A molten salt material with high energy storage density and a preparation method thereof

By using the KNO3-NaNO2-KNO2 ternary system and modified ceramic and graphite materials in nitrate molten salt, the problem of low specific heat capacity and energy storage density of nitrate molten salt materials is solved, and high energy storage density and rapid heat transfer are achieved. effect.

CN115746798BActive Publication Date: 2024-10-08BEIJING MINLI ENERGY STORAGE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211383180.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-05
Publication Date
2024-10-08
Estimated Expiration
2042-11-05

AI Technical Summary

Technical Problem

Existing nitrate molten salt materials have low specific heat capacity and energy storage density, and cannot effectively improve their thermal conductivity and stability.

Method used

The KNO3-NaNO2-KNO2 ternary nitric acid molten salt system is used, and modified ceramic powder and high thermal conductivity porous support material graphite are added to it. The thermal conductivity and stability of the molten salt are improved through spraying and electrostatic adsorption, and the ceramics are strengthened. Anti-oxidation properties of materials.

Benefits of technology

It significantly increases the specific heat capacity and energy storage density of molten nitrate salt, enhances its thermal conductivity and stability, achieves rapid heat transfer and captures carbon dioxide, and has environmental protection effects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115746798B_ABST
    Figure CN115746798B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of molten salt materials, and discloses a molten salt material with high energy storage density and a preparation method thereof. The preparation method of the molten salt material with high energy storage density comprises the following steps: (1) preparing modified ceramic powder; (2) mixing and stirring dehydrated KNO3 powder, dehydrated NaNO2 powder, dehydrated KNO2 powder and modified ceramic powder, heating, and statically melting to obtain a nitrate molten salt mixed system; (3) kneading, carbonizing and purifying graphite, graphene oxide, phenolic resin binder and mesophase carbon microspheres to obtain a purified graphite mixture; (4) mixing the purified graphite mixture, nanosilver and hydrotalcite powder to obtain a graphite mixture; statically pressing the graphite mixture to obtain a graphite block; infiltrating the graphite block with the nitrate molten salt mixed system to obtain a molten salt material. The prepared molten salt material is added with a variety of functional additives and modified, and has the advantages of high thermal conductivity and high energy storage density.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of molten salt materials, and in particular to a molten salt material with high energy storage density and a preparation method thereof. Background Art

[0002] Molten salt refers to a molten inorganic salt formed by a mixture of metal cations and non-metal anions. Molten salt is solid at room temperature and pressure, and turns into liquid after reaching a certain temperature, making the molten salt system a common heat transfer and heat storage medium. Common molten salt materials include fluoride salts, chloride salts, sulfates, nitrates, etc. Molten salt materials represented by nitrates are important materials in the field of high-temperature phase change, and have broad application prospects in the fields of solar energy, industrial waste heat utilization, etc.

[0003] Existing research on nitrate molten salt materials is as follows: Patent application CN113817451A discloses a method for preparing a binary molten salt of a nitrate system. Potassium chloride and sodium chloride are selected to prepare a binary molten salt through a strong acid cation exchange resin. For example, patent application CN113429946A discloses a method for preparing a heat-conductive nitrate molten salt. Single crystal silicon is added to the nitrate molten salt to improve the thermal conductivity of the nitrate molten salt. However, the above-mentioned nitrate molten salt systems cannot effectively improve the disadvantages of low specific heat capacity and low energy storage density of nitrate molten salt materials. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a method for preparing a molten salt material with high energy storage density, comprising the following steps:

[0005] Step (1) Preparation of modified ceramic powder: Yb2SiO5 powder and Yb2Si2O7 powder are mixed and stirred to obtain a mixed material; the mixed material is sprayed on the ceramic powder to obtain a sprayed ceramic powder.

[0006] In the above process, Yb2SiO5 powder and Yb2Si2O7 powder are mixed to prepare a mixed material, which is sprayed on the ceramic powder to obtain a protective coating of the ceramic powder.

