A composite negative electrode material and preparation method thereof and lithium ion battery

By synchronously generating transition metal sulfide and carbon nanotubes during low-temperature polymerization of conductive monomers, the problem of poor dispersion of transition metal sulfide is solved, and the electrochemical performance and cycle stability of the negative electrode material of lithium-ion battery are improved. , simplifies the preparation process.

CN115732653BActive Publication Date: 2024-12-06SICHUAN BAISHIGE NEW ENERGY CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211129760.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-16
Publication Date
2024-12-06
Estimated Expiration
2042-09-16

AI Technical Summary

Technical Problem

The dispersion of transition metal sulfides in existing transition metal sulfide-carbon composite materials is poor, affecting the electrochemical performance.

Method used

The soft template method is used to synchronize transition metal sulfide and carbon nanotubes during the low-temperature polymerization of conductive monomers. The transition metal sulfide-carbon nanotube composite material is prepared by high-temperature calcination to ensure that the transition metal sulfide is raw in the preparation process of carbon nanotubes. bit generation to improve dispersion.

Benefits of technology

The electrochemical performance and cycle stability of the composite material are improved, the preparation process is simplified, the preparation difficulty is reduced, and the aggregation and volume expansion of transition metal sulfide particles are avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115732653B_ABST
    Figure CN115732653B_ABST
Patent Text Reader

Abstract

The present invention provides a composite negative electrode material and a preparation method thereof and a lithium ion battery, and relates to the technical field of lithium ion batteries. The preparation method comprises the following steps: mixing a soft template agent with an acidic solution, stirring at 0°C to obtain a soft template solution; S2: adding a transition metal salt and a conductive monomer to the soft template solution to obtain a pre-reaction mixed solution; S3: dropping an ammonium persulfate solution into the pre-reaction mixed solution, polymerizing at 0°C to obtain a composite material precursor; S4: calcining the composite material precursor under an inert atmosphere at 800-1000°C, washing, and drying to obtain a composite negative electrode material. The preparation method of the composite negative electrode material provided by the present invention adopts a soft template method, and in the low-temperature polymerization process of the conductive monomer, a transition metal salt is used to simultaneously prepare a transition metal sulfide, and after high-temperature calcination, the transition metal sulfide in the obtained composite material has good dispersibility, which helps to improve the electrochemical performance of the composite material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a composite negative electrode material and a preparation method thereof, and a lithium ion battery. Background Art

[0002] Transition metal sulfides have been proven to have high theoretical capacity and good mechanical properties, and are highly promising negative electrode materials for lithium-ion batteries. However, transition metal sulfides have poor electrical conductivity and are prone to collapse of the electrode structure due to their large volume expansion during the charge and discharge process. Direct use as negative electrode materials for lithium-ion batteries will lead to rapid decay of battery capacity and reduced cycle stability.

[0003] Currently, transition metal sulfide-carbon composite materials are usually prepared by compounding transition metal sulfide with carbon material to inhibit the aggregation and volume expansion of transition metal sulfide particles, thereby improving the electrochemical stability while also increasing the conductivity of the material.

[0004] In the existing preparation process of transition metal sulfide-carbon composite materials, such as the invention patent with publication number CN107978745A, it is usually necessary to prepare the transition metal sulfide and the carbon material separately, and then mix the two for compounding; the composite material obtained by this preparation method is prone to the problem of poor dispersion of transition metal sulfide, which affects the electrochemical performance of the composite material. Summary of the invention

[0005] The technical problem to be solved by the present invention is: in order to solve the problem of poor dispersibility of transition metal sulfides in transition metal sulfide-carbon composite materials in the prior art, the present invention provides a method for preparing a composite negative electrode material. The preparation method generates transition metal sulfides and carbon nanotubes in situ at the same time, has a simple preparation process, and at the same time, the transition metal sulfide has good dispersibility, thereby solving the problem of poor dispersibility of transition metal sulfides in the prior art.

