Epitaxial growth equipment restart method

By using a combination method of hydrogen, etching gas and silicon source gas in the epitaxial growth equipment, the moisture and metal impurities in the reaction chamber are removed, and the problem of low MCLT after the equipment is restarted is solved, and the productivity and quality of the epitaxial wafer is improved.

CN115747756BActive Publication Date: 2024-11-22XIAN ESWIN MATERIAL TECHNOLOGY CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211562148.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-07
Publication Date
2024-11-22
Estimated Expiration
2042-12-07

AI Technical Summary

Technical Problem

After the epitaxial growth equipment is restarted, metal impurities and moisture residues lead to a low life of minority carriers, affecting the productivity and quality of epitaxial wafers. The prior art is difficult to effectively remove, resulting in a decrease in productivity.

Method used

By injecting hydrogen into the reaction chamber of the epitaxial growth device and purge, followed by etching gas and silicon source gas at a specific temperature, the inlet flow rate and time are adjusted to remove moisture and metal impurities and measure minority carrier life. MCLT until the predetermined value is reached.

Benefits of technology

By changing the inflow rate and time of the etching gas and silicon source gas, moisture and metal impurities in the reaction chamber can be removed faster, the time to reach the MCLT setting value can be shortened, and the production efficiency of the epitaxial wafer can be improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115747756B_ABST
    Figure CN115747756B_ABST
Patent Text Reader

Abstract

The present invention provides a method for restarting an epitaxial growth device, and belongs to the field of semiconductor manufacturing technology. The method for restarting an epitaxial growth device comprises: injecting hydrogen into a reaction chamber arranged in the epitaxial growth device and purging hydrogen for a predetermined time; placing a wafer on a susceptor inside the reaction chamber; introducing an etching gas into the reaction chamber at a first temperature, with a flow rate of 15SLM to 20SLM and a duration of 30 to 40s; introducing a silicon source gas into the reaction chamber at a second temperature, with a flow rate of 20SLM to 30SLM and a duration of 40 to 60s; measuring the minority carrier MCLT of the epitaxial wafer after growing the epitaxial wafer, and when the MCLT reaches a predetermined value, completing the restart of the epitaxial growth device. The technical solution of the present invention can improve the productivity of epitaxial wafers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of semiconductor manufacturing, and in particular to a method for restarting epitaxial growth equipment. Background Art

[0002] At present, epitaxial wafers play a pivotal role in the integrated circuit industry. The epitaxial growth process of silicon wafers is to perform CVD (chemical vapor deposition) on the surface of polished silicon wafers, using gaseous silicon compounds such as TCS (trichlorosilane) to react with hydrogen on the surface of the heated silicon substrate or undergo thermal decomposition to reduce to silicon, and then deposit it on the surface of the silicon substrate in the form of single crystals:

[0003] SiHCl3+H2→Si↓+3HCl

[0004] Compared with polished wafers, epitaxial wafers have lower oxygen content, carbon content, and defect density, can better control thickness and resistivity, have metal gettering and good conductivity, and are widely used in highly integrated IC devices.

[0005] During the epitaxial layer growth process, the cavity of the epitaxial growth equipment contains a large amount of moisture, including metal impurities generated when the epitaxial growth process is carried out at high temperature. If there are metal impurities in the chamber, the metal impurities occupy a certain energy level in the energy gap, and these energy levels will become the recombination centers of excessive carriers, thereby reducing the life span of minority carriers (Minority Carrier Life Time, MCLT), and epitaxial wafers that meet the requirements cannot be manufactured. Therefore, after the epitaxial growth is completed, preventive maintenance (PM) is required for the epitaxial growth equipment to meet the environment required for the next production. After PM, there will be residual moisture and metal impurities in the epitaxial equipment, and at this time, the epitaxial furnace needs to be restarted in order to manufacture epitaxial wafers.

[0006] When the epitaxial growth system is restarted, the wafer quality is ensured by repeating the ventilation, heating and stabilization steps in the chamber to execute the restart procedure. However, after the restart, there are still many metal contaminants in the thermally stable state in the epitaxial reaction chamber. In order to make the MCLT value of the epitaxial wafer obtained by the metal contamination test reach the set value, a sufficiently long time is required to bake the epitaxial reaction chamber and transfer the wafer, which will reduce the productivity of the epitaxial wafer. Summary of the invention

[0007] In order to solve the above technical problems, the present invention provides a method for restarting an epitaxial growth device, which can improve the productivity of epitaxial wafers.