[0007] Step (2) Preparation of a nitrate molten salt mixed system: drying KNO3, NaNO2 and KNO2 respectively to obtain dehydrated KNO3 powder, dehydrated NaNO2 powder and dehydrated KNO2 powder; mixing, stirring, heating and statically melting the dehydrated KNO3 powder, dehydrated NaNO2 powder and dehydrated KNO2 powder to obtain a nitrate molten salt mixed system;

[0008] In the above reaction process, a KNO3-NaNO2-KNO2 ternary nitrate molten salt system is prepared.

[0009] Step (3) Preparation of purified graphite: mixing and stirring graphite, graphene oxide, phenolic resin binder and mesophase carbon microspheres to obtain an intermediate; kneading the intermediate to obtain a crushed mixture; carbonizing the crushed mixture to obtain a carbonized graphite mixed material; purifying the carbonized graphite mixed material to obtain a purified graphite mixture;

[0010] In the above reaction process, a densified graphite mixture is prepared.

[0011] Step (4) Preparation of molten salt material with high energy storage density: ball milling hydrotalcite to obtain hydrotalcite powder; mixing the purified graphite mixture, nanosilver and hydrotalcite powder to obtain a graphite mixture; static pressing the graphite mixture to obtain a rectangular graphite block; contacting and infiltrating the nitrate molten salt mixture system with the graphite block to obtain a molten salt material with high energy storage density.

[0012] In the above reaction process, the density of the densified graphite mixture is further enhanced by adding nanosilver and ball-milled hydrotalcite powder. At the same time, nanosilver is used to enhance the thermal properties of the graphite mixture, and hydrotalcite is used to capture carbon dioxide gas near the molten salt system.

[0013] Preferably, the ratio of the mixed material to the ceramic powder in step (1) is (45-50) g:50 g.

[0014] Preferably, in step (2), the mixed amount ratio of dehydrated KNO3 powder, dehydrated NaNO2 powder, dehydrated KNO2 powder and modified ceramic powder is 10g:5g:6g:(5-10)g.

[0015] Preferably, in step (2), the static melting temperature is 400-410° C. and the static melting time is 4 hours.

[0016] Preferably, in step (3), the carbonization temperature is 750-800°C; and the purification temperature is 2000-2200°C.

[0017] Preferably, in step (4), the static pressure temperature is 25° C. and the static pressure pressure is 250-280 MPa.

[0018] Preferably, in step (3), the ratio of the purified graphite mixture, nanosilver and hydrotalcite powder is (45-50) g: (10-20) g: (5-10) g.

[0019] Preferably, in step (4), the infiltration pressure is 3-4 standard atmospheres, and the infiltration time is 2-3 hours.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] (1) The present invention adopts KNO3-NaNO2-KNO2 ternary nitrate molten salt, and the mixed molten salt ratio itself can improve the specific heat capacity of nitrate molten salt. At the same time, by doping ceramic materials in the mixed molten salt system, on the one hand, the thermal conductivity of the mixed molten salt system can be enhanced; on the other hand, the ceramic material itself is chemically inert, which can enhance the stability of nitrate molten salt. However, since the molten salt is a corrosive medium, the oxidation of the ceramic material is accelerated, resulting in rapid degradation of the ceramic performance. By modifying the ceramic material and spraying Yb2SiO5 and Yb2Si2O7 as a protective coating, the ceramic material and the molten salt as a corrosive medium are isolated, thereby effectively improving the stability of the ceramic material.

[0022] (2) In order to further improve the stability of the mixed molten salt and realize the encapsulation of the molten salt pile, the liquid phase infiltration method is used to realize the composite of the mixed molten salt system and the high thermal conductivity porous support material. At the same time, it can also improve the thermal conductivity of the molten salt material and realize rapid heat transfer. Among them, the high thermal conductivity porous support material is selected as graphite. Before the graphite and the mixed molten salt system are composited, the graphite is densified.