[0006] The technical solution adopted by the present invention to solve its technical problem is:

[0007] A method for preparing a composite negative electrode material comprises the following steps:

[0008] S1: Mix the soft template agent with the acidic solution and stir at 0°C to obtain a soft template solution;

[0009] S2: adding a transition metal salt and a conductive monomer to the soft template solution to obtain a pre-reaction mixed solution;

[0010] S3: adding ammonium persulfate dropwise to the pre-reaction mixture to carry out polymerization reaction at 0° C. to obtain a composite material precursor;

[0011] S4: calcining the composite material precursor in an inert atmosphere at 800-1000° C., washing, and drying to obtain a composite negative electrode material.

[0012] Optionally, the soft template is methyl orange; and the acidic solution is hydrochloric acid solution.

[0013] Optionally, the transition metal salt is selected from at least one of cobalt salts, nickel salts, zinc salts, manganese salts, iron salts and tin salts.

[0014] Optionally, the transition metal salt is selected from at least one of transition metal nitrates and transition metal sulfates.

[0015] Optionally, the conductive monomer is selected from at least one of an aniline monomer and a pyrrole monomer.

[0016] Optionally, the molar ratio of the soft template to the conductive monomer is 1:(5-15).

[0017] Optionally, the mass ratio of the transition metal salt to the conductive monomer is (140-200):41.

[0018] Optionally, the molar ratio of the ammonium persulfate to the conductive monomer is 1:1.

[0019] Another object of the present invention is to provide a composite negative electrode material, which is prepared by the method for preparing the composite negative electrode material as described above.

[0020] Another object of the present invention is to provide a lithium-ion battery comprising the composite negative electrode material as described above.

[0021] The beneficial effects of the present invention are:

[0022] The preparation method of the composite negative electrode material provided by the present invention adopts a soft template method, and during the low-temperature polymerization process of a conductive monomer, a transition metal sulfide is simultaneously prepared by a transition metal salt, and then after high-temperature calcination, a transition metal sulfide-carbon nanotube composite material can be obtained; since the transition metal sulfide is generated in situ during the preparation process of the carbon nanotubes, the transition metal sulfide in the obtained composite material has good dispersibility, which helps to improve the electrochemical performance of the composite material. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] The present invention is further described below in conjunction with the accompanying drawings and embodiments.

[0024] Figure 1 is a TEM photograph of the composite negative electrode material prepared in Example 1 of the present invention;

[0025] Figure 2 is the XPS spectrum of the composite negative electrode material prepared in Example 1 of the present invention;

[0026] Figure 3 This is the cycle performance curve of the composite negative electrode material prepared in Example 1 of the present invention at a current density of 0.3 A / g. DETAILED DESCRIPTION

[0027] The present invention is now further described in detail. The embodiments described below are exemplary and intended to be used to explain the present invention, but cannot be understood as limiting the present invention. All other embodiments obtained by ordinary technicians in this field without creative work based on the embodiments of the present invention belong to the scope of protection of the present invention.

[0028] In order to solve the problem of poor dispersibility of transition metal sulfides in the prior art, the present invention provides a method for preparing a composite negative electrode material, which comprises the following steps:

[0029] The preparation method of the composite negative electrode material provided by the present invention adopts a soft template method, and during the low-temperature polymerization process of a conductive monomer, a transition metal sulfide is simultaneously prepared by a transition metal salt, and then after high-temperature calcination, a transition metal sulfide-carbon nanotube composite material can be obtained; since the transition metal sulfide is generated in situ during the preparation process of the carbon nanotubes, the transition metal sulfide in the obtained composite material has good dispersibility, which helps to improve the electrochemical performance of the composite material.

[0030] The preparation method of the composite negative electrode material provided by the present invention comprises the following steps: the ammonium persulfate added during the in-situ polymerization process serves as an initiator for the in-situ polymerization reaction on the one hand, and as a sulfur source for transition metal sulfides on the other hand, and simultaneously serves as a sulfur source, so that the obtained carbon nanotubes are S-doped carbon nanotubes, thereby further improving the electrochemical performance of the composite negative electrode material.

[0031] In addition, since the preparation method of the composite negative electrode material provided by the present invention does not require the separate preparation of transition metal sulfides and carbon nanotubes, while improving the electrochemical performance of the composite negative electrode material, it also helps to reduce the preparation steps, simplify the preparation process, and reduce the difficulty of preparation.

[0032] In the present invention, the soft template agent in step S1 is preferably methyl orange; the acidic solution is a hydrochloric acid solution, and further preferably the concentration of the hydrochloric acid solution is 0.05 mol / L, and the stirring time in step S1 is half an hour.

[0033] The purpose of adding hydrochloric acid is to increase the solubility of monomers (such as aniline and pyrrole) in the solution; methyl orange is used as a soft template, which will self-assemble into supramolecular aggregates in the solution and act as a template. The monomers are polymerized on its surface. When the polymerization is completed, the methyl orange template is removed to obtain a tubular structure, and then carbon nanotubes can be obtained.

[0034] The transition metal sulfide in the present invention can be at least one of cobalt sulfide, nickel sulfide, zinc sulfide, manganese sulfide, iron sulfide, and tin sulfide. Therefore, the present invention preferably selects the transition metal salt from at least one of cobalt salts, nickel salts, zinc salts, manganese salts, iron salts, and tin salts; and further preferably selects the transition metal salt from at least one of transition metal nitrates and transition metal sulfates; specifically, the present invention preferably selects the transition metal salt to be Co(NO3)2·6H2O.

[0035] In order to improve the electrochemical performance of the composite negative electrode material, the conductive monomer in the preferred step S2 of the present invention is selected from at least one of aniline monomer and pyrrole monomer, so that the carbon nanotubes obtained after calcination are N, S doped carbon nanotubes. The composite negative electrode material obtained by the present invention is a transition metal sulfide-N, S doped carbon nanotube composite material, so as to further improve the electrochemical performance of the composite negative electrode material.

[0036] In order to ensure that the reactants react fully, the reaction time of the polymerization reaction in step S3 of the present invention is preferably 24 hours.

[0037] The preferred inert atmosphere in step S4 of the present invention is a nitrogen atmosphere, and the preferred calcination time in step S4 is 3 hours. After calcination, the unstable substances are removed by pickling. The specific pickling process is to use 0.5 mol / L H2SO4 solution to pickle at 80°C for 8 hours to remove the unstable substances, and then wash with deionized water.

[0038] In order to take into account both the electrochemical performance and reaction efficiency of the composite negative electrode material, the present invention preferably has a molar ratio of the soft template to the conductive monomer of 1: (5-15); preferably has a mass ratio of the transition metal salt to the conductive monomer of (140-200): 41; and preferably has a molar ratio of ammonium persulfate to the conductive monomer of 1: 1.

[0039] Another object of the present invention is to provide a composite negative electrode material, which is prepared by the method for preparing the composite negative electrode material as described above.

[0040] The composite negative electrode material provided by the present invention is a transition metal sulfide-N, S doped carbon nanotube composite material. The composite negative electrode material is composited with transition metal sulfide and N, S doped carbon nanotubes, and while ensuring the capacity of the negative electrode material, the aggregation and volume expansion of transition metal sulfide particles are suppressed, thereby improving the conductivity and cycle stability of the composite negative electrode material. In addition, since the present invention simultaneously prepares transition metal sulfide through transition metal salt during the low-temperature polymerization of conductive monomers, and then obtains the transition metal sulfide-N, S doped carbon nanotube composite material after high-temperature calcination, the transition metal sulfide is in-situ generated during the preparation of N, S doped carbon nanotubes, and the transition metal sulfide in the obtained composite material has good dispersibility, which helps to further improve the electrochemical performance and cycle stability of the composite material.

[0041] Another object of the present invention is to provide a lithium ion battery, which comprises the composite negative electrode material as described above.

[0042] The lithium ion battery provided by the present invention uses a transition metal sulfide-N, S doped carbon nanotube composite material as a negative electrode material, which improves the electrochemical performance and cycle stability of the lithium ion battery while ensuring a relatively high capacity.

[0043] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.

[0044] The electrochemical properties of the materials in the embodiments of the present invention and the comparative examples were tested according to the following method: the materials prepared in the embodiments and the comparative examples were used as the negative electrode active material, and were evenly mixed with polyvinylidene fluoride (PVDF) (dissolved in N-methylpyrrolidone) and conductive carbon black in a mass ratio of 90:5:5, coated into an electrode film, and dried in a vacuum drying oven at 120°C for 12 hours. After rolling and punching, a hard carbon negative electrode sheet was obtained; a metal lithium sheet was used as the counter electrode, 1 mol / L NaPF6 (EC-DEC=1:1) was used as the electrolyte, and the hard carbon negative electrode sheets obtained above were assembled into 2430 button batteries in a glove box to test their electrochemical properties.

