A method for preparing high-purity cesium salt and high-purity rubidium salt
By using tartaric acid to react with potassium ions to generate soluble potassium tartrate, combined with recrystallization and subsequent processing, the problem of residual potassium ions in the existing technology was solved, the purity of rubidium and cesium salts was successfully improved, and high-purity rubidium and cesium salts were achieved. Cesium salt preparation.
Patent Information
- Application Number
- CN202211401445.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-09
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-11-09
AI Technical Summary
In the prior art, when rubidium and cesium are extracted from mineral raw materials, it is difficult to effectively remove potassium ions, resulting in low purity of rubidium salts and cesium salts, and the water solubility and structural similarity of potassium make their removal difficult.
Use tartaric acid as a potassium remover, add tartaric acid to the potassium-containing rubidium-cesium alum solution, control the reaction conditions and the amount of tartaric acid, and react the tartaric acid with potassium ions to generate soluble potassium tartrate. Combined with recrystallization means, the rubidium-cesium alum will crystallize. The form is precipitated, while potassium remains in the solution, and then aluminum removal, extraction and back-extraction are performed to separate high-purity rubidium salts and cesium salts.
The almost complete removal of potassium ions is achieved, and the purity of the obtained rubidium cesium alum and cesium salt is higher than 99.9% and 99.5% respectively, which significantly improves the purity and economic benefits of the product.
Smart Images

Figure CN115725855B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of alkali metal element extraction, and in particular relates to a method for preparing high-purity cesium salt and high-purity rubidium salt. Background Art
[0002] Rare and precious metals rubidium, cesium and various salts and compounds are widely used in photoelectric tubes, electric light sources, X-ray image intensifiers, conversion crystals, time and frequency standards, special glasses, special ceramics, catalysts, catalyst additives, catalyst resurrection agents, bioengineering, magnetohydrodynamic power generation, thermoelectric ion conversion power generation, ion propulsion engines, laser energy conversion to electrical energy, ion cloud long-distance special communications and other special fields due to their excellent and irreplaceable photoelectric effects and special properties.
[0003] Rubidium and cesium are active in nature, easily lose their outer electrons, and exist in the form of soluble salts in the solution. Rubidium and cesium are abundant in nature, but the content is low, and they often coexist with other alkali metals such as lithium, sodium, and potassium. In the prior art, the extraction methods of rubidium and cesium include precipitation, ion exchange, and extraction. However, alkali metals of the same main group have very similar physical and chemical properties, among which potassium interferes most seriously with rubidium and cesium, and potassium has good water solubility. Therefore, due to the considerable difficulty in separating and extracting rubidium and cesium, there are more potassium ions remaining in the obtained rubidium salts and cesium salts, resulting in low purity and quality.
[0004] Therefore, a method is needed to improve the quality of rubidium salt and cesium salt and reduce the potassium content. Summary of the invention
[0005] 1. Technical issues to be resolved
[0006] In the prior art, when rubidium and cesium are extracted from mineral raw materials, potassium ions can be supersaturated and crystallized by recrystallization, and rubidium and cesium are left in the mother liquor after filtration to achieve potassium removal. However, common potassium salts are soluble compounds, so after potassium is removed by the above-mentioned prior art, a considerable portion of potassium ions are still enriched in the mother liquor, mixed with rubidium and cesium, affecting the purity of the product rubidium salt and cesium salt. Therefore, due to the good water solubility of potassium salts and the structural similarity of potassium with rubidium and cesium, the removal of potassium in rubidium-cesium minerals is recognized as a difficult problem in the industry.
[0007] The present invention anticipates using tartaric acid as a potassium removal agent, adding tartaric acid to a rubidium-cesium alum solution containing potassium, and controlling the reaction conditions and the amount of tartaric acid, so that tartaric acid and potassium ions react to generate soluble potassium tartrate, and then cooling and recrystallizing the system in combination with a recrystallization method, so that the rubidium-cesium alum is precipitated in the form of crystals, while potassium remains in the solution as potassium tartrate, thereby obtaining rubidium-cesium alum with extremely low potassium content, and then continuing to perform aluminum removal, extraction, back extraction and other treatments on the rubidium-cesium alum to separate and obtain high-purity rubidium salt and cesium salt.
[0008] (II) Technical solution
[0009] In order to achieve the above object, the main technical solutions adopted by the present invention include:
[0010] A method for preparing high-purity cesium salt and high-purity rubidium salt comprises the following steps:
[0011] S1: dissolving the rubidium-cesium mixed raw material in deionized water to obtain a first solution;
[0012] S2: adding tartaric acid to the first solution, heating and stirring the solution while adding the tartaric acid to react, and obtaining a second solution after the reaction is completed; allowing the second solution to stand, cool and recrystallize, and then centrifuging to obtain crystals and a potassium tartrate solution;
[0013] S3: dissolving the crystals in deionized water, and then adding an aluminum removal agent to remove aluminum, thereby obtaining an aluminum removal solution and a first precipitate;
[0014] S4: extracting the aluminum removal solution with cesium to obtain a cesium-extracted organic phase and cesium-extracted residual water, and then stripping the cesium-extracted organic phase with ammonium salt or acid as a stripping agent to obtain a cesium stripping solution;
[0015] S5: extracting cesium residual water with rubidium to obtain an organic phase extracted with rubidium, and then stripping the organic phase with ammonium salt or acid as a stripping agent to obtain a rubidium stripping solution;
[0016] S6: finely filter the cesium stripping solution and the rubidium stripping solution respectively, and then sequentially evaporate and concentrate, dry, calcine, redissolve and dry again to obtain cesium salt and rubidium salt.
[0017] The rubidium-cesium mixed raw material mentioned in the present invention is a mixture of cesium alum, rubidium alum and potassium alum that has undergone simple enrichment pre-treatment, and also contains other metal ions or anion impurities, including but not limited to lithium ions, sodium ions, iron ions, calcium ions, magnesium ions, sulfate ions, etc., wherein the content of rubidium and cesium is relatively low, and specifically can be rubidium-cesium minerals that have undergone enrichment treatment, low-grade crude mixed alum, or waste containing rubidium and cesium, etc.
[0018] In the method for preparing high-purity cesium salt and high-purity rubidium salt as described above, preferably, in step S1, the first solution is obtained by mixing the rubidium-cesium mixed raw material with deionized water in a mass ratio of 1:3-1:7, and heating to 70-95°C to completely dissolve the rubidium-cesium alum. Cesium alum is a poorly soluble complex salt, and a large amount of water needs to be added to completely dissolve it at room temperature. However, too much water will cause the rubidium-cesium concentration in the first solution to be too low, which is not conducive to subsequent extraction. Therefore, the present invention preferably dissolves the rubidium-cesium alum in a small amount of water at a higher temperature to improve the extraction efficiency of rubidium and cesium.
[0019] The method for preparing high-purity cesium salt and high-purity rubidium salt as described above, preferably, in step S2, the molar ratio of the added tartaric acid to the potassium in the first solution is 0.2-0.7, the temperature for adding tartaric acid to the first solution for reaction is 50-95° C., and the reaction time of the first solution with tartaric acid is 1-3 h;
[0020] After the second solution is prepared, the second solution is allowed to stand for 12-24 hours to cool and recrystallize, thereby obtaining rubidium cesium alum crystals that contain almost no potassium and a potassium tartrate solution with a high concentration. The rubidium cesium alum crystals are subsequently dissolved and aluminum is removed, and the potassium tartrate solution can be recycled to obtain potassium salt, or potassium tartrate can be directly extracted and recycled.
[0021] In the present invention, the chemical reaction principle of tartaric acid and potassium is: C4H6O6+2K→K2C4H4O6, and the product is potassium tartrate with good solubility.