[0023] (3) Densified graphite is prepared by mixing graphite, reduced graphene oxide, carbon densifier mesophase carbon microspheres, nanosilver and phenolic resin binder. On the one hand, graphene oxide is a hexagonal honeycomb lattice structure formed by hybridization of carbon atoms. It has a large surface area and a high thermal conductivity coefficient, which can improve the thermal conductivity of the substrate; at the same time, graphene oxide has abundant functional groups such as carbon, carboxyl, and hydroxyl, which can react with nanosilver. The doping of nanosilver can not only enhance the thermal properties of the mixed molten salt, but also fill the layered voids of graphite and reduced graphene oxide, so that the density of graphite is increased, the leakage and penetration of the mixed molten salt system are prevented, and the packaging effect of the solid fuel molten salt pile is played. At the same time, the added graphene oxide can adsorb the metal cations in the molten salt by electrostatic action, thereby inhibiting the growth and agglomeration of the added hydrotalcite nuclei, so that the hydrotalcite can be evenly dispersed in the molten salt system, effectively capturing the nearby carbon dioxide gas, and achieving better environmental protection effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 is a process flow chart for preparing modified ceramic powder according to the present invention;

[0025] Figure 2 It is a process flow chart of preparing a nitrate molten salt mixed system according to the present invention;

[0026] Figure 3 This is a process flow chart of preparing a molten salt material with high energy storage density according to the present invention;

[0027] Figure 4It is a line graph of the phase change latent heat enthalpy data of the high energy storage density molten salt material prepared by the present invention. DETAILED DESCRIPTION

[0028] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention. Example

[0029] This embodiment discloses a method for preparing a molten salt material with high energy storage density, which comprises the following steps:

[0030] Step 1: Preparation of modified ceramic powder

[0031] 1) 30 g of Yb2SiO5 powder and 25 g of Yb2Si2O7 powder were mixed and stirred to obtain a mixed material; wherein the mixing and stirring speed was 1000 r / min and the mixing and stirring time was 30 min.

[0032] 2) 45 g of the mixed material was sprayed on 50 g of ceramic powder using vacuum plasma spraying technology to obtain modified ceramic powder.

[0033] Step 2: Preparation of molten nitrate mixed system

[0034] 1) Dry 10 g of KNO3, 5 g of NaNO2 and 6 g of KNO2 to obtain dehydrated KNO3 powder, dehydrated NaNO2 powder and dehydrated KNO2 powder respectively; wherein the drying temperature is 90°C and the drying time is 10 h.

[0035] 2) 10 g of dehydrated KNO3 powder, 5 g of dehydrated NaNO2 powder, 6 g of dehydrated KNO2 powder and 5 g of modified ceramic powder are mixed, stirred, heated and statically melted to obtain a nitrate molten salt mixture system; wherein the stirring speed is 1000 r / min and the mixing time is 30 min; the static melting temperature is 400°C and the static melting time is 4 h.

[0036] Step 3: Preparation of purified graphite mixture

[0037] 1) 50 g of graphite, 15 g of graphene oxide, 15 g of phenolic resin binder and 8 g of mesocarbon microspheres were kneaded to obtain a crushed mixture; wherein the kneading time was 30 min;

[0038] 2) The pulverized mixture is carbonized to obtain a carbonized graphite mixture; wherein the carbonization temperature is 750°C and the carbonization time is 4 hours. The carbonized graphite mixture is purified to obtain a purified graphite mixture; wherein the purification temperature is 2000°C and the purification time is 1 hour;

[0039] Step 4: Preparation of molten salt materials with high energy storage density

[0040] 1) ball milling the hydrotalcite to obtain hydrotalcite powder; wherein the fineness of the hydrotalcite powder is 3 mm;

[0041] 2) 45g of the purified graphite mixture, 10g of nanosilver and 5g of hydrotalcite powder were mixed to obtain a graphite mixture. The graphite mixture was poured into a rectangular mold and a graphite block with a size of 10mm×10mm×3mm was prepared by static pressing; wherein the static pressing temperature was 25°C and the static pressing pressure was 250MPa.

[0042] 3) The nitrate molten salt mixed system is placed in a reactor, and then the reactor is vacuumed and heated, and argon is filled into the heated reactor to obtain a reactor filled with argon; wherein, the heating temperature is 500°C and the pressure is one standard atmosphere; then the nitrate molten salt mixed system is contacted and infiltrated with the graphite block to obtain a molten salt material with high energy storage density. During the infiltration period, argon is continuously filled into the reactor so that the pressure in the reactor is 3 standard atmospheres; the infiltration time is 2 hours. Example

[0043] This embodiment discloses a method for preparing a molten salt material with high energy storage density, which comprises the following steps:

[0044] Step 1: Preparation of modified ceramic powder

[0045] 1) 30 g of Yb2SiO5 powder and 25 g of Yb2Si2O7 powder were mixed and stirred to obtain a mixed material; wherein the mixing and stirring speed was 1100 r / min and the mixing and stirring time was 35 min.

[0046] 2) 46 g of the mixed material was sprayed on 50 g of ceramic powder using vacuum plasma spraying technology to obtain modified ceramic powder.

[0047] Step 2: Preparation of molten nitrate mixed system

[0048] 1) Dry 10 g of KNO3, 5 g of NaNO2 and 6 g of KNO2 respectively to obtain dehydrated KNO3 powder, dehydrated NaNO2 powder and dehydrated KNO2 powder; wherein the drying temperature is 92°C and the drying time is 10.5 h.

[0049] 2) 10 g of dehydrated KNO3 powder, 5 g of dehydrated NaNO2 powder, 6 g of dehydrated KNO2 powder and 6 g of modified ceramic powder are mixed, stirred, heated, and statically melted to obtain a nitrate molten salt mixture system; wherein the stirring speed is 1200 r / min, and the mixing time is 55 min; the static melting temperature is 402°C, and the static melting time is 4 h.

[0050] Step 3: Preparation of purified graphite mixture

[0051] 1) 55 g of graphite, 15 g of graphene oxide, 15 g of phenolic resin binder and 8 g of mesocarbon microspheres were kneaded to obtain a crushed mixture; wherein the kneading time was 38 min;

[0052] 2) The pulverized mixture is carbonized to obtain a carbonized graphite mixture; wherein the carbonization temperature is 760°C and the carbonization time is 4 hours. The carbonized graphite mixture is purified to obtain a purified graphite mixture; wherein the purification temperature is 2010°C and the purification time is 1 hour;

[0053] Step 4: Preparation of molten salt materials with high energy storage density

[0054] 1) ball milling the hydrotalcite to obtain hydrotalcite powder; wherein the fineness of the hydrotalcite powder is 4 mm;

[0055] 2) 46 g of the purified graphite mixture, 12 g of nanosilver and 6 g of hydrotalcite powder were mixed to obtain a graphite mixture. The graphite mixture was poured into a rectangular mold and a graphite block of 10 mm × 10 mm × 3 mm in size was prepared by static pressing; wherein the static pressing temperature was 25° C. and the static pressing pressure was 250 MPa.

[0056] 3) Put the nitrate molten salt mixed system into a reactor, then evacuate and heat the reactor, fill the heated reactor with argon, and obtain a reactor filled with argon; wherein the heating temperature is 500°C and the pressure is one standard atmosphere; then contact and infiltrate the nitrate molten salt mixed system with the graphite block to obtain a molten salt material with high energy storage density. During the infiltration period, continue to fill the reactor with argon so that the pressure in the reactor is 3 standard atmospheres; the infiltration time is 2 hours. Example

[0057] This embodiment discloses a method for preparing a molten salt material with high energy storage density, which comprises the following steps:

[0058] Step 1: Preparation of modified ceramic powder

[0059] 1) 30 g of Yb2SiO5 powder and 26 g of Yb2Si2O7 powder were mixed and stirred to obtain a mixed material; wherein the mixing and stirring speed was 1200 r / min and the mixing and stirring time was 36 min.

[0060] 2) 47 g of the mixed material was sprayed on 50 g of ceramic powder using vacuum plasma spraying technology to obtain modified ceramic powder.

[0061] Step 2: Preparation of molten nitrate mixed system

[0062] 1) Dry 10 g of KNO3, 5 g of NaNO2 and 6 g of KNO2 respectively to obtain dehydrated KNO3 powder, dehydrated NaNO2 powder and dehydrated KNO2 powder; wherein the drying temperature is 92°C and the drying time is 10.5 h.

[0063] 2) 10 g of dehydrated KNO3 powder, 5 g of dehydrated NaNO2 powder, 6 g of dehydrated KNO2 powder and 7 g of modified ceramic powder are mixed, stirred, heated and statically melted to obtain a nitrate molten salt mixed system; wherein the stirring speed is 1300 r / min and the mixing time is 56 min; the static melting temperature is 405°C and the static melting time is 4 h.