[0045] Example 1

[0046] This embodiment provides a method for preparing a composite negative electrode material, comprising the following steps:

[0047] S1: Add 1 mmol of methyl orange into a three-necked flask filled with 80 mL of 0.05 mol / L hydrochloric acid solution, stir at 0°C for half an hour to obtain a soft template solution;

[0048] S2: 3.32 g Co(NO3)2·6H2O and 0.82 g aniline were added to the soft template solution to obtain a pre-reaction mixture;

[0049] S3: adding ammonium persulfate dropwise to the pre-reaction mixture at a uniform rate, wherein the molar ratio of ammonium persulfate to aniline is 1:1, and polymerizing the mixture at 0° C. for 24 hours to obtain a composite material precursor;

[0050] S4: After the composite material precursor is rotary evaporated at 50-70°C, the resulting product is calcined under nitrogen conditions at a calcination temperature of 900°C for 3 hours. Finally, it is pickled with 0.5 mol / L H2SO4 solution at 80°C for 8 hours to remove unstable substances, and then washed with deionized water and dried to obtain a Co9S8 / N,S doped CNTs composite, i.e., a composite negative electrode material.

[0051] The composite negative electrode material prepared in this example was tested, see Figure 1 , Figure 2 As shown, the composite material prepared in this embodiment is a transition metal sulfide-N, S doped carbon nanotube composite material.

[0052] The composite negative electrode material was used as a negative electrode material for a lithium-ion battery for performance testing; after testing, see Figure 3 As shown, the composite negative electrode material has a reversible specific capacity of 775 mAh / g at a current density of 0.1 A / g, and still has a reversible capacity of 682 mAh / g after 100 cycles at a current density of 0.3 A / g, showing excellent cycle stability.

[0053] Example 2

[0054] This embodiment provides a method for preparing a composite negative electrode material, comprising the following steps:

[0055] S1: Add 1 mmol of methyl orange into a three-necked flask filled with 80 mL of 0.05 mol / L hydrochloric acid solution, stir at 0°C for half an hour to obtain a soft template solution;

[0056] S2: 2.8 g Co(NO3)2·6H2O and 0.82 g aniline were added to the soft template solution to obtain a pre-reaction mixture;

[0057] S3: adding ammonium persulfate dropwise to the pre-reaction mixture at a uniform rate, wherein the molar ratio of ammonium persulfate to aniline is 1:1, and polymerizing the mixture at 0° C. for 24 hours to obtain a composite material precursor;

[0058] S4: After the composite material precursor is rotary evaporated at 50-70°C, the resulting product is calcined under nitrogen conditions at a calcination temperature of 800°C for 3 hours. Finally, it is pickled with 0.5 mol / L H2SO4 solution at 80°C for 8 hours to remove unstable substances, and then washed with deionized water and dried to obtain a Co9S8 / N,S doped CNTs composite, i.e., a composite negative electrode material.

[0059] The performance of the composite negative electrode material was tested as a negative electrode material for a lithium-ion battery. After testing, the composite negative electrode material had a reversible specific capacity of 810 mAh / g at a current density of 0.1 A / g, and still had a reversible capacity of 725 mAh / g after 100 cycles at a current density of 0.3 A / g, showing excellent cycle stability.

[0060] Example 3

[0061] This embodiment provides a method for preparing a composite negative electrode material, comprising the following steps:

[0062] S1: Add 1 mmol of methyl orange into a three-necked flask filled with 80 mL of 0.05 mol / L hydrochloric acid solution, stir at 0°C for half an hour to obtain a soft template solution;

[0063] S2: 4 g Co(NO3)2·6H2O and 0.82 g aniline were added to the soft template solution to obtain a pre-reaction mixture;

[0064] S3: adding ammonium persulfate dropwise to the pre-reaction mixture at a uniform rate, wherein the molar ratio of ammonium persulfate to aniline is 1:1, and polymerizing the mixture at 0° C. for 24 hours to obtain a composite material precursor;

[0065] S4: After the composite material precursor is rotary evaporated at 50-70°C, the resulting product is calcined under nitrogen conditions at a calcination temperature of 1000°C for 3 hours. Finally, it is pickled with 0.5 mol / L H2SO4 solution at 80°C for 8 hours to remove unstable substances, and then washed with deionized water and dried to obtain a Co9S8 / N,S doped CNTs composite, i.e., a composite negative electrode material.