[0022] In the present invention, the amount of tartaric acid has a key impact on the removal effect of potassium. The amount of tartaric acid is too little, for example, when the molar ratio with potassium in the first solution is 0.1, the potassium tartrate generated is insufficient, and some potassium ions will be precipitated in the form of crystallization with rubidium and cesium during cooling recrystallization, thereby affecting the purity of rubidium and cesium. And when the amount of tartaric acid is too much, for example, when the molar ratio with potassium in the first solution is 2.0, tartaric acid will generate potassium hydrogen tartrate with potassium, and the solubility of potassium hydrogen tartrate is relatively small, and most of potassium hydrogen tartrate will directly precipitate in the form of precipitation, but potassium hydrogen tartrate still has certain solubility, so even if potassium is precipitated in the form of potassium hydrogen tartrate, there will still be some residues in the mother liquor, affecting the purity of rubidium and cesium, and in this case, if cooling recrystallization is adopted, potassium and rubidium and cesium cannot be completely separated.
[0023] When tartaric acid is added in excess, only one carboxyl group in the tartaric acid reacts with potassium to generate potassium hydrogen tartrate. In the present invention, a small amount of tartaric acid is added, the potassium content in the solution is excessive, and both carboxyl groups in the tartaric acid participate in the reaction, generating potassium tartrate with potassium.
[0024] The reaction temperature of adding tartaric acid to the first solution for reaction has an important influence on the reaction rate. Firstly, the temperature can make the tartaric acid dissolve quickly. Secondly, the temperature range can make the tartaric acid and potassium ions react quickly and completely, thereby improving production efficiency.
[0025] In the present invention, the purpose of standing is to make the rubidium-cesium alum precipitate as completely as possible. When the standing time is too short, the concentration of rubidium and cesium remaining in the mother liquor is high, which leads to insufficient yield of rubidium and cesium.
[0026] In the method for preparing high-purity cesium salt and high-purity rubidium salt as described above, preferably, in step S3, after the crystals are dissolved in deionized water, a barium hydroxide solution or a calcium hydroxide solution is added as an aluminum removal agent to remove aluminum, and then the obtained mixture is centrifuged and finely filtered to obtain an aluminum removal solution and a first precipitate.
[0027] In the method for preparing high-purity cesium salt and high-purity rubidium salt as described above, preferably, before performing step S4, calcium hydroxide or barium hydroxide solution is added to the dealuminization solution to adjust the pH of the system to alkaline, and then fine filtration is performed to obtain a causticized dealuminization solution and a precipitated residue.
[0028] In step S4, cesium is extracted from the causticized aluminum removal solution to obtain a cesium extracted organic phase and cesium extracted residual water, and the cesium extracted residual water is used to prepare a rubidium extracted stock solution.
[0029] In the method for preparing high-purity cesium salt and high-purity rubidium salt as described above, preferably, in step S4 and step S5, the extractant is a mixture of t-BAMBP, diethylbenzene and kerosene.
[0030] In the method for preparing high-purity cesium salt and high-purity rubidium salt as described above, preferably, in step S4, before stripping, the cesium-extracted organic phase is washed with ammonia water as a washing agent to obtain a washing liquid and a washed cesium-extracted organic phase, and the obtained washing liquid is recycled;
[0031] Then, the washed cesium-extracted organic phase is stripped with ammonium salt or acid as a stripping agent to obtain a cesium stripping solution and a lean organic phase.
[0032] In the present invention, the role of ammonia water is to remove rubidium in the cesium extraction organic phase. Ammonia water can just wash away rubidium without washing away all cesium. Other detergents will wash away both rubidium and cesium at the same time.
[0033] The method for preparing high-purity cesium salt and high-purity rubidium salt as described above, preferably, before performing step S5, calcium hydroxide or barium hydroxide solution is added to the cesium extraction residual water, the pH of the system is adjusted to alkaline, and the obtained mixture is filtered and separated to obtain a causticized rubidium extraction stock solution and a precipitate residue. If calcium hydroxide is added, the precipitate residue is calcium slag, and if barium hydroxide is added, the precipitate residue is barium slag. Since strong bases of the same family as rubidium will introduce impurities such as sodium or potassium, it is extremely difficult to separate from rubidium. Therefore, the present invention also uses barium hydroxide or calcium hydroxide solution to causticize the cesium extraction residual water, and then separates and removes it through a precision filtration method such as a microporous filter membrane to obtain a causticized rubidium extraction stock solution.
[0034] In step S5, rubidium is extracted from the causticized rubidium extraction stock solution to obtain a rubidium extraction organic phase and rubidium extraction residual water. The rubidium extraction organic phase is stripped using ammonium salt or acid as a stripping agent to obtain a rubidium stripping solution and a lean organic phase.
[0035] In the method for preparing high-purity cesium salt and high-purity rubidium salt as described above, preferably, in step S4 and step S5, the ammonium salt is ammonium carbonate, and the acid is hydrochloric acid, sulfuric acid, nitric acid, oxalic acid or formic acid. By using the above various acids as stripping agents, cesium chloride and rubidium chloride, cesium sulfate and rubidium sulfate, rubidium nitrate and cesium nitrate, cesium oxalate and rubidium oxalate, and cesium formate and rubidium formate can be obtained respectively.
[0036] Described stripping agent is preferably ammonium carbonate.From price and technology, the preparation of rubidium carbonate cesium carbonate product is more difficult, and product price is higher, and the present invention has prepared high-purity rubidium carbonate and cesium carbonate by selecting ammonium carbonate as stripping agent, and higher economic benefit can be obtained.In addition, rubidium carbonate and cesium carbonate can also be converted into other types of rubidium salts and cesium salts in use, such as cesium chloride and rubidium chloride, cesium oxalate and rubidium oxalate, and cesium formate and rubidium formate, etc., and application range is more extensive, while cesium chloride and rubidium chloride, cesium sulfate and rubidium sulfate, rubidium nitrate and cesium nitrate, cesium oxalate and rubidium oxalate, and cesium formate and rubidium formate, etc. are not easily converted into other types of rubidium salts and cesium salts.
[0037] (III) Beneficial effects
[0038] The beneficial effects of the present invention are:
[0039] The present invention adopts tartaric acid as a potassium removal agent, adds tartaric acid to a rubidium cesium alum solution containing potassium, reacts tartaric acid with potassium ions to generate soluble potassium tartrate, and then cools and recrystallizes the system, so that the rubidium cesium alum is precipitated in the form of crystals, and potassium remains in the solution as potassium tartrate, thereby obtaining rubidium cesium alum with extremely low potassium content. After tartaric acid is used to remove potassium, the obtained rubidium cesium alum is relatively pure, and the residual potassium content is less than 0.0035% of the rubidium cesium alum crystal mass, and almost complete removal of potassium is achieved. The potassium content in the obtained potassium tartrate solution is high, and potassium salt can be obtained by means such as evaporation and crystallization, and potassium ions are recycled.
[0040] In addition, after removing potassium from rubidium-cesium alum, the present invention also performs aluminum removal, extraction and back extraction on the rubidium-cesium alum to separate and obtain rubidium salt with a purity higher than 99.9% and cesium salt with a purity higher than 99.5%, and the product purity is relatively high. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 The present invention provides a process flow chart for preparing high-purity cesium salt and high-purity rubidium salt. DETAILED DESCRIPTION
[0042] In order to better explain the present invention and facilitate understanding, the present invention is described in detail below through specific implementation modes in conjunction with the accompanying drawings.
[0043] Example 1
[0044] This embodiment provides a method for preparing high-purity cesium salt and high-purity rubidium salt, comprising the following steps:
[0045] S1: Add 200 g of the rubidium-cesium mixed raw material to deionized water so that the mass ratio of rubidium-cesium alum to deionized water is 1:3, heat to 70° C., and stir continuously during the heating process to completely dissolve the rubidium-cesium alum to obtain a first solution.
[0046] S2: Add tartaric acid to the first solution, control the molar ratio of the added tartaric acid to the potassium in the first solution to 0.3, heat to 55°C, and stir continuously during the heating process to dissolve the tartaric acid, and react for 2 hours to prepare a second solution, then let the second solution stand for 18 hours, cool it to room temperature and recrystallize, and centrifuge to obtain rubidium cesium alum crystals and potassium tartrate solution.
[0047] S3: Dissolve the rubidium cesium alum crystals in deionized water, then slowly add 1 mol / L barium hydroxide solution, and when the pH reaches 7.2, the reaction ends, and continue stirring for 0.5 hours to generate aluminum hydroxide and barium sulfate. Centrifuge the generated mixture, and filter the obtained clear liquid with a microporous filter membrane to obtain an aluminum removal solution and a barium slag precipitate.
[0048] S4: Add 1 mol / L barium hydroxide solution to the dealuminization solution, adjust the pH of the dealuminization solution to 13.5, and then filter it with a microporous filter membrane to obtain a causticized dealuminization solution and barium slag. Use a mixed solvent of t-BAMBP, diethylbenzene and kerosene as an extractant to extract cesium from the causticized dealuminization solution to obtain a cesium extracted organic phase and cesium extracted residual water. Use ammonia water as a detergent to wash the cesium extracted organic phase to obtain a washing liquid and a washed cesium extracted organic phase. Then use ammonium carbonate as a stripping agent to strip the washed cesium extracted organic phase to obtain a cesium stripping liquid and a lean organic phase.
[0049] S5: Add 1 mol / L barium hydroxide solution to the cesium extraction residual water, adjust the pH of the cesium extraction residual water to 13.5, and then filter and separate the obtained mixture to obtain causticized rubidium extraction stock solution and barium slag. Use a mixed solvent of t-BAMBP, diethylbenzene and kerosene as an extractant to extract rubidium from the causticized rubidium extraction stock solution to obtain a rubidium extraction organic phase and rubidium extraction residual water, and then use ammonium carbonate as a stripping agent to strip the rubidium extraction organic phase to obtain a rubidium stripping solution and a lean organic phase.
[0050] S6: finely filter the cesium stripping solution and the rubidium stripping solution respectively, and then sequentially evaporate and concentrate, dry, calcine, redissolve and dry again to obtain cesium carbonate and barium carbonate.
[0051] Example 2
[0052] This embodiment provides a method for preparing high-purity cesium salt and high-purity rubidium salt. The difference from Embodiment 1 is that in step S2, the molar ratio of the added tartaric acid to the potassium in the first solution is controlled to be 0.2.
[0053] Example 3
[0054] This embodiment provides a method for preparing high-purity cesium salt and high-purity rubidium salt. The difference from Embodiment 1 is that in step S2, the molar ratio of the added tartaric acid to the potassium in the first solution is controlled to be 0.55.
[0055] Example 4
[0056] This embodiment provides a method for preparing high-purity cesium salt and high-purity rubidium salt, which is different from Embodiment 1 in that in step S2, the heating temperature is 50°C.
[0057] Example 5
[0058] This embodiment provides a method for preparing high-purity cesium salt and high-purity rubidium salt, which is different from Embodiment 1 in that in step S2, the heating temperature is 90°C.
[0059] Example 6
[0060] This embodiment provides a method for preparing high-purity cesium salt and high-purity rubidium salt, which is different from Embodiment 1 in that, in step S2, the second solution is allowed to stand for 12 hours.
[0061] Example 7
[0062] This embodiment provides a method for preparing high-purity cesium salt and high-purity rubidium salt, which is different from Embodiment 1 in that, in step S2, the second solution is allowed to stand for 24 hours.
[0063] Example 8
[0064] This embodiment provides a method for preparing high-purity cesium salt and high-purity rubidium salt, which is different from Embodiment 1 in that, in step S1, the mass ratio of rubidium cesium alum to deionized water is 1:7.
[0065] Example 9
[0066] This embodiment provides a method for preparing high-purity cesium salt and high-purity rubidium salt, which is different from Embodiment 1 in that in step S1, heating is performed to 95°C.
[0067] Example 10
[0068] This embodiment provides a method for preparing high-purity cesium salt and high-purity rubidium salt. The difference from Embodiment 1 is that in step S4 and step S5, the stripping agent used is nitric acid, and the obtained products are rubidium nitrate and cesium nitrate.
[0069] Embodiment 11
[0070] This embodiment provides a method for preparing high-purity cesium salt and high-purity rubidium salt. The difference from Embodiment 1 is that in step S4 and step S5, the stripping agent used is hydrochloric acid, and the obtained products are rubidium chloride and cesium chloride.
[0071] Comparative Example 1
[0072] The difference between this comparative example and Example 1 is that the amount of tartaric acid added in step S2 is 0. Since tartaric acid is not added in this comparative example, potassium salt solution and rubidium-cesium alum crystals are obtained after cooling and recrystallization.
[0073] Comparative Example 2
[0074] The difference between this comparative example and Example 1 is that in step S2, the molar ratio of the added tartaric acid to the potassium in the first solution is 2.0. In this comparative example, after the reaction of tartaric acid and potassium ions is completed and the solution is allowed to stand, potassium hydrogen tartrate precipitate and mother liquor are obtained.
[0075] Comparative Example 3
[0076] The difference between this comparative example and Example 1 is that in step S2, the molar ratio of the added tartaric acid to the potassium in the first solution is 0.05.
[0077] Comparative Example 4
[0078] The difference between this comparative example and Example 1 is that in step S2, the heating temperature is 30°C.
[0079] Comparative Example 5
[0080] The difference between this comparative example and Example 1 is that in step S2, the heating temperature is 45°C.
[0081] Comparative Example 6
[0082] The difference between this comparative example and Example 1 is that in step S2, the standing time of the second solution is 8 hours.
[0083] The potassium ion content in the solution obtained by dissolving the rubidium cesium alum crystals obtained in the above Examples 1-11, Comparative Example 1, and Comparative Examples 3-6 in water was detected, and the potassium ion content in the rubidium cesium alum mother liquor obtained in Comparative Example 2 was detected. The test results are shown in Table 1.
[0084] Table 1 Residual potassium ion content in each embodiment and comparative example (unit: mass percentage)
[0085] Example 1 0.0027% Example 2 0.0032% Example 3 0.0029% Example 4 0.0029% Example 5 0.0031% Example 6 0.0034% Example 7 0.0027% Example 8 0.0030% Example 9 0.0035% Example 10 0.0032% Embodiment 11 0.0035% Comparative Example 1 3.02% Comparative Example 2 0.0470% Comparative Example 3 0.0097% Comparative Example 4 0.0178% Comparative Example 5 0.0225% Comparative Example 6 0.0420%
[0086] The purity of the cesium carbonate and rubidium carbonate, or other types of cesium salts and rubidium salts obtained in the above Examples 1-11 and Comparative Examples 1-6 was tested. The test results are shown in Table 2.
[0087] Table 2 Comparison of the purity of cesium salt and rubidium salt obtained in each embodiment and comparative example (unit: mass percentage)
[0088] Cesium carbonate Rubidium carbonate Example 1 99.5% 99.9% Example 2 99.5% 99.9% Example 3 99.5% 99.9% Example 4 99.5% 99.8% Example 5 99.5% 99.9% Example 6 99.5% 99.8% Example 7 99.5% 99.9% Example 8 99.5% 99.9% Example 9 99.5% 99.9% Example 10 99.5% 99.9% Embodiment 11 99.5% 99.9% Comparative Example 1 90.3% 90.1% Comparative Example 2 92.9% 96.8% Comparative Example 3 95.2% 95.4% Comparative Example 4 93.7% 94.2% Comparative Example 5 94.1% 94.9% Comparative Example 6 99.4% 93.5%
[0089] With reference to the industry standard YS / T 789-2012 for rubidium carbonate and the industry standard YS / T 756-2011 for cesium carbonate, the contents (mass percentage) of various components and elements in the cesium carbonate and rubidium carbonate products of Example 1 were tested. The specific results are shown in Tables 3 and 4.
