Aqueous hyperbranched polymer and preparation method thereof

Through the esterification and neutralization reaction of acid anhydride and alcohol, hyperbranched polymer is constructed, which solves the problems of unstable and high energy consumption of hyperbranched polymers in the prior art, and achieves stable dissolution of aqueous hyperbranched polymers and efficient synthesis improves environmental applicability.

CN115746273BActive Publication Date: 2024-11-12CNOOC CHANGZHOU PAINT & COATINGS IND RES INST +3
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211460416.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-17
Publication Date
2024-11-12
Estimated Expiration
2042-11-17

AI Technical Summary

Technical Problem

The existing hyperbranched polymers form a turbid liquid state in water, making it difficult to maintain a stable water-based state, and the synthesis process has low reaction efficiency, high energy consumption, and poor environmental protection and applicability.

Method used

Acid anhydride and alcohol are used as raw materials to construct hyperbranched polymers through esterification and melt polymerization, and combined with neutralization reactions to avoid the introduction of organic solvents, so as to achieve the water-based hyperbranched polymers and improve their water solubility and environmental applicability.

Benefits of technology

The stable dissolution of hyperbranched polymers in water is achieved, the reaction efficiency and environmental applicability are improved, the process energy consumption is reduced, the formation of turbid liquid state is avoided, and the application basis for water-based environmental protection is provided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FDA0005052339890000011
    Figure FDA0005052339890000011
  • Figure GDA0005052339900000011
    Figure GDA0005052339900000011
  • Figure GDA0005052339900000021
    Figure GDA0005052339900000021
Patent Text Reader

Abstract

The present invention provides an aqueous hyperbranched polymer and a preparation method thereof. The aqueous hyperbranched polymer preparation method provided by the present invention adopts anhydride and alcohol as raw materials, takes esterification reaction as reaction principle, utilizes melt polymerization as reaction means to construct hyperbranched polymer, and the melt polymerization method avoids the introduction of organic solvent, and does not require post-processing, which not only improves the environmental applicability of resin, reduces process energy consumption, but also improves reaction efficiency, and can achieve rapid esterification. In addition, the water solubility of hyperbranched polymer is improved by neutralization and salt formation, and hyperbranched polymer can be directly dissolved in water without using any organic auxiliary agent, and hyperbranched polymer can be easily water-based, and aqueous hyperbranched polymer solution will not form a turbid liquid state, and aqueous hyperbranched polymer solution can be transparent or translucent, and aqueous hyperbranched polymer solution can maintain a stable aqueous state.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hyperbranched polymers, and in particular relates to an aqueous hyperbranched polymer and a preparation method thereof. Background Art

[0002] Hyperbranched polymers are widely used in biology, chemical industry and medicine due to their simple synthesis operation and mild technical route. At present, hyperbranched polymers are generally solvent-based. Due to the increasingly strict control of VOC by the state in recent years, solvent-based hyperbranched polymers are not applicable to certain fields with high environmental protection requirements. Due to the water-based nature of solvent-based hyperbranched polymers, a considerable number of hydrophilic groups such as carboxyl, amino, hydroxyl and ether bonds are usually introduced into the molecular structure, but solvent-based hyperbranched polymers and water will form a turbid liquid state, which is difficult to maintain a stable aqueous state. In addition, the reaction efficiency of the synthesis process of solvent-based hyperbranched polymers is low, the energy consumption is high, and the environmental applicability is poor. Summary of the invention

[0003] The purpose of the embodiments of the present invention is to provide an aqueous hyperbranched polymer to solve the technical problems that the existing hyperbranched polymer forms a turbid liquid state with water, it is difficult to maintain a stable aqueous state, it is not easy to achieve the aqueous state of the hyperbranched polymer, the process reaction efficiency is low, the energy consumption is high, and the environmental applicability is poor.

[0004] To achieve the above object, the technical solution adopted by the present invention is: to provide an aqueous hyperbranched polymer, comprising the following components in the following mass percentages:

[0005]

[0006]

[0007] Optionally, the acid anhydride is at least one of maleic anhydride, methyltetrahydrophthalic anhydride, succinic anhydride and phthalic anhydride.

[0008] Optionally, the alcohol is at least one of pentaerythritol, glycerol and trimethylolpropane.

[0009] Optionally, the catalyst is at least one of tetraethylammonium bromide, triethylamine, tetrabutylammonium bromide and triphenylphosphine.

[0010] Optionally, the amine is at least one of diethylenetriamine, triethylenetetramine, tetraethylenepentamine and ammonia water.

[0011] Optionally, the molar ratio of the acid anhydride to the alcohol is (45-64):20.

[0012] Another object of the embodiments of the present invention is to provide a method for preparing an aqueous hyperbranched polymer.

[0013] To achieve the above object, the technical solution adopted by the present invention is: to provide a method for preparing an aqueous hyperbranched polymer that can prepare the aqueous hyperbranched polymer provided by any of the above schemes, and the method for preparing the aqueous hyperbranched polymer comprises the following steps:

[0014] Step S01, weighing anhydride, alcohol, catalyst, amine and deionized water respectively according to the components contained in the aqueous hyperbranched polymer described in any of the above schemes;

[0015] Step S02, dehydration of raw materials: dehydration of the anhydride, alcohol, catalyst and amine in step S01 is performed by vacuum method;

[0016] Step S03, half-esterification reaction: mixing anhydride and alcohol in a predetermined ratio, and performing a half-esterification reaction under heating and stirring conditions to obtain a primary hyperbranched polymer whose external groups are carboxyl groups;

[0017] Step S04, esterification reaction: adding a catalyst and a predetermined proportion of alcohol to the primary hyperbranched polymer whose external group is a carboxyl group in step S03, and performing an esterification reaction under heating and stirring conditions to obtain a secondary hyperbranched polymer whose external group is a hydroxyl group;

[0018] Step S05, esterification reaction: adding a predetermined proportion of anhydride to the second-generation hyperbranched polymer whose external group is a hydroxyl group in step S04, and performing a half-esterification reaction under heating and stirring conditions to obtain a second-generation hyperbranched polymer whose external group is a carboxyl group;

[0019] Step S06, neutralization reaction: adding amine to the second-generation hyperbranched polymer whose external group is a carboxyl group in step S05, performing a neutralization reaction under heating and stirring conditions, and adding deionized water to obtain an aqueous hyperbranched polymer.

[0020] Optionally, in step S03, the molar ratio of the acid anhydride to the alcohol is (3-4):1.

[0021] Optionally, in step S04, the molar ratio of the primary hyperbranched polymer whose external group is a carboxyl group to the alcohol is 1:(3-4).

[0022] Optionally, in step S05, the molar ratio of the second-generation hyperbranched polymer whose external groups are hydroxyl groups to the acid anhydride is 1:(6-8).

[0023] Compared with the prior art, the one or more technical solutions in the embodiments of the present invention have at least one of the following beneficial effects:

[0024] The aqueous hyperbranched polymer in the embodiment of the present invention or the aqueous hyperbranched polymer prepared by the preparation method in the embodiment of the present invention adopts anhydride and alcohol as raw materials, takes esterification reaction as reaction principle, and utilizes melt polymerization as reaction means to construct the hyperbranched polymer. The melt polymerization method avoids the introduction of organic solvents, and does not require post-treatment, which not only improves the environmental applicability of the resin, reduces process energy consumption, but also improves reaction efficiency, and can achieve rapid esterification. In addition, the water solubility of the hyperbranched polymer is improved by neutralization and salt formation. Under the condition of not using any organic auxiliary agent, the hyperbranched polymer can be directly dissolved in water, and the hyperbranched polymer is easily made water-based, and the aqueous hyperbranched polymer solution will not form a turbid liquid state, and the aqueous hyperbranched polymer solution can be transparent or translucent, and the aqueous hyperbranched polymer solution can maintain a stable aqueous state. DETAILED DESCRIPTION

[0025] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0026] The embodiment of the present invention provides an aqueous hyperbranched polymer that can be directly dissolved in water without using any organic additives, maintains a stable aqueous state, improves the environmental applicability of the resin, reduces process energy consumption, improves reaction efficiency, and can achieve rapid esterification, so as to overcome the defects of existing hyperbranched polymers that provide hydrophilicity through hydrophilic groups, the hydrophilic groups and water will form a turbid liquid state, it is difficult to maintain a stable aqueous state, and it is not easy to achieve the water-based hyperbranched polymer.

[0027] The aqueous hyperbranched polymer provided by the embodiment of the present invention comprises the following components in the following mass percentages:

[0028]

[0029] Specifically, the purity of the raw materials selected in the embodiments of the present invention is above 99.9%. Thus, the water-based hyperbranched polymer provided in the embodiments of the present invention.

[0030] Since the water-based hyperbranched polymer provided by the embodiment of the present invention adopts anhydride and alcohol as raw materials, takes esterification reaction as reaction principle, and utilizes melt polymerization as reaction means to construct the hyperbranched polymer, the melt polymerization method avoids the introduction of organic solvents, and does not require post-treatment, which not only improves the environmental applicability of the resin, reduces process energy consumption, but also improves reaction efficiency, and can achieve rapid esterification. In addition, the water solubility of the hyperbranched polymer is improved by neutralization and salt formation, and the hyperbranched polymer can be directly dissolved in water without using any organic auxiliary agent, and the hyperbranched polymer is easily made water-based, and a turbid liquid state will not be formed, and a stable water-based state is maintained, which further provides a research basis for the application of hyperbranched polymers in the field of water-based environmental protection.

[0031] Optionally, in some of the embodiments, the acid anhydride is at least one of maleic anhydride, methyltetrahydrophthalic anhydride, succinic anhydride and phthalic anhydride.

[0032] Optionally, in some of the embodiments, the alcohol is at least one of pentaerythritol, glycerol and trimethylolpropane.

[0033] Optionally, in some of the embodiments, the catalyst is at least one of tetraethylammonium bromide, triethylamine, tetrabutylammonium bromide and triphenylphosphine.

[0034] Optionally, in some of the embodiments, the amine is at least one of diethylenetriamine, triethylenetetramine, tetraethylenepentamine and ammonia water.

[0035] Optionally, in some of the embodiments, the molar ratio of anhydride to alcohol is (45-64):20, that is, the total molar ratio of anhydride to alcohol is 9:4-16:5.

[0036] The present invention also provides a method for preparing the aqueous hyperbranched polymer in the above embodiment.

[0037] In some embodiments, the method for preparing an aqueous hyperbranched polymer provided by the present invention comprises the following steps:

[0038] Step S01, weighing 36.08-48.36% of anhydride, 12.41-21.92% of alcohol, 0.05-0.10% of catalyst, 19.41-29.53% of amine and 16.64-20.67% of deionized water respectively according to mass percentage as components contained in the aqueous hyperbranched polymer.

[0039] Step S02, dehydration of raw materials: dehydration of the anhydride, alcohol, catalyst and amine in step S01 by vacuum;

[0040] Step S03, half-esterification reaction: mixing anhydride and alcohol in a predetermined ratio, and performing a half-esterification reaction under heating and stirring conditions to obtain a primary hyperbranched polymer whose external groups are carboxyl groups;

[0041] Step S04, esterification reaction: adding a catalyst and a predetermined proportion of alcohol to the first-generation hyperbranched polymer whose external group is a carboxyl group in step S03, and performing an esterification reaction under heating and stirring conditions to obtain a second-generation hyperbranched polymer whose external group is a hydroxyl group;

[0042] Step S05, esterification reaction: adding a predetermined proportion of anhydride to the second-generation hyperbranched polymer whose external group is a hydroxyl group in step S04, and performing a half-esterification reaction under heating and stirring conditions to obtain a second-generation hyperbranched polymer whose external group is a carboxyl group;

[0043] Step S06, neutralization reaction: adding amine to the second-generation hyperbranched polymer whose external group is a carboxyl group in step S05, performing a neutralization reaction under heating and stirring conditions, and adding deionized water to obtain an aqueous hyperbranched polymer.

[0044] The aqueous hyperbranched polymer prepared by the aqueous hyperbranched polymer preparation method provided by the embodiment of the present invention adopts anhydride and alcohol as raw materials, takes esterification reaction as reaction principle, utilizes melt polymerization as reaction means to construct the hyperbranched polymer, and the melt polymerization method avoids the introduction of organic solvents, and does not require post-treatment, which not only improves the environmental applicability of the resin, reduces process energy consumption, but also improves reaction efficiency, and can achieve rapid esterification. In addition, the water solubility of the hyperbranched polymer is improved by neutralization and salt formation, and the hyperbranched polymer can be directly dissolved in water without using any organic auxiliary agent, and the hyperbranched polymer is easily water-based, and a turbid liquid state will not be formed, and a stable aqueous state is maintained, which further provides a research basis for the application of hyperbranched polymers in the field of aqueous environmental protection.

[0045] Optionally, in step S02, the dehydration operation is performed by vacuum means, which means vacuum heating and drying to remove moisture from the raw material.

[0046] Optionally, in step S03, the molar ratio of the acid anhydride to the alcohol is (3-4):1, the acid anhydride is at least one of maleic anhydride, methyltetrahydrophthalic anhydride, succinic anhydride and phthalic anhydride, and the alcohol is at least one of pentaerythritol, glycerol and trimethylolpropane. The stirring speed is 200-2000 r / min, and the reaction is stirred at a temperature of 60-90°C for 4-6 hours.

[0047] Optionally, in step S04, the molar ratio of the primary hyperbranched polymer whose external group is a carboxyl group to the alcohol is 1:(3-4), the alcohol is at least one of pentaerythritol, glycerol and trimethylolpropane, the stirring speed is 200-2000 r / min, and the reaction is stirred at a temperature of 180-220°C for 4-6 hours.

[0048] Optionally, in step S05, the molar ratio of the second-generation hyperbranched polymer whose external group is a hydroxyl group to the acid anhydride is 1:(6-8), the acid anhydride is at least one of maleic anhydride, methyltetrahydrophthalic anhydride, succinic anhydride and phthalic anhydride, the stirring speed is 200-2000 r / min, and the reaction is stirred at a temperature of 60-90°C for 4-6 hours.

[0049] Optionally, in step S06, the stirring speed is 200-2000 r / min, and the stirring reaction is carried out at a temperature of 60-80°C for 2-4 hours.

[0050] In order to enable the above implementation details and operations of the present invention to be clearly understood by those skilled in the art, and to significantly demonstrate the improved performance of the water-based hyperbranched polymer and the preparation method thereof of the present invention, the implementation of the present invention is illustrated by way of examples below.

[0051] Example 1

[0052] (1) Drying of raw materials

[0053] Vacuum phthalic anhydride and trimethylolpropane at 50°C for 1 h and store them in a sealed bottle for later use.

[0054] (2) Half-esterification reaction

[0055] The phthalic anhydride 444.21g and trimethylolpropane 134.06g obtained in step (1) were heated under stirring conditions and reacted for a period of time at a stirring speed of 200r / min, a reaction temperature of 60°C and a reaction time of 4h to obtain a primary hyperbranched polymer whose external groups are carboxyl groups.

[0056] (3) Esterification reaction

[0057] Add 402.01 g of trimethylolpropane and 2.95 g of triphenylphosphine to the product obtained in step (2), heat the mixture under stirring, and react for a period of time at a stirring speed of 200 r / min, a reaction temperature of 180° C., and a reaction time of 4 h to obtain a second-generation hyperbranched polymer whose external groups are hydroxyl groups;

[0058] (4) Half-esterification reaction

[0059] Add 888.16 g of phthalic anhydride to the product obtained in step (3), raise the temperature under stirring, and react for a period of time at a stirring speed of 200 r / min, a reaction temperature of 60° C., and a reaction time of 4 h to obtain a second-generation hyperbranched polymer whose external group is a carboxyl group;

[0060] (5) Neutralization reaction

[0061] Add 618.43 g of diethylenetriamine to the product obtained in step (4), heat up under stirring, react for a period of time, the stirring speed is 200 r / min, the reaction temperature is 60° C., the reaction time is 2 h, and 497.39 g of deionized water is added to obtain an aqueous hyperbranched polymer solution.

[0062] Example 2

[0063] (1) Drying of raw materials

[0064] Vacuum maleic anhydride and trimethylolpropane at 50°C for 1 h and store in a sealed bottle for later use.

[0065] (2) Half-esterification reaction

[0066] 294.53 g of maleic anhydride and 134.21 g of trimethylolpropane obtained in step (1) were heated under stirring conditions and reacted for a period of time at a stirring speed of 500 r / min, a reaction temperature of 70° C., and a reaction time of 5 h to obtain a primary hyperbranched polymer whose external groups are carboxyl groups.

[0067] (3) Esterification reaction

[0068] Add 402.33 g of trimethylolpropane and 2.49 g of triphenylphosphine to the product obtained in step (2), heat the mixture under stirring, and react for a period of time at a stirring speed of 800 r / min, a reaction temperature of 190° C., and a reaction time of 5 h to obtain a second-generation hyperbranched polymer whose external groups are hydroxyl groups;

[0069] (4) Half-esterification reaction

[0070] Add 588.45 g of maleic anhydride to the product obtained in step (3), heat the mixture under stirring, and react for a period of time at a stirring speed of 900 r / min, a reaction temperature of 70° C., and a reaction time of 5 h to obtain a second-generation hyperbranched polymer whose external groups are carboxyl groups;

[0071] (5) Neutralization reaction

[0072] Add 618.12 g of diethylenetriamine to the product obtained in step (4), heat up under stirring, react for a period of time, the stirring speed is 1000 r / min, the reaction temperature is 70° C., the reaction time is 3 h, and 407.22 g of deionized water is added to obtain an aqueous hyperbranched polymer solution.

[0073] Example 3

[0074] (1) Drying of raw materials

[0075] Succinic anhydride and trimethylolpropane were vacuumed at 50°C for 1 h and stored in a sealed bottle for later use.

[0076] (2) Half-esterification reaction

[0077] 300.97 g of succinic anhydride and 134.19 g of trimethylolpropane obtained in step (1) were heated under stirring conditions and reacted for a period of time at a stirring speed of 2000 r / min, a reaction temperature of 90° C., and a reaction time of 6 h to obtain a primary hyperbranched polymer whose external groups are carboxyl groups.

[0078] (3) Esterification reaction

[0079] Add 402.95 g of trimethylolpropane and 2.52 g of triphenylphosphine to the product obtained in step (2), heat the mixture under stirring, and react for a period of time at a stirring speed of 2000 r / min, a reaction temperature of 220° C., and a reaction time of 6 h to obtain a second-generation hyperbranched polymer whose external groups are hydroxyl groups;

[0080] (4) Half-esterification reaction

[0081] Add 600.73 g of succinic anhydride to the product obtained in step (3), heat the mixture under stirring, and react for a period of time at a stirring speed of 2000 r / min, a reaction temperature of 90° C., and a reaction time of 6 h to obtain a second-generation hyperbranched polymer whose external groups are carboxyl groups;

[0082] (5) Neutralization reaction

[0083] Add 618.98 g of diethylenetriamine to the product obtained in step (4), heat up under stirring, react for a period of time, the stirring speed is 2000 r / min, the reaction temperature is 80° C., the reaction time is 4 h, and 411.57 g of deionized water is added to obtain an aqueous hyperbranched polymer solution.

[0084] Example 4

[0085] (1) Drying of raw materials

[0086] Evacuate methyltetrahydrophthalic anhydride and trimethylolpropane at 50°C for 1 h and store them in a sealed bottle for later use.

[0087] (2) Half-esterification reaction

[0088] 498.53 g of methyltetrahydrophthalic anhydride and 134.99 g of trimethylolpropane obtained in step (1) were heated under stirring conditions and reacted for a period of time at a stirring speed of 1200 r / min, a reaction temperature of 80° C., and a reaction time of 5 h to obtain a primary hyperbranched polymer whose external groups are carboxyl groups.

[0089] (3) Esterification reaction

[0090] Add 402.41 g of trimethylolpropane and 3.18 g of triphenylphosphine to the product obtained in step (2), heat the mixture under stirring, and react for a period of time at a stirring speed of 1000 r / min, a reaction temperature of 200° C., and a reaction time of 5 h to obtain a second-generation hyperbranched polymer whose external groups are hydroxyl groups;

[0091] (4) Half-esterification reaction

[0092] Add 996.17 g of methyltetrahydrophthalic anhydride to the product obtained in step (3), heat the mixture under stirring, and react for a period of time at a stirring speed of 1500 r / min, a reaction temperature of 80° C., and a reaction time of 5 h to obtain a second-generation hyperbranched polymer whose external groups are carboxyl groups;

[0093] (5) Neutralization reaction

[0094] Add 618.18 g of diethylenetriamine to the product obtained in step (4), heat up under stirring, react for a period of time, the stirring speed is 1100 r / min, the reaction temperature is 75° C., the reaction time is 3 h, and 530.88 g of deionized water is added to obtain an aqueous hyperbranched polymer solution.