[0066] The performance of the composite negative electrode material was tested as a negative electrode material for a lithium-ion battery. After testing, the composite negative electrode material had a reversible specific capacity of 657 mAh / g at a current density of 0.1 A / g, and still had a reversible capacity of 578 mAh / g after 100 cycles at a current density of 0.3 A / g, showing excellent cycle stability.

[0067] Example 4

[0068] The difference between this embodiment and embodiment 1 is that the conductive monomer in step S2 is pyrrole.

[0069] The composite negative electrode material prepared in this embodiment was used as a negative electrode material for a lithium ion battery for performance testing; after testing, the composite negative electrode material had a reversible specific capacity of 780 mAh / g at a current density of 0.1 A / g, and still had a reversible capacity of 680 mAh / g after 100 cycles at a current density of 0.3 A / g, showing excellent cycle stability.

[0070] Comparative Example 1

[0071] This comparative example provides a method for preparing a negative electrode material, comprising the following steps:

[0072] S1: Add 1 mmol of methyl orange into a three-necked flask filled with 80 mL of 0.05 mol / L hydrochloric acid solution, stir at 0°C for half an hour to obtain a soft template solution;

[0073] S2: adding 0.82 g of aniline to the soft template solution to obtain a pre-reaction solution;

[0074] S3: adding ammonium persulfate dropwise to the pre-reaction solution at a uniform rate, wherein the molar ratio of ammonium persulfate to aniline is 1:1, and polymerizing the solution at 0° C. for 24 hours to obtain a carbon nanotube precursor;

[0075] S4: After the carbon nanotube precursor is rotary evaporated at 50-70°C, the obtained product is calcined under nitrogen conditions at a calcination temperature of 800°C for 3 hours to obtain N, S doped CNTs, i.e., negative electrode materials.

[0076] Since cobalt nitrate is not added in this comparative example, no sulfide is generated during the reaction, and therefore no washing process is required in step S4.

[0077] The negative electrode material prepared in the comparative example was used as the negative electrode material of a lithium-ion battery for performance testing; after testing, the composite negative electrode material had a reversible specific capacity of 377 mAh / g at a current density of 0.1 A / g, and had a reversible capacity of 267 mAh / g after 100 cycles at a current density of 0.3 A / g.

[0078] Comparative Example 2

[0079] This comparative example provides a method for preparing a composite negative electrode material, comprising the following steps:

[0080] S1: Add 1 mmol of methyl orange into a three-necked flask filled with 80 mL of 0.05 mol / L hydrochloric acid solution, stir at 0°C for half an hour to obtain a soft template solution;

[0081] S2: adding 0.82 g of aniline to the soft template solution to obtain a pre-reaction solution;

[0082] S3: adding ammonium persulfate dropwise to the pre-reaction solution at a uniform rate, wherein the molar ratio of ammonium persulfate to aniline is 1:1, and polymerizing the solution at 0° C. for 24 hours to obtain a carbon nanotube precursor;

[0083] S4: After the carbon nanotube precursor is subjected to rotary evaporation at 50-70°C, the obtained product is calcined under nitrogen conditions at a calcination temperature of 900°C for 3 hours to obtain N, S doped CNTs;

[0084] S5: Disperse 60 mg of the prepared N, S-doped CNTs into 30 mL of water, then add 0.5 mmol Co(NO3)2·6H2O and 4 mmol thiourea, stir for 2 h until uniform, and dry at 80°C; calcine the resulting product under nitrogen conditions at a calcination temperature of 800°C and keep the temperature constant for 1 h to obtain a Co9S8 / N, S-doped CNTs composite, i.e., a composite negative electrode material.

[0085] The composite negative electrode material prepared in this comparative example was used as a negative electrode material for a lithium-ion battery for performance testing; after testing, the composite negative electrode material had a reversible specific capacity of 752 mAh / g at a current density of 0.1 A / g, and had a reversible capacity of 461 mAh / g after 100 cycles at a current density of 0.3 A / g.

[0086] Comparative Example 3

[0087] The difference between this comparative example and Example 1 is that the amount of Co(NO3)2·6H2O added in step S2 is 2.4 g.

[0088] The composite negative electrode material was used as a negative electrode material for a lithium-ion battery for performance testing; after testing, the composite negative electrode material had a reversible specific capacity of 452 mAh / g at a current density of 0.1 A / g, and had a reversible capacity of 308 mAh / g after 100 cycles at a current density of 0.3 A / g.

[0089] Comparative Example 4

[0090] The difference between this comparative example and Example 1 is that the amount of Co(NO3)2·6H2O added in step S2 is 4.4 g.

[0091] The composite negative electrode material was used as a negative electrode material for a lithium-ion battery for performance testing; after testing, the composite negative electrode material had a reversible specific capacity of 699 mAh / g at a current density of 0.1 A / g, and had a reversible capacity of 415 mAh / g after 100 cycles at a current density of 0.3 A / g.

[0092] It can be seen from the test data of the above embodiments and comparative examples that the composite negative electrode materials prepared in the embodiments of the present invention have a relatively high capacity and excellent cycle stability.

[0093] In the negative electrode material prepared in Comparative Example 1, the prepared CNTs mainly play the role of carrier in the composite, which can effectively alleviate the volume expansion of sulfide during charging and discharging and improve its conductivity, but its specific capacity as a negative electrode material itself is relatively low.

[0094] Although the composite negative electrode material prepared in Comparative Example 2 is also a Co9S8 / N,S doped CNTs composite, the preparation process is complicated, and the formed sulfide can only be loaded on the surface of CNTs. The formed sulfide particles are large, and CNTs cannot effectively alleviate its volume expansion during the charge and discharge process, resulting in poor cycle stability.

[0095] The composite negative electrode material prepared in Comparative Example 3 has a high carbon content, resulting in a low capacity, and the impact on the cycle performance is not very obvious.

[0096] The composite negative electrode material prepared in Comparative Example 4 has a high sulfide content, which will lead to poor cycle performance.

[0097] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A method for preparing a composite negative electrode material, characterized in that: The steps include: S1: Mix the soft template agent with the acidic solution and stir at 0°C to obtain a soft template solution; S2: adding a transition metal salt and a conductive monomer to the soft template solution to obtain a pre-reaction mixed solution; S3: adding ammonium persulfate dropwise to the pre-reaction mixture to carry out polymerization reaction at 0° C. to obtain a composite material precursor; S4: calcining the composite material precursor in an inert atmosphere at 800-1000° C., washing, and drying to obtain a composite negative electrode material; The conductive monomer is selected from at least one of an aniline monomer and a pyrrole monomer; The soft template is methyl orange.

2. The composite negative electrode material according to claim 1, characterized in that The acidic solution is a hydrochloric acid solution.

3. The method for preparing the composite negative electrode material according to claim 1, characterized in that: The transition metal salt is selected from at least one of cobalt salts, nickel salts, zinc salts, manganese salts, iron salts and tin salts.

4. The method for preparing the composite negative electrode material according to claim 3, characterized in that: The transition metal salt is selected from at least one of transition metal nitrates and transition metal sulfates.

5. The method for preparing a composite negative electrode material according to any one of claims 1 to 4, characterized in that: The molar ratio of the soft template to the conductive monomer is 1:(5-15).

6. The method for preparing the composite negative electrode material according to claim 5, characterized in that: The mass ratio of the transition metal salt to the conductive monomer is (140-200):

41.

7. The method for preparing the composite negative electrode material according to claim 5, characterized in that: The molar ratio of the ammonium persulfate to the conductive monomer is 1:

1.

8. A composite negative electrode material, characterized in that: The composite negative electrode material is prepared by the method for preparing the composite negative electrode material according to any one of claims 1 to 7.

9. A lithium ion battery, characterized in that: Comprising the composite negative electrode material as claimed in claim 8.