2. The method according to claim 1, wherein: The halogen-containing titanium silicon molecular sieve contains 0.5%-4% halogen and 0.8%-2.5% carbon, respectively, accounting for the total weight of the molecular sieve.
3. The method according to claim 1, wherein: In the halogen-containing titanium silicon molecular sieve, the halogen is one of fluorine, chlorine, bromine and iodine.
4. The method according to claim 1, wherein: R XRF / R XPS The value is 2.5-4.
5. The method according to claim 1, wherein: In the halogen-containing titanium silicon molecular sieve, the molecular sieve titanium silicon molar ratio is (0.001-0.05):
1.
6. The method according to claim 1, wherein: In the halogen-containing titanium silicon molecular sieve, the framework structure of the molecular sieve is an MFI structure.
7. The method according to claim 1, wherein: The halogen-containing titanium silicon molecular sieve has a micropore specific surface area of 350-420 m 2 / g, and the micropore volume is 0.130-0.170mL / g.
8. The method according to claim 1, wherein: The carbonyl-containing compound is an aldehyde, ketone, acid, ester, or carboxylate with a carbon number of C2-C20 and contains at least one carbonyl group.
9. The method according to claim 8, wherein: The aldehyde is one or more of acetaldehyde, propionaldehyde, butyraldehyde, valeraldehyde, hexanal, heptaldehyde, acrolein, crotonaldehyde, pentenaldehyde, hexenaldehyde, benzaldehyde, phenylacetaldehyde, malondialdehyde, succinic dialdehyde, glutaraldehyde, adipaldehyde, and furandicarboxaldehyde; the ketone is one or more of acetone, butanone, pentanone, hexanone, heptanone, dodecanone, cyclopentanone, cyclohexanone, cyclooctanone, cyclododecanone, acetophenone, propiophenone, cyclopentanedione, cyclohexanedione, cyclohexenone, and anthraquinone; the acid is acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, aminocaproic acid, mercaptocaproic acid, stearic acid, oleic acid, ricinoleic acid, malonic acid, succinic dialdehyde, The ester is one or more of methyl formate, methyl acetate, ethyl acetate, ethyl formate, butyl acetate, propyl acetate, dimethyl malonate, dimethyl succinate, dimethyl glutarate, dimethyl adipate, diethyl adipate, and dimethyl furandicarboxylate; the carboxylate is one or more of ammonium acetate, ammonium propionate, ammonium butyrate, ammonium valerate, ammonium caproate, ammonium benzoate, ammonium malonate, ammonium succinate, ammonium glutarate, ammonium adipate, and ammonium furandicarboxylate.
10. The method according to claim 1, wherein: The ammonia is aqueous ammonia or liquid ammonia.
11. The method according to claim 1, wherein: The solvent includes water, C6-C12 alkane, and C2-C10 alcohol.
12. The method according to claim 11, wherein: The C6-C12 alkane is one or more of hexane, heptane, octane, decane, cyclohexane, cyclooctane, benzene, toluene, xylene, ethylbenzene, and isopropylbenzene; the C2-C10 alcohol is one or more of ethanol, propanol, butanol, pentanol, hexanol, octanol, cyclopentanol, cyclohexanol, cyclohexanediol, benzyl alcohol, and phenylethyl alcohol.
13. The method according to claim 1, wherein: The molar ratio of hydrogen peroxide to the carbonyl compound is (0.3-3):1, the molar ratio of ammonia to the carbonyl compound is (0.3-5):1, and the molar ratio of the solvent to the carbonyl compound is (2-50):
1.
14. The method according to claim 1, wherein: The weight hourly space velocity of the carbonyl compound based on the halogen-containing titanium silicon molecular sieve is 0.1-3h -1 .
15. The method according to claim 1, wherein: The contacting is carried out at 40-100°C.
Citation Information
Patent Citations
Preparation method for Ti-Si molecular sieve
CN1260241A
Preparation of porous crystalline synthetic material comprised of silicon and titanium oxides
US4410501A
Fluorine-containing titanium-silicon molecular sieve with MWW (Manual Wire Wrap) structure and preparation method and application thereof
CN102627291A
Preparation method of cyclohexanone-oxime
CN103288675A
Titanium silicalite molecular sieve catalyst and application of titanium silicalite molecular sieve in cyclohexanone ammoximation
CN104874419A
Cited By
Modified molecular sieve, preparation method thereof and application of modified molecular sieve in ammoximation reaction
CN120288797A