A functionalized olefin rubber material and preparation method thereof

Through the sulfur radical-vinyl-containing functional modification reaction, the problem of limited types of expensive catalysts and functional modifiers in olefin rubber modification is solved, and efficient and macroscopic preparation of functionalized olefin rubber materials is achieved, and the reaction complexity and Gel side reactions provide a wide variety of rubber composite materials.

CN115725027BActive Publication Date: 2024-11-15SOUTH CHINA UNIV OF TECH
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202211547260.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-05
Publication Date
2024-11-15
Estimated Expiration
2042-12-05

AI Technical Summary

Technical Problem

The existing olefin rubber modification technology requires the use of expensive catalysts, the types of functional modifiers are limited, the reaction process is complex and cumbersome, and gel side reactions are prone to occur.

Method used

Using the functional modification reaction of sulfur radical-vinyl-containing group, the crosslinked olefin rubber reacts with vinyl-containing modifiers at high temperatures, and a variety of functional groups are introduced to realize the functional modification of olefin rubber, avoiding expensive catalysts. and complex reaction processes.

Benefits of technology

It has achieved efficient introduction of various functional modifiers into the olefin rubber chain structure, solving the problems of limited types of functional modifiers and low reaction efficiency, and prepared easy-to-access and rich variety of functional olefin rubber materials as a brand new rubber composite Material interface coupling agent.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FHA0000006570450000011
    Figure FHA0000006570450000011
  • Figure GHA0000006570460000021
    Figure GHA0000006570460000021
  • Figure GHA0000006570460000041
    Figure GHA0000006570460000041
Patent Text Reader

Abstract

The present invention provides a functionalized olefin rubber material and a preparation method thereof, comprising the following steps: firstly, olefin rubber, rubber activator, rubber accelerator and sulfur are blended to prepare a rubber compound, and cross-linked olefin rubber is obtained after vulcanization treatment; then the cross-linked olefin rubber is crushed and mixed with a modifier and a good solvent to be uniformly stirred and reacted at high temperature; after the reaction is completed, the reactant is poured into a non-good solvent for washing and precipitation, and the functionalized olefin rubber is obtained after drying. The present invention is suitable for preparing various functionalized olefin rubber materials with functional groups, and the preparation method has the advantages of simple process, easy to obtain raw materials and rich variety, high yield and large-scale preparation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polymer materials, and more specifically to a functionalized olefin rubber material and a preparation method thereof. Background Art

[0002] As the most widely used and largest amount of rubber in the rubber industry, olefin rubber has been modified by introducing specific functional groups to improve its comprehensive performance and expand its application range. The commonly used olefin rubber modification technologies can be divided into two ways: monomer copolymerization and grafting modification. The former is to overcome the difference in the reactivity rate between the copolymer monomer and the diene monomer, and usually requires the use of specific expensive catalysts, such as; the latter is limited by the reaction inertness of olefin rubber itself, and the types of functional groups that can be introduced are small and the efficiency is low, there are many side reactions and the post-processing is cumbersome.

[0003] For example, a Chinese patent (patent number: CN113292667A) discloses a multi-polymer and a preparation method thereof. Based on the coordination polymerization technology, the copolymerization of various functional olefin monomers and conjugated diene monomers is realized, and functional groups are successfully introduced into the molecular chain structure of the prepared olefin rubber. However, this method often relies on specific and complex rare earth catalytic system technology; and in the reported related literature (J.Appl.Polym.Sci., 2013, 129, 2735; RSCAdv., 2019, 9, 18888) and patents (CN110818973A, CN108017727A), the thiol-ene click chemistry between the unsaturated double bonds in the olefin rubber and the thiol-containing compounds is used to graft functional groups on its side chains, but the thiol-containing compounds involved in this method are limited to alkyl thiols and their derivatives, and there are gel side reactions to varying degrees during the modification process. Other reported post-modification technologies for olefin rubbers are also mostly based on the unsaturated double bonds in the molecular chain structure of olefin rubbers, such as reacting olefin rubbers with functional modifiers containing reactive groups such as triazolinedione (Nat. Chem., 2014, 6, 815) or tetrazine (CN110506075A). However, there are fewer types of functional modifiers available for this method. Summary of the invention

[0004] The purpose of the present invention is to provide a functionalized olefin rubber material and a preparation method thereof, so as to solve the problems in the prior art that olefin rubber modification requires the use of expensive catalysts, the types of functional modifiers are limited, the reaction process is complicated and cumbersome, the reaction efficiency is low, and gelation side reactions will occur.

[0005] In order to achieve the above object, the present invention provides a method for preparing a functionalized olefin rubber material, comprising the following steps:

[0006] S1, blending olefin rubber, rubber activator, rubber accelerator and sulfur to prepare a rubber mix, and obtaining a cross-linked olefin rubber after vulcanization treatment;

[0007] S2, stirring and mixing the cross-linked olefin rubber, vinyl-containing modifier and good solvent prepared in step S1, and reacting at 140-200° C. for 10-120 min;

[0008] S3. Washing the precipitate in a non-good solvent and drying it to obtain a functionalized olefin rubber material.

[0009] Preferably, the vulcanization treatment method in step S1 includes molding at 140-190° C. and 15-20 kgf pressure according to the positive vulcanization time; and crushing the cross-linked olefin rubber in step S2 into powder.

[0010] Preferably, the olefin rubber is one or a combination of butadiene rubber, styrene-butadiene rubber, natural rubber, isoprene rubber, nitrile rubber, epoxy natural rubber, butyl rubber, chloroprene rubber, and EPDM rubber.

[0011] Preferably, the rubber activator is a combination of zinc oxide and stearic acid in a weight ratio of 5:1 to 2:1; the weight ratio of the rubber activator to the olefin rubber is 3:100 to 7:100.

[0012] Preferably, the rubber accelerator is one or a combination of benzothiazoles, thiurams, sulfenamides, guanidines, and dithiocarbamates; and the weight ratio of the rubber accelerator to the olefin rubber is 0.5:100 to 6:100.

[0013] Preferably, the weight ratio of the sulfur to the olefin rubber is 1.5:100 to 20:100.

[0014] Preferably, the vinyl-containing modifier is one or a combination of the compound of formula I, the compound of formula II, and the compound of formula III; the ratio of the vinyl-containing modifier is 100-1000 mL: 100 g of the cross-linked olefin rubber;

[0015]

[0016] Wherein, R in structural formula I, II, and III is selected from a hydrogen atom or a methyl group;

[0017] R1 in structural formula I is selected from a hydrogen atom, a C1-C18 alkane group, an oxygen-containing group, a nitrogen-containing group, and a silicon-containing group;

[0018] R2 in structural formula II is selected from a hydrogen atom, an oxygen-containing group, and a nitrogen-containing group;

[0019] R3, R4 and R5 in the structural formula III are selected from hydrogen atoms, C1-C6 alkane groups, phenyl groups, oxygen-containing groups and nitrogen-containing groups.

[0020] Preferably, the good solvent is one or a combination of acetone, butanone, cyclohexanone, tetrahydrofuran, n-hexane, cyclohexane, n-heptane, dichloromethane, chloroform, toluene, and xylene; the ratio of the good solvent is 500-1400 mL: 100 g of the cross-linked olefin rubber.

[0021] Preferably, the non-good solvent is one or a combination of methanol, ethanol, n-propanol, isopropanol, n-butanol, ethylene glycol, methyl acetate, ethyl acetate, and acetonitrile; the ratio of the non-good solvent is 500-1400 mL: 100 g of the cross-linked olefin rubber.

[0022] The present invention provides a functionalized olefin rubber material prepared by the preparation method described in the above scheme.

[0023] The present invention has the following beneficial effects:

[0024] The method of the present invention utilizes a sulfur free radical-vinyl functional modification reaction, and can efficiently introduce a variety of vinyl-containing functional modifiers into the olefin rubber chain structure to achieve functional modification of the olefin rubber. Various functional groups can be introduced into the chain structure of the sulfur-crosslinked olefin rubber, and the grafted functionalized olefin rubber material can be used as a new type of rubber composite material interface coupling agent.

[0025] The functionalized olefin rubber material prepared by the present invention not only has readily available raw materials and abundant types, but can also be prepared in large quantities. It also solves the problems of the existing olefin rubber modification technology, such as the need to use expensive catalysts, limited types of functional modifiers, complicated and cumbersome reaction processes, low reaction efficiency, and the generation of gel side reactions. DETAILED DESCRIPTION

[0026] The present invention will be further described below in conjunction with specific embodiments.

[0027] The invention provides a method for preparing a functionalized olefin rubber material. The method is completed in two major steps: firstly preparing cross-linked rubber powder, and then preparing the functionalized olefin rubber material by reacting the cross-linked rubber powder with a modifier.

[0028] The principle is as follows: based on the principle of dynamic covalent polymerization, the reaction between sulfur free radicals and vinyl-containing functional modifiers is utilized to release the sulfur cross-linking network structure in the cross-linked rubber powder while introducing various functional groups into the chain structure of the olefin rubber, thereby realizing efficient and large-scale preparation of various functionalized olefin rubber materials.

[0029] The present invention provides a method for preparing a functionalized olefin rubber material, comprising the following steps:

[0030] S1. Blending olefin rubber, rubber activator, rubber accelerator and sulfur in an open mixer or internal mixer to prepare a rubber compound, and vulcanizing the rubber to obtain a cross-linked olefin rubber; wherein the vulcanization treatment method is to perform high temperature molding at 140-190° C. and a pressure of 15-20 kgf according to the positive vulcanization time. wherein the positive vulcanization time at a specific temperature is directly measured by a rotorless vulcanizer.

[0031] S2, mechanically crushing the cross-linked olefin rubber prepared in step S1 in an open mixer or an internal mixer to obtain a cross-linked rubber powder;

[0032] S3, placing the cross-linked rubber powder, the modifier and the good solvent prepared in step S2 in a reaction kettle, stirring and mixing them evenly, and reacting them at 140-200° C. for 10-120 minutes. The reaction time is determined by measuring the infrared spectra and nuclear magnetic hydrogen spectra of the products obtained at different reaction times, calculating the interaction between the grafting amount and the reaction time, and finally determining the reaction time.

[0033] S4, then pouring it into a non-good solvent to wash the precipitate, and drying it to obtain a functionalized olefin rubber material.

[0034] The olefin rubber is one or a combination of butadiene rubber, styrene-butadiene rubber, natural rubber, isoprene rubber, nitrile rubber, epoxy natural rubber, butyl rubber, chloroprene rubber, and EPDM rubber. Since the present invention utilizes the free radicals generated by the cleavage of the disulfide / polysulfide bonds in the sulfur cross-linked rubber to initiate the grafting of the vinyl monomer, most olefin rubbers can be cross-linked by sulfur.

[0035] The rubber activator is zinc oxide and stearic acid; the weight ratio of the rubber activator to the olefin rubber is 3:100-7:100; the weight ratio of zinc oxide to stearic acid is 5:1-2:1.

[0036] The rubber accelerator is one or a combination of benzothiazoles, thiurams, sulfenamides, guanidines, dithiocarbamates, etc.; the weight ratio of the rubber accelerator to the olefin rubber is 0.5:100 to 6:100.

[0037] The weight ratio of sulfur to olefin rubber is 1.5:100 to 20:100.

[0038] The blending method in step S1 includes: if an open mixer is used for blending, the blending temperature is room temperature and the blending time is 5-10 minutes; if an internal mixer is used for blending, the blending temperature is 30-80° C. and the blending time is 5-10 minutes.

[0039] In step S2, if the mechanical crushing is performed by an open mill, the crushing temperature is room temperature and the crushing time is 10-30 minutes; if the mechanical crushing is performed by an internal mixer, the crushing temperature is 30-80°C and the blending time is 10-30 minutes.

[0040] The modifier is selected from one or more of the compounds of formula I, formula II and formula III, and the dosage of the modifier is 100-1000 mL: 100 g cross-linked rubber powder.

[0041]

[0042] R in the structural formulas I, II and III is selected from a hydrogen atom or a methyl group;

[0043] R1 in structural formula I is selected from a hydrogen atom, a C1-C18 alkane group, an oxygen-containing group, a nitrogen-containing group, and a silicon-containing group;

[0044] R2 in structural formula II is selected from a hydrogen atom, an oxygen-containing group, and a nitrogen-containing group;

[0045] R3, R4, and R5 in structural formula III are selected from hydrogen atoms, C1-C6 alkane groups, phenyl groups, oxygen-containing groups, and nitrogen-containing groups;

[0046] Thus the modifiers include styrene, allylbenzene, vinyltoluene, 3-methylstyrene, 2,4-dimethyl-1-alkenylbenzene, 1-methyl-4-(1-methylvinyl)benzene, 4-vinylbiphenyl, 3-vinylaniline, 4-vinylaniline, 4-vinylbenzoic acid, methyl 4-vinylbenzoate, acrylic acid, methyl acrylate, ethyl acrylate, propyl acrylate, n-butyl acrylate, isobutyl acrylate, tert-butyl acrylate, n-octyl acrylate, isooctyl acrylate, dodecyl acrylate, tetradecyl acrylate, hexadecyl acrylate, octadecyl acrylate, hydroxyethyl acrylate, hydroxypropyl acrylate, glycidyl acrylate, ethoxyethoxyethyl acrylate, 2-ethylcyanoacrylate, 2-cyclohexyl acrylate, isobornyl acrylate, acrylamide, N-hydroxymethylacrylamide, butoxymethylacrylamide, methacrylic acid, methyl methacrylate, One or a combination of ethyl methacrylate, propyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, tert-butyl methacrylate, isooctyl methacrylate, dodecyl methacrylate, hexadecyl methacrylate, octadecyl methacrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, 2-ethoxyethyl methacrylate, cyclohexyl methacrylate, isobornyl methacrylate, methacrylamide, trifluoroethyl methacrylate, glycidyl methacrylate, methacryloxypropyltrimethoxysilane, methacryloxymethyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, methylvinyldimethoxysilane, methylvinyldiethoxysilane, dimethylphenylvinylsilane, triphenylvinylsilane; the amount of the modifier is 100-1000mL: 100g cross-linked rubber powder.

[0047] The good solvent is one or a combination of acetone, butanone, cyclohexanone, tetrahydrofuran, n-hexane, cyclohexane, n-heptane, dichloromethane, chloroform, toluene and xylene; the dosage of the good solvent is 500-1400mL: 100g cross-linking rubber powder.

[0048] The non-good solvent is one or a combination of methanol, ethanol, n-propanol, isopropanol, n-butanol, ethylene glycol, methyl acetate, ethyl acetate, acetonitrile, etc.; the amount of the non-good solvent is 500-1400mL: 100g cross-linked rubber powder.

[0049] Example 1

[0050] Preparation of cross-linked rubber powder 1: Add styrene-butadiene rubber, rubber activator (zinc oxide and stearic acid), rubber accelerator N-cyclohexyl-2-benzothiazole sulfenamide (CZ) and sulfur into an open mill in sequence according to the formula in Table 1-1, mix at room temperature for 5 minutes to prepare a rubber mix, and perform high-temperature molding at 150°C and 20 kgf according to the positive vulcanization time to obtain a cross-linked olefin 1, which is then put into an open mill and crushed at room temperature for 10 minutes to obtain a cross-linked rubber powder 1;

[0051] Preparation of functionalized olefin rubber material 1: Place the prepared cross-linked rubber powder 1, acrylic acid (AC) and n-heptane in a reactor according to the ratio in Table 1-2, stir and mix evenly, and react at 170°C for 20 minutes; after the reaction, pour the reactant into ethyl acetate to wash and precipitate, to obtain a series of purified functionalized olefin rubber materials 1, corresponding to sample 11, sample 12, sample 13 and sample 14 respectively.

[0052] Preparation of comparative sample 1: Add styrene-butadiene rubber into an open mixing mill and mix at room temperature for 15 minutes to obtain comparative sample 1.

[0053] Table 1-1 Cross-linked rubber powder 1 formula

[0054] Styrene Butadiene Rubber Zinc Oxide Stearic acid Accelerator CZ sulfur Dosage(g) 100 5 1 6 20

[0055] Table 1-2 Reaction raw material ratios of samples 11-14

[0056] Sample 11 Sample 12 Sample 13 Sample 14 Cross-linked rubber powder 1(g) 100 100 100 100 AC(mL) 100 500 800 1000 n-Heptane (mL) 1400 1000 700 500

[0057] The prepared samples 11-14 and comparative sample 1 were tested by hydrogen nuclear magnetic resonance spectrum, gel permeation chromatography and differential scanning calorimetry to determine their AC grafting rate, number average molecular weight and glass transition temperature. The test results are shown in Tables 1-3.

[0058] Table 1-3 Molecular chain parameters of samples 11-14 and comparative sample 1

[0059] Sample 11 Sample 12 Sample 13 Sample 14 Comparison sample 1 AC grafting rate (%) 2.1 6.7 12.5 14.3 - Number average molecular weight (g / mol) 10800 14500 17300 21700 255400 Glass transition temperature(℃) -43.4 -38.2 -34.8 -32.5 -50.5

[0060] Comparing the comparative sample 1 and samples 11-14 in Table 1-3, it can be seen that the glass transition temperature of the samples is significantly improved compared with the comparative samples. The AC grafting rate, number average molecular weight and glass transition temperature of the samples all increase with the increase of AC addition, proving that the molecular chain parameters of functionalized olefin rubber materials can be adjusted by adjusting the raw material ratio.

[0061] Example 2 A method for preparing a functionalized olefin rubber material

[0062] (1) Preparation of cross-linked rubber powder 2: natural rubber, rubber activator (zinc oxide and stearic acid), rubber accelerator CZ and sulfur were added to an internal mixer in sequence according to the formula in Table 2-1, and mixed at 50°C for 10 min to prepare a rubber mix. The obtained rubber mix was subjected to high-temperature molding at 143°C and 15 kgf according to the positive vulcanization time to obtain cross-linked olefin 2, which was then put into an internal mixer and crushed at 50°C for 30 min to obtain cross-linked rubber powder 2;

[0063] (2) Preparation of functionalized olefin rubber material 2: 100 g of cross-linked rubber powder 2, 500 mL of hydroxyethyl acrylate (HEA) and 1000 mL of xylene were placed in a reactor and stirred to mix evenly, and reacted at 140°C for 30, 60, 90 and 120 min. After the reaction, the reactants were poured into ethanol to wash the precipitate, thereby obtaining a series of purified functionalized olefin rubber materials 2, corresponding to sample 21, sample 22, sample 23 and sample 24, respectively.

[0064] (3) Preparation of Comparative Sample 2: Natural rubber was added into an internal mixer and mixed at 50° C. for 40 min to obtain Comparative Sample 2.

[0065] Table 2-1 Cross-linked rubber powder 2 formula

[0066] Natural rubber Zinc Oxide Stearic acid Accelerator CZ sulfur Dosage(g) 100 3 1 3 10

[0067] The prepared samples 21-24 and comparative sample 2 were tested by hydrogen nuclear magnetic resonance spectrum, gel permeation chromatography and differential scanning calorimetry to determine their HEA grafting rate, number average molecular weight and glass transition temperature. The test results are shown in Table 2-2.

[0068] Table 1-2 Molecular chain parameters of samples 11-14 and comparative sample 1

[0069]

[0070]

[0071] Comparing the comparative sample 2 and samples 21-24 in Table 2-2, it can be seen that the glass transition temperature of the sample is significantly improved compared with the comparative sample. The HEA grafting rate, number average molecular weight and glass transition temperature of the sample all increase with the increase of high temperature reaction time, proving that the molecular chain parameters of the functionalized olefin rubber material can be adjusted by regulating the high temperature reaction time.

[0072] Example 3 Preparation method of a functionalized olefin rubber material

[0073] (1) Preparation of cross-linked rubber powder 3: Butadiene rubber, rubber activator (zinc oxide and stearic acid), rubber accelerator CZ and sulfur were added to an internal mixer in sequence according to the formula in Table 3-1, and mixed at room temperature for 5 minutes to prepare a rubber mix. The obtained rubber mix was subjected to high-temperature molding at 160°C and 20 kgf according to the positive vulcanization time to obtain a cross-linked olefin 3, which was then put into an open mixer and crushed at room temperature for 20 minutes to obtain a cross-linked rubber powder 3;

[0074] (2) Preparation of functionalized olefin rubber material 3: 100 g of cross-linked rubber powder 3, 500 mL of styrene (St) and 1000 mL of cyclohexane were placed in a reactor and stirred to mix evenly, and reacted at 140, 160, 180 and 200 °C for 10 min. After the reaction, the reactants were poured into methanol to wash the precipitate, thereby obtaining a series of purified functionalized olefin rubber materials 3, corresponding to sample 31, sample 32, sample 33 and sample 34, respectively.

[0075] (3) Preparation of Comparative Sample 3: Natural rubber was added into an open mixing mill and mixed at room temperature for 25 minutes to obtain Comparative Sample 3.

[0076] Table 3-1 Cross-linked rubber powder 2 formula

[0077] Butadiene rubber Zinc Oxide Stearic acid Accelerator CZ sulfur Dosage(g) 100 5 2 1.5 5

[0078] The prepared samples 31-34 and comparative sample 3 were tested by hydrogen nuclear magnetic resonance spectrum, gel permeation chromatography and differential scanning calorimetry to determine their St grafting rate, number average molecular weight and glass transition temperature. The test results are shown in Table 3-2.

[0079] Table 3-2 Molecular chain parameters of samples 31-34 and comparative sample 3

[0080]

[0081]

[0082] Comparing the comparative sample 3 and samples 31-34 in Table 3-2, it can be seen from the analysis that the glass transition temperature of the sample is significantly improved compared with the comparative sample. The St grafting rate, number average molecular weight and glass transition temperature of the sample all increase with the increase of high temperature reaction time, proving that the molecular chain parameters of the functionalized olefin rubber material can be adjusted by regulating the high temperature reaction temperature. However, the existing technologies such as copolymerization reactions are prone to violent polymerization at high temperatures; the thiol click system is prone to gel side reactions at high temperatures. Therefore, only the method of the present invention overcomes the influence of high temperature, thereby improving the reaction efficiency.

[0083] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing a functionalized olefin rubber material, It is characterized in that The following steps are involved: S1, blending olefin rubber, rubber activator, rubber accelerator and sulfur to prepare a rubber mix, and obtaining a cross-linked olefin rubber after vulcanization treatment; S2, stirring and mixing the cross-linked olefin rubber, vinyl-containing modifier and good solvent prepared in step S1, and reacting at 140-200° C. for 10-120 min; S3. Washing the precipitate in a non-good solvent and drying it to obtain a functionalized olefin rubber material.

2. The method for preparing the functionalized olefin rubber material according to claim 1, It is characterized in that The vulcanization treatment method in step S1 includes molding at 140-190° C. and 15-20 kgf pressure according to the positive vulcanization time; and crushing the cross-linked olefin rubber in step S2 into powder.

3. The method for preparing the functionalized olefin rubber material according to claim 1, It is characterized in that The olefin rubber is one or a combination of butadiene rubber, styrene-butadiene rubber, natural rubber, isoprene rubber, nitrile rubber, epoxy natural rubber, butyl rubber, chloroprene rubber, and EPDM rubber.

4. The method for preparing the functionalized olefin rubber material according to claim 1, It is characterized in that The rubber activator is a combination of zinc oxide and stearic acid in a weight ratio of 5:1 to 2:1; the weight ratio of the rubber activator to the olefin rubber is 3:100 to 7:

100.

5. The method for preparing the functionalized olefin rubber material according to claim 1, It is characterized in that The rubber accelerator is one or a combination of benzothiazoles, thiurams, sulfenamides, guanidines, and dithiocarbamates; the weight ratio of the rubber accelerator to the olefin rubber is 0.5:100 to 6:

100.

6. The method for preparing the functionalized olefin rubber material according to claim 1, It is characterized in that The weight ratio of the sulfur to the olefin rubber is 1.5:100 to 20:

100.

7. The method for preparing the functionalized olefin rubber material according to claim 1, It is characterized in that The vinyl-containing modifier is one or a combination of the compound of formula I, the compound of formula II, and the compound of formula III; the ratio of the vinyl-containing modifier is 100-1000 mL: 100 g of the cross-linked olefin rubber; Wherein, R in structural formula I, II, and III is selected from a hydrogen atom or a methyl group; R1 in structural formula I is selected from a hydrogen atom, a C1-C18 alkane group, an oxygen-containing group, a nitrogen-containing group, and a silicon-containing group; R2 in structural formula II is selected from a hydrogen atom, an oxygen-containing group, and a nitrogen-containing group; R3, R4 and R5 in the structural formula III are selected from hydrogen atoms, C1-C6 alkane groups, phenyl groups, oxygen-containing groups and nitrogen-containing groups.

8. The method for preparing the functionalized olefin rubber material according to claim 1, It is characterized in that The good solvent is one or a combination of acetone, butanone, cyclohexanone, tetrahydrofuran, n-hexane, cyclohexane, n-heptane, dichloromethane, chloroform, toluene, and xylene; the ratio of the good solvent is 500-1400 mL: 100 g of the cross-linked olefin rubber.

9. The method for preparing the functionalized olefin rubber material according to claim 1, It is characterized in that The non-good solvent is one or a combination of methanol, ethanol, n-propanol, isopropanol, n-butanol, ethylene glycol, methyl acetate, ethyl acetate, and acetonitrile; the ratio of the non-good solvent is 500-1400 mL: 100 g of the cross-linked olefin rubber.

10. The functionalized olefin rubber material prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Modified diene polymer and preparation method thereof and rubber composition and vulcanized rubber

    CN108017727A

  • Rubber composition for tires, and pneumatic tires

    CN110506075A

  • Thermally reversible crosslinking modified elastomer material and preparation method thereof

    CN110818973A

  • Multi-polymer and preparation method thereof

    CN113292667A

  • Thermoplastic elastomeric material and process for its manufacturing

    CN101023110A