[0090] Table 3 Comparison of the contents of various components and elements in rubidium carbonate in Example 1 and industry standards
[0091]
[0092] Table 4 Comparison of the contents of components and elements in cesium carbonate in Example 1 and industry standards
[0093]
[0094] The above is only a preferred embodiment of the present invention, and does not limit the present invention in other forms. Any person skilled in the art can use the above disclosed technical content to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the technical solution of the present invention still belongs to the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing high-purity cesium salt and high-purity rubidium salt, characterized in that: The steps include: S1: dissolving a rubidium-cesium mixed raw material in deionized water to obtain a first solution; the rubidium-cesium mixed raw material is a mixture of cesium alum, rubidium alum and potassium alum, and contains sulfate ions; S2: Add tartaric acid to the first solution, heat and stir to react while adding the tartaric acid, and obtain a second solution after the reaction is completed; let the second solution stand, cool and recrystallize, and then centrifuge to obtain crystals and potassium tartrate solution; in this step, the molar ratio of the added tartaric acid to the potassium in the first solution is 0.2-0.7, and the temperature for adding tartaric acid to the first solution for reaction is 50-95°C; the reaction time of the first solution with tartaric acid is 1-3h; after the second solution is prepared, let the second solution stand for 12-24h, cool and recrystallize, and obtain rubidium cesium alum crystals; S3: dissolving the crystals in deionized water, and then adding an aluminum removal agent to remove aluminum, to obtain an aluminum removal solution and a first precipitate; in this step, after dissolving the crystals in deionized water, a barium hydroxide solution or a calcium hydroxide solution is added as an aluminum removal agent to remove aluminum, and then the obtained mixture is centrifuged and finely filtered to obtain an aluminum removal solution and a first precipitate; S4: extracting the aluminum removal solution with cesium to obtain a cesium-extracted organic phase and cesium-extracted residual water, and then stripping the cesium-extracted organic phase with ammonium salt or acid as a stripping agent to obtain a cesium stripping solution; S5: extracting cesium residual water with rubidium to obtain an organic phase extracted with rubidium, and then stripping the organic phase with ammonium salt or acid as a stripping agent to obtain a rubidium stripping solution; S6: finely filtering the cesium stripping solution and the rubidium stripping solution respectively, and then sequentially performing evaporation concentration, drying, calcination, re-dissolving and re-drying to obtain cesium salt and rubidium salt; In step S4 and step S5, the ammonium salt is ammonium carbonate, and the acid is hydrochloric acid, sulfuric acid, nitric acid, oxalic acid or formic acid.
2. The method for preparing high-purity cesium salt and high-purity rubidium salt according to claim 1, characterized in that: In step S1, the first solution is obtained by mixing the rubidium-cesium mixed raw material and deionized water in a mass ratio of 1:3-1:7, and heating to 70-95° C. to completely dissolve the rubidium-cesium alum.
3. The method for preparing high-purity cesium salt and high-purity rubidium salt according to claim 1, characterized in that: Before performing step S4, calcium hydroxide or barium hydroxide solution is added to the aluminum removal solution to adjust the pH of the system to alkaline, and then the system is finely filtered to obtain a caustic aluminum removal solution and a precipitated slag; In step S4, cesium extraction is performed on the causticized aluminum removal solution.
4. The method for preparing high-purity cesium salt and high-purity rubidium salt according to claim 1, characterized in that: In step S4 and step S5, the extractant is a mixture of t-BAMBP, diethylbenzene and kerosene.
5. The method for preparing high-purity cesium salt and high-purity rubidium salt according to claim 1, characterized in that: In step S4, before stripping, the cesium-extracted organic phase is washed with ammonia water as a washing agent to obtain a washing liquid and a washed cesium-extracted organic phase; Then, the washed cesium-extracted organic phase is stripped with ammonium salt as stripping agent to obtain cesium stripping solution.
6. The method for preparing high-purity cesium salt and high-purity rubidium salt according to claim 1, characterized in that: Before performing step S5, calcium hydroxide or barium hydroxide solution is added to the cesium extraction residual water to adjust the pH of the system to alkaline, and the obtained mixture is filtered and separated to obtain a causticized rubidium extraction stock solution and a precipitated residue; In step S5, rubidium is extracted from the causticized rubidium extraction stock solution.