[0008] In order to achieve the above object, the technical solution adopted in the embodiment of the present invention is:

[0009] A method for restarting an epitaxial growth device, comprising:

[0010] Injecting hydrogen into a reaction chamber disposed in the epitaxial growth device and purging the hydrogen for a predetermined time;

[0011] placing a wafer on a susceptor inside the reaction chamber;

[0012] Introduce etching gas into the reaction chamber at a first temperature with a flow rate of 15 SLM to 20 SLM for a duration of 30 to 40 seconds;

[0013] Introduce silicon source gas into the reaction chamber at a second temperature with a flow rate of 20 SLM to 30 SLM for a duration of 40 to 60 seconds;

[0014] After the epitaxial wafer is grown, the minority carrier MCLT of the epitaxial wafer is measured, and when the MCLT reaches a predetermined value, the epitaxial growth equipment is restarted.

[0015] In some embodiments, after placing the wafer on the susceptor inside the reaction chamber, the method further comprises:

[0016] The reaction chamber is heated to a predetermined first temperature and then the reaction chamber is stabilized.

[0017] In some embodiments, the first temperature is 1100°C-1200°C.

[0018] In some embodiments, the second temperature is 1075°C-1175°C.

[0019] In some embodiments, the silicon source gas is trichlorosilane gas;

[0020] The etching gas is HCL.

[0021] In some embodiments, measuring the MCLT of the epitaxial wafer after growing the epitaxial wafer further includes repeatedly performing the steps of removing the epitaxial wafer from the reaction chamber and cleaning the reaction chamber after manufacturing the epitaxial wafer until the MCLT reaches a predetermined value.

[0022] In some embodiments, the step of measuring the MCLT of the epitaxial wafer is performed when multiple runs are performed, wherein the process of manufacturing one epitaxial wafer is referred to as one run.

[0023] In some embodiments, epitaxial wafers corresponding to 50, 100, 150, 200, 250, 300, 350, and 400 runs were taken as sample wafers and the MCLT values ​​were measured.

[0024] The beneficial effects of the present invention are:

[0025] In this embodiment, by changing the flow rate and introduction time of the etching gas and the silicon source gas, moisture and metal impurities in the reaction chamber can be removed at a faster rate, so the time required to reach the MCLT setting value to perform the re-operation of the epitaxial growth equipment can be reduced, thereby improving the production efficiency of the epitaxial wafer. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 A schematic diagram showing a flow chart of a method for restarting an epitaxial growth device according to an embodiment of the present invention;

[0027] Figure 2 A schematic diagram showing the structure of an epitaxial growth device according to an embodiment of the present invention;

[0028] Figure 3 A schematic diagram showing the changes of MCLT in the reaction chamber when the epitaxial growth equipment is restarted;

[0029] Figure 4 A schematic diagram showing the temperature and time of each process during each operation when the epitaxial growth equipment is restarted. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical solution and advantages of the embodiment of the present invention clearer, the technical solution of the embodiment of the present invention will be clearly and completely described below in conjunction with the drawings of the embodiment of the present invention. Obviously, the described embodiment is a part of the embodiment of the present invention, not all of the embodiments. Based on the described embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present invention.

[0031] In the description of the present invention, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", and "third" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance.

[0032] In the related art, after the epitaxial growth equipment is restarted, the metal impurities remaining in the etching and thin film growth process cannot be effectively eliminated, thereby affecting the time required for MCLT to recover to the set value. The restart time of the epitaxial growth equipment is also affected, thereby affecting the production efficiency of the epitaxial wafer.

[0033] In order to solve the above technical problems, the present invention provides a method for restarting an epitaxial growth device, which can improve the productivity of epitaxial wafers.

[0034] The embodiment of the present invention provides a method for restarting an epitaxial growth device, such as Figure 1 As shown, including:

[0035] Step 101: injecting hydrogen into a reaction chamber disposed in the epitaxial growth device and purging the hydrogen for a predetermined time. Specifically, hydrogen may be continuously introduced into the reaction chamber during the entire restart process. Through the transport of hydrogen, moisture and substances in the reaction chamber may be more effectively discharged.