[0064] Step 3: Preparation of purified graphite mixture

[0065] 1) 55 g of graphite, 15 g of graphene oxide, 15 g of phenolic resin binder and 8 g of mesocarbon microspheres were kneaded to obtain a crushed mixture; wherein the kneading time was 40 min;

[0066] 2) The pulverized mixture is carbonized to obtain a carbonized graphite mixture; wherein the carbonization temperature is 770°C and the carbonization time is 4 hours. The carbonized graphite mixture is purified to obtain a purified graphite mixture; wherein the purification temperature is 2040°C and the purification time is 1 hour;

[0067] Step 4: Preparation of molten salt materials with high energy storage density

[0068] 1) ball milling the hydrotalcite to obtain hydrotalcite powder; wherein the fineness of the hydrotalcite powder is 4 mm;

[0069] 2) 47 g of the purified graphite mixture, 15 g of nanosilver and 7 g of hydrotalcite powder were mixed to obtain a graphite mixture. The graphite mixture was poured into a rectangular mold and a graphite block of 10 mm × 10 mm × 3 mm in size was prepared by static pressing; wherein the static pressing temperature was 25° C. and the static pressing pressure was 255 MPa.

[0070] 3) The nitrate molten salt mixed system is placed in a reactor, and then the reactor is vacuumed and heated, and argon is filled into the heated reactor to obtain a reactor filled with argon; wherein the heating temperature is 500°C and the pressure is one standard atmosphere; the nitrate molten salt mixed system is then contacted and infiltrated with the graphite block to obtain a molten salt material with high energy storage density. During the infiltration period, argon is continuously filled into the reactor so that the pressure in the reactor is 3.5 standard atmospheres; the infiltration time is 2.5 hours. Example

[0071] This embodiment discloses a method for preparing a molten salt material with high energy storage density, which comprises the following steps:

[0072] Step 1: Preparation of modified ceramic powder

[0073] 1) 30 g of Yb2SiO5 powder and 28 g of Yb2Si2O7 powder were mixed and stirred to obtain a mixed material; wherein the mixing and stirring speed was 1300 r / min and the mixing and stirring time was 38 min.

[0074] 2) 48 g of the mixed material was sprayed on 50 g of ceramic powder using vacuum plasma spraying technology to obtain modified ceramic powder.

[0075] Step 2: Preparation of molten nitrate mixed system

[0076] 1) Dry 10 g of KNO3, 5 g of NaNO2 and 6 g of KNO2 respectively to obtain dehydrated KNO3 powder, dehydrated NaNO2 powder and dehydrated KNO2 powder; wherein the drying temperature is 95°C and the drying time is 10.6 h.

[0077] 2) 10 g of dehydrated KNO3 powder, 5 g of dehydrated NaNO2 powder, 6 g of dehydrated KNO2 powder and 8 g of modified ceramic powder are mixed, stirred, heated and statically melted to obtain a nitrate molten salt mixed system; wherein the stirring speed is 1400 r / min and the mixing time is 58 min; the static melting temperature is 407°C and the static melting time is 4 h.

[0078] Step 3: Preparation of purified graphite mixture

[0079] 1) 55 g of graphite, 15 g of graphene oxide, 15 g of phenolic resin binder and 8 g of mesocarbon microspheres were kneaded to obtain a crushed mixture; wherein the kneading time was 42 min;

[0080] 2) The pulverized mixture is carbonized to obtain a carbonized graphite mixture; wherein the carbonization temperature is 780°C and the carbonization time is 4 hours. The carbonized graphite mixture is purified to obtain a purified graphite mixture; wherein the purification temperature is 2100°C and the purification time is 1 hour;

[0081] Step 4: Preparation of molten salt materials with high energy storage density

[0082] 1) ball milling the hydrotalcite to obtain hydrotalcite powder; wherein the fineness of the hydrotalcite powder is 4 mm;

[0083] 2) 48g of the purified graphite mixture, 17g of nanosilver and 8g of hydrotalcite powder were mixed to obtain a graphite mixture. The graphite mixture was poured into a rectangular mold and a graphite block of 10mm×10mm×3mm rectangular size was prepared by static pressing; wherein the static pressing temperature was 25°C and the static pressing pressure was 265MPa.

[0084] 3) The nitrate molten salt mixed system is placed in a reactor, and then the reactor is vacuumed and heated, and argon is filled into the heated reactor to obtain a reactor filled with argon; wherein the heating temperature is 500°C and the pressure is one standard atmosphere; the nitrate molten salt mixed system is then contacted and infiltrated with the graphite block to obtain a molten salt material with high energy storage density. During the infiltration period, argon is continuously filled into the reactor, so that the pressure in the reactor is 3.8 standard atmospheres; the infiltration time is 2.8 hours. Example

[0085] This embodiment discloses a method for preparing a molten salt material with high energy storage density, which comprises the following steps:

[0086] Step 1: Preparation of modified ceramic powder

[0087] 1) 30 g of Yb2SiO5 powder and 30 g of Yb2Si2O7 powder were mixed and stirred to obtain a mixed material; wherein the mixing and stirring speed was 1500 r / min and the mixing and stirring time was 40 min.

[0088] 2) 50 g of the mixed material is sprayed on 50 g of ceramic powder by vacuum plasma spraying technology to obtain modified ceramic powder.

[0089] Step 2: Preparation of molten nitrate mixed system

[0090] 1) Dry 10 g of KNO3, 5 g of NaNO2 and 6 g of KNO2 respectively to obtain dehydrated KNO3 powder, dehydrated NaNO2 powder and dehydrated KNO2 powder; wherein the drying temperature is 100°C and the drying time is 12 h.

[0091] 2) 10 g of dehydrated KNO3 powder, 5 g of dehydrated NaNO2 powder, 6 g of dehydrated KNO2 powder and 7 g of modified ceramic powder are mixed, stirred, heated and statically melted to obtain a nitrate molten salt mixture system; wherein the stirring speed is 1500 r / min and the mixing time is 60 min; the static melting temperature is 410°C and the static melting time is 4 h.

[0092] Step 3: Preparation of purified graphite mixture

[0093] 1) 55 g of graphite, 15 g of graphene oxide, 15 g of phenolic resin binder and 8 g of mesocarbon microspheres were kneaded to obtain a crushed mixture; wherein the kneading time was 50 min;

[0094] 2) Carbonizing the crushed mixture to obtain a carbonized graphite mixture; wherein the carbonization temperature is 800°C and the carbonization time is 4 hours. Purifying the carbonized graphite mixture to obtain a purified graphite mixture; wherein the purification temperature is 2200°C and the purification time is 1 hour;

[0095] Step 4: Preparation of molten salt materials with high energy storage density

[0096] 1) ball milling the hydrotalcite to obtain hydrotalcite powder; wherein the fineness of the hydrotalcite powder is 4 mm;

[0097] 2) 50 g of the purified graphite mixture, 20 g of nanosilver and 10 g of hydrotalcite powder were mixed to obtain a graphite mixture. The graphite mixture was poured into a rectangular mold and a graphite block of 10 mm × 10 mm × 3 mm rectangular size was prepared by static pressing; wherein the static pressing temperature was 25° C. and the static pressing pressure was 280 MPa.

[0098] 3) The nitrate molten salt mixed system is placed in a reactor, and then the reactor is vacuumed and heated, and argon is filled into the heated reactor to obtain an argon-filled reactor; wherein the heating temperature is 500°C and the pressure is one standard atmosphere; the nitrate molten salt mixed system is then contacted and infiltrated with a graphite block to obtain a molten salt material with a high energy storage density. During the infiltration period, argon is continuously filled into the reactor so that the pressure in the reactor is 4 standard atmospheres; the infiltration time is 3 hours.

[0099] Comparative Example 1

[0100] The difference between this comparative example and Example 1 is that the ceramic powder is not modified and the mixture of Yb2SiO5 powder and Yb2Si2O7 powder is sprayed. The other steps and raw materials are the same as those in Example 1.

[0101] Comparative Example 2

[0102] The difference between this comparative example and Example 1 is that the nano silver powder is removed, and the remaining steps and raw materials are the same as Example 1.