[0095] Example 5

[0096] (1) Drying of raw materials

[0097] Vacuum maleic anhydride and pentaerythritol at 50°C for 1 h and store them in a sealed bottle for later use.

[0098] (2) Half-esterification reaction

[0099] 392.77 g of maleic anhydride and 136.45 g of pentaerythritol obtained in step (1) were heated under stirring conditions and reacted for a period of time at a stirring speed of 1800 r / min, a reaction temperature of 90° C., and a reaction time of 6 h to obtain a primary hyperbranched polymer whose external groups are carboxyl groups.

[0100] (3) Esterification reaction

[0101] Add 544.71 g of pentaerythritol and 3.22 g of triphenylphosphine to the product obtained in step (2), heat the mixture under stirring, and react for a period of time at a stirring speed of 1600 r / min, a reaction temperature of 210° C., and a reaction time of 6 h to obtain a second-generation hyperbranched polymer whose external groups are hydroxyl groups;

[0102] (4) Half-esterification reaction

[0103] Add 1176.58 g of maleic anhydride to the product obtained in step (3), raise the temperature under stirring, and react for a period of time at a stirring speed of 1700 r / min, a reaction temperature of 70° C., and a reaction time of 4 h to obtain a second-generation hyperbranched polymer whose external group is a carboxyl group;

[0104] (5) Neutralization reaction

[0105] Add 1236.56 g of diethylenetriamine to the product obtained in step (4), heat up under stirring, react for a period of time, the stirring speed is 900 r / min, the reaction temperature is 70° C., the reaction time is 3 h, and 697.43 g of deionized water is added to obtain an aqueous hyperbranched polymer solution.

[0106] Example 6

[0107] (1) Drying of raw materials

[0108] Succinic anhydride and pentaerythritol were placed in a vacuum at 50°C for 1 h and stored in a sealed bottle for later use.

[0109] (2) Half-esterification reaction

[0110] 400.31 g of succinic anhydride and 136.37 g of pentaerythritol obtained in step (1) were heated under stirring conditions and reacted for a period of time at a stirring speed of 800 r / min, a reaction temperature of 85° C., and a reaction time of 4 h to obtain a primary hyperbranched polymer whose external groups are carboxyl groups.

[0111] (3) Esterification reaction

[0112] Add 544.67 g of pentaerythritol and 3.27 g of triphenylphosphine to the product obtained in step (2), heat the mixture under stirring, and react for a period of time at a stirring speed of 1400 r / min, a reaction temperature of 185° C., and a reaction time of 4 h to obtain a second-generation hyperbranched polymer whose external groups are hydroxyl groups;

[0113] (4) Half-esterification reaction

[0114] Add 1201.11 g of succinic anhydride to the product obtained in step (3), heat the mixture under stirring, and react for a period of time at a stirring speed of 1300 r / min, a reaction temperature of 80° C., and a reaction time of 4 h to obtain a second-generation hyperbranched polymer whose external groups are carboxyl groups;

[0115] (5) Neutralization reaction

[0116] Add 1236.19 g of diethylenetriamine to the product obtained in step (4), heat up under stirring, react for a period of time, the stirring speed is 900 r / min, the reaction temperature is 65° C., the reaction time is 2 h, and 703.73 g of deionized water is added to obtain an aqueous hyperbranched polymer solution.

[0117] Example 7

[0118] (1) Drying of raw materials

[0119] Evacuate methyltetrahydrophthalic anhydride and pentaerythritol at 50°C for 1 h and store them in a sealed bottle for later use.

[0120] (2) Half-esterification reaction

[0121] 664.78 g of methyltetrahydrophthalic anhydride and 136.89 g of pentaerythritol obtained in step (1) were heated under stirring conditions and reacted for a period of time at a stirring speed of 1100 r / min, a reaction temperature of 90° C., and a reaction time of 6 h to obtain a primary hyperbranched polymer whose external groups are carboxyl groups.

[0122] (3) Esterification reaction

[0123] Add 544.83 g of pentaerythritol and 4.03 g of triphenylphosphine to the product obtained in step (2), heat the mixture under stirring, and react for a period of time at a stirring speed of 500 r / min, a reaction temperature of 180° C., and a reaction time of 6 h to obtain a second-generation hyperbranched polymer whose external groups are hydroxyl groups;

[0124] (4) Half-esterification reaction

[0125] Add 1992.46 g of methyltetrahydrophthalic anhydride to the product obtained in step (3), heat the mixture under stirring, and react for a period of time at a stirring speed of 400 r / min, a reaction temperature of 90° C., and a reaction time of 6 h to obtain a second-generation hyperbranched polymer whose external groups are carboxyl groups;

[0126] (5) Neutralization reaction

[0127] Add 1236.73 g of diethylenetriamine to the product obtained in step (4), heat up under stirring, react for a period of time, the stirring speed is 900 r / min, the reaction temperature is 60° C., the reaction time is 4 h, and 915.24 g of deionized water is added to obtain an aqueous hyperbranched polymer solution.

[0128] Example 8

[0129] (1) Drying of raw materials

[0130] Vacuum phthalic anhydride and pentaerythritol at 50°C for 1 h and store them in a sealed bottle for later use.

[0131] (2) Half-esterification reaction

[0132] 592.12 g of phthalic anhydride and 136.14 g of pentaerythritol obtained in step (1) were heated under stirring conditions and reacted for a period of time at a stirring speed of 600 r / min, a reaction temperature of 80° C., and a reaction time of 4 h to obtain a primary hyperbranched polymer whose external groups are carboxyl groups.

[0133] (3) Esterification reaction

[0134] Add 544.62 g of pentaerythritol and 3.87 g of triphenylphosphine to the product obtained in step (2), heat the mixture under stirring, and react for a period of time at a stirring speed of 700 r / min, a reaction temperature of 200° C., and a reaction time of 6 h to obtain a second-generation hyperbranched polymer whose external groups are hydroxyl groups;

[0135] (4) Half-esterification reaction

[0136] Add 1632.20 g of phthalic anhydride to the product obtained in step (3), raise the temperature under stirring, and react for a period of time at a stirring speed of 1900 r / min, a reaction temperature of 70° C., and a reaction time of 6 h to obtain a second-generation hyperbranched polymer whose external group is a carboxyl group;

[0137] (5) Neutralization reaction

[0138] Add 1236.98 g of diethylenetriamine to the product obtained in step (4), heat up under stirring, react for a period of time, the stirring speed is 1500 r / min, the reaction temperature is 60° C., the reaction time is 4 h, and 828.68 g of deionized water is added to obtain an aqueous hyperbranched polymer solution.

[0139] Comparative Example

[0140] The raw materials required for synthesizing a solvent-based hyperbranched polymer and an organic solvent are put into a reactor at one time, and the solvent-based hyperbranched polymer is synthesized by a one-step method. The synthesized solvent-based hyperbranched polymer is used as a comparative example in the experiment.

[0141] Performance Testing

[0142] The water-based hyperbranched polymers prepared in Examples 1 to 8 and the solvent-based hyperbranched polymers in the comparative examples were tested for water solubility, and the test results are listed in Table 1.

[0143] Table 1 Water solubility test results of the aqueous hyperbranched polymers prepared in Examples 1 to 8 and the solvent-based hyperbranched polymers in the comparative examples

[0144]

[0145] As can be seen from Table 1, compared with the hyperbranched polymer of the solvent type in the comparative example, which is in a turbid liquid state, the water-based hyperbranched polymer obtained in Examples 1 to 8 is in an emulsion state, translucent, and transparent state, and has good water solubility. Wherein, Example 2 is compared with Example 1, because the hydrophilic ability of maleic anhydride is stronger than that of phthalic anhydride, and Example 2 shows more excellent hydrophilicity. Compared with Example 1, Example 5 and Example 7 have 4 hydroxyls in pentaerythritol, which has better hydrophilicity, so Example 5 and Example 7 have excellent hydrophilicity. In addition, due to the poor hydrophilicity of succinic anhydride and methyltetrahydrophthalic anhydride, the hyperbranched product prepared by them and trimethylolpropane is in an emulsion state or translucent state, so the water-based hyperbranched polymer in Example 3, Example 4, Example 6, and Example 8 is in an emulsion state or translucent state.

[0146] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A water-based hyperbranched polymer, characterized in that According to the percentage by mass, the following components are included: Acid anhydride, alcohol, catalyst and amine are subjected to a vacuum dehydration operation to dehydrate the raw materials; acid anhydride and alcohol in a predetermined ratio are mixed, and a semi-esterification reaction is carried out under heating and stirring conditions to obtain a first-generation hyperbranched polymer whose external group is a carboxyl group; a catalyst and a predetermined ratio of alcohol are added to the first-generation hyperbranched polymer whose external group is a carboxyl group, and an esterification reaction is carried out under heating and stirring conditions to obtain a second-generation hyperbranched polymer whose external group is a hydroxyl group; acid anhydride in a predetermined ratio is added to the second-generation hyperbranched polymer whose external group is a hydroxyl group, and a semi-esterification reaction is carried out under heating and stirring conditions to obtain a second-generation hyperbranched polymer whose external group is a carboxyl group; amine is added to the second-generation hyperbranched polymer whose external group is a carboxyl group, and a neutralization reaction is carried out under heating and stirring conditions, and after adding deionized water, the water-based hyperbranched polymer can be obtained; The catalyst is at least one of tetraethylammonium bromide, triethylamine, tetrabutylammonium bromide and triphenylphosphine; the amine is at least one of diethylenetriamine, triethylenetetramine, tetraethylenepentamine and ammonia water; the acid anhydride is at least one of succinic anhydride and phthalic anhydride; and the alcohol is at least one of pentaerythritol, glycerol and trimethylolpropane.

2. The aqueous hyperbranched polymer according to claim 1, characterized in that The molar ratio of the acid anhydride to the alcohol is (45-64):

20.

3. A method for preparing an aqueous hyperbranched polymer, characterized in that: The steps include: Step S01, weighing anhydride, alcohol, catalyst, amine and deionized water respectively according to the components contained in the aqueous hyperbranched polymer according to any one of claims 1 to 2; Step S02, dehydration of raw materials: dehydration of the anhydride, alcohol, catalyst and amine in step S01 is performed by vacuum method; Step S03, half-esterification reaction: mixing anhydride and alcohol in a predetermined ratio, and performing a half-esterification reaction under heating and stirring conditions to obtain a primary hyperbranched polymer whose external groups are carboxyl groups; Step S04, esterification reaction: adding a catalyst and a predetermined proportion of alcohol to the primary hyperbranched polymer whose external group is a carboxyl group in step S03, and performing an esterification reaction under heating and stirring conditions to obtain a secondary hyperbranched polymer whose external group is a hydroxyl group; Step S05, esterification reaction: adding a predetermined proportion of anhydride to the second-generation hyperbranched polymer whose external group is a hydroxyl group in step S04, and performing a half-esterification reaction under heating and stirring conditions to obtain a second-generation hyperbranched polymer whose external group is a carboxyl group; Step S06, neutralization reaction: adding amine to the second-generation hyperbranched polymer whose external group is a carboxyl group in step S05, performing a neutralization reaction under heating and stirring conditions, and adding deionized water to obtain an aqueous hyperbranched polymer.

4. The method for preparing an aqueous hyperbranched polymer as claimed in claim 3, wherein: In the step S03, the molar ratio of the acid anhydride to the alcohol is (3-4):

1.

5. The method for preparing an aqueous hyperbranched polymer according to claim 3, wherein: In the step S04, the molar ratio of the primary hyperbranched polymer whose external groups are carboxyl groups to the alcohol is 1:(3-4).

6. The method for preparing an aqueous hyperbranched polymer according to any one of claims 3 to 5, characterized in that: In the step S05, the molar ratio of the second-generation hyperbranched polymer whose external groups are hydroxyl groups to the acid anhydride is 1:(6-8).