[0036] Step 102: placing a wafer on a susceptor inside the reaction chamber; introducing an etching gas into the reaction chamber at a first temperature with a flow rate of 15 SLM to 20 SLM and a duration of 30 to 40 seconds;

[0037] In some embodiments, the flow rate of the etching gas may be 15 SLM, 16 SLM, 17 SLM, 18 SLM, 19 SLM or 20 SLM. The duration of introducing the etching gas may be 30 s, 32 s, 34 s, 36 s, 38 s or 40 s.

[0038] Step 103: introducing silicon source gas into the reaction chamber at a second temperature with a flow rate of 20 SLM to 30 SLM and a duration of 40 to 60 seconds;

[0039] In some embodiments, the flow rate of the silicon source gas may be 20 SLM, 22 SLM, 24 SLM, 26 SLM, 28 SLM or 30 SLM. The duration of introducing the silicon source gas may be 40 s, 45 s, 50 s, 55 s, 58 s or 60 s.

[0040] Step 104: After growing the epitaxial wafer, the minority carrier MCLT of the epitaxial wafer is measured. When the MCLT reaches a predetermined value, the epitaxial growth equipment is restarted.

[0041] In this embodiment, by changing the flow rate and introduction time of the etching gas and the silicon source gas, moisture and metal impurities in the reaction chamber can be removed at a faster rate, so the time required to reach the MCLT setting value to perform the re-operation of the epitaxial growth equipment can be reduced, thereby improving the production efficiency of the epitaxial wafer.

[0042] like Figure 2 As shown, the epitaxial reaction device 100 of this embodiment includes a reaction chamber, and also includes: an air inlet 101, an air outlet 102, and a susceptor 103 located in the reaction chamber. The susceptor 103 is a part on which a wafer is mounted when performing an epitaxial process, and the susceptor 103 can be composed of a plate made of a material such as carbon graphite or silicon carbide. The susceptor 103 is supported by a spindle and a susceptor support member located at the bottom of the susceptor 103, and the susceptor support member is arranged at various positions of the spindle along the edge direction of the susceptor 103.

[0043] The epitaxial film is vapor-grown on the wafer at high temperature in the reaction chamber of the epitaxial reaction equipment. After the epitaxial film is grown on the wafer, an epitaxial wafer is obtained. If there are metal impurities or residual moisture in the reaction chamber, the manufactured epitaxial wafer is contaminated by the metal impurities, so the quality of the epitaxial wafer cannot be guaranteed.

[0044] Therefore, after performing each process, the reaction chamber performs preventive maintenance (PM), thereby generating residual moisture in the reaction chamber after the PM. The residual moisture may be removed by a process such as baking the inside of the chamber.

[0045] In some embodiments, after placing the wafer on the susceptor inside the reaction chamber, the method further comprises:

[0046] The reaction chamber is heated to a predetermined first temperature, and then the reaction chamber is stabilized, so that the reaction chamber can be baked, moisture in the reaction chamber can be removed, and the temperature of each position in the reaction chamber can be kept consistent, such as making the temperature of the lower part and the upper part of the base equal.

[0047] In some embodiments, the first temperature may be 1100° C.-1200° C. Specifically, the first temperature may be 1100° C., 1110° C., 1120° C., 1130° C., 1140° C., 1150° C., 1160° C., 1170° C., 1180° C., 1190° C. or 1200° C.

[0048] In this embodiment, the susceptor can be stabilized by etching the surface of the susceptor used to manufacture the epitaxial wafer and depositing a silicon film on the surface of the susceptor.

[0049] The susceptor contains moisture and contaminants on the surface in contact with the wafer after the high temperature process, so the susceptor surface needs to be stabilized to remove moisture, contaminants, metal substances and various residues.

[0050] In this embodiment, an etching gas may be introduced into the reaction chamber at a first temperature with a flow rate of 15 SLM to 20 SLM for a duration of 30 to 40 seconds to remove moisture, pollutants, metal substances and various residues on the susceptor. Thereafter, a silicon source gas may be introduced into the reaction chamber at a second temperature with a flow rate of 20 SLM to 30 SLM for a duration of 40 to 60 seconds to form a silicon film of a certain thickness on the susceptor, thereby stabilizing the susceptor.