[0103] In all the above embodiments and comparative examples, Yb2SiO5 powder comes from Jiangxi Ketai New Materials Co., Ltd. with the article number KT2021; Yb2SiO5 and Yb2Si2O7 come from Wuxi Kaitianxing Electro-Optical Materials Co., Ltd. with the article number YSO; the ceramic powder is selected as alumina, which comes from Qinghe Huichu Welding Materials Co., Ltd. with the article number Al2O3-11; graphite comes from Qingdao Jinhai Graphite Products Co., Ltd.; graphene oxide comes from Shenzhen Guosen Linghang Technology Co., Ltd. with the CAS number 9001, model 7782-42-5, and article number GS-1210.

[0104] Test: The phase change latent heat enthalpy of the unit mass of the prepared molten salt material with high energy storage density was measured using a differential scanning calorimeter. The test results are shown in Table 1:

[0105] It can be seen from the test results of Table 1 that with the increase in the content of the modified ceramic powder, nanosilver and hydrotalcite powder in Examples 1-5 of the present invention, the energy storage density of the prepared molten salt material continues to increase, that is, the value of the latent heat of phase change enthalpy of the prepared unit mass of the molten salt material continues to increase. However, since the ceramic powder is not modified in Comparative Example 1 and the mixed material of Yb2SiO5 powder and Yb2Si2O7 powder is sprayed, the added ceramic powder is accelerated to corrode in the molten salt medium, causing the performance of the ceramic to decline, which is manifested as a decrease in the latent heat of phase change enthalpy of the molten salt material. Since nanosilver powder is not added in Comparative Example 2, nanosilver itself can electrostatically adsorb with graphene oxide and be intercalated in graphene oxide, further enhancing the density of graphite, making the mixed molten salt system unstable, the energy storage density decreases, and the value of the latent heat of phase change enthalpy of the molten salt material decreases.

[0106] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a molten salt material with high energy storage density, characterized in that: The following steps are involved: Step (1) Preparation of modified ceramic powder: Yb2SiO5 powder and Yb2Si2O7 powder are mixed and stirred to obtain a mixed material; the mixed material is sprayed on the ceramic powder to obtain a modified ceramic powder, and the amount ratio of the mixed material to the ceramic powder is (45-50):50; Step (2) Preparation of a nitrate molten salt mixed system: KNO3, NaNO2 and KNO2 are dried respectively to obtain dehydrated KNO3 powder, dehydrated NaNO2 powder and dehydrated KNO2 powder respectively; the dehydrated KNO3 powder, dehydrated NaNO2 powder and dehydrated KNO2 powder are mixed, stirred, heated and statically melted with modified ceramic powder to obtain a nitrate molten salt mixed system, wherein the amount ratio of the dehydrated KNO3 powder, dehydrated NaNO2 powder, dehydrated KNO2 powder and modified ceramic powder is 10:5:6:(5-10); Step (3) Preparation of purified graphite: Graphite, graphene oxide, phenolic resin binder and mesophase carbon microspheres are kneaded, carbonized and purified to obtain a purified graphite mixture, wherein the carbonization temperature is 750-800°C; and the purification temperature is 2000-2200°C; Step (4) Preparation of a molten salt material with high energy storage density: ball milling hydrotalcite to obtain hydrotalcite powder; mixing a purified graphite mixture, nanosilver and hydrotalcite powder to obtain a graphite mixture; statically pressing the graphite mixture to obtain a graphite block; infiltrating the graphite block with a molten nitrate salt mixture system to obtain a molten salt material with high energy storage density; the mixing ratio of the purified graphite mixture, nanosilver and hydrotalcite powder is (45-50):(10-20):(5-10).

2. The method for preparing a molten salt material with high energy storage density according to claim 1, characterized in that: The static melting temperature in step (2) is 400-410° C. and the static melting time is 4 hours.

3. The method for preparing a molten salt material with high energy storage density according to claim 1, characterized in that: In the step (4), the static pressure temperature is 25° C. and the static pressure pressure is 250-280 MPa.

4. The method for preparing a molten salt material with high energy storage density according to claim 1, characterized in that: In the step (4), the infiltration pressure is 3-4 standard atmospheres, and the infiltration time is 2-3 hours.

5. A molten salt material with high energy storage density prepared by the method according to any one of claims 1 to 4.