[0051] In some embodiments, the second temperature may be 1075° C.-1175° C. Specifically, the second temperature may be 1075° C., 1085° C., 1095° C., 1105° C., 1115° C., 1125° C., 1135° C., 1145° C., 1155° C., 1165° C. or 1175° C.

[0052] In some embodiments, the silicon source gas may be trichlorosilane gas, and the etching gas may be HCL.

[0053] In some embodiments, measuring the MCLT of the epitaxial wafer after growing the epitaxial wafer further includes repeatedly performing the steps of removing the epitaxial wafer from the reaction chamber and cleaning the reaction chamber after manufacturing the epitaxial wafer until the MCLT reaches a predetermined value.

[0054] In some embodiments, the step of measuring the MCLT of the epitaxial wafer is performed when multiple runs are performed, wherein the process of manufacturing one epitaxial wafer is called one run. In this way, it can be determined whether the MCLT value of the epitaxial wafer reaches the set value.

[0055] In some embodiments, epitaxial wafers corresponding to 50, 100, 150, 200, 250, 300, 350, and 400 runs were taken as sample wafers and the MCLT values ​​were measured.

[0056] In some embodiments, when the MCLT reaches a predetermined value, the step of restarting the epitaxial growth apparatus is completed.

[0057] After the sample wafer with the epitaxial film formed thereon is removed from the reaction chamber, a process of removing the natural oxide film by hydrofluoric acid treatment is performed. In addition, iodine is thinly deposited on the epitaxial wafer, and then the surface of the epitaxial wafer is scanned to measure the MCLT level.

[0058] Minority carrier lifetime (MCLT) can be a metric to determine the readiness of a system to restart epitaxial growth. MCLT refers to the average time required for excess minority electrons to recombine, and the more impurities in the reaction chamber, the lower the MCLT.

[0059] Therefore, the MCLT of the sample wafers corresponding to 50, 100, 150, 200, 250, 300, 350 and 400 runs is measured, and when the MCLT satisfies the predetermined value, it can be determined that the preparation for restarting the epitaxial growth system is completed. When the MCLT value does not meet the predetermined value, multiple runs are continued.

[0060] In one embodiment, when MCLT reaches a predetermined value, the restart procedure of the epitaxial growth system is completed, and the predetermined value can be set to 2800us, which means that the contaminants such as metal particles in the reaction chamber are almost all removed and do not affect the quality of the epitaxial wafers subsequently manufactured.

[0061] In a specific example, the epitaxial growth equipment restart method includes the following steps:

[0062] Step S1, introducing hydrogen into the upper chamber and the lower chamber of the reaction chamber for a duration of the entire process;

[0063] Step S2, placing the wafer on the base of the reaction chamber, and heating the reaction chamber to 1180° C.;

[0064] Step S3, executing the reaction chamber baking process, the baking temperature is set to 1180° C., and the duration is 65 seconds;

[0065] Step S4, performing a surface etching process, introducing etching gas HCL into the reaction chamber, with a flow rate of 15SLM-20SLM, a duration of 30-40s, and a temperature set to 1180°C;

[0066] Step S5, executing a thin film growth process, introducing silicon source gas TCS into the reaction chamber, with a flow rate of 20 SLM to 30 SLM, a duration of 40 to 60 seconds, and a temperature set to 1125° C.;

[0067] Step S6, manufacturing epitaxial wafers, measuring the MCLT values ​​of epitaxial wafers corresponding to 50, 100, 150, 200, 250, 300, 350 and 400 runs, if the MCLT value meets the set value, it can be considered that the epitaxial furnace restart process is completed. If the MCLT value does not meet the set value, it is necessary to repeat the process of S1 to S6 to ensure the MCLT value required when the epitaxial furnace is restarted.

[0068] Figure 3 The figure shows the change of MCLT level inside the reaction chamber when the epitaxial furnace is prepared for restarting in the prior art and the embodiment of the present invention. It can be seen that in the prior art, the MCLT value of the epitaxial wafer is less than 500us for 50 runs; the MCLT value of the epitaxial wafer is less than 1500us for 100 runs; the MCLT value of the epitaxial wafer is about 1600us for 200 runs; the MCLT value of the epitaxial wafer is less than 2000us for 250 runs; the MCLT value of the epitaxial wafer is less than 2500us for 300 runs; the MCLT value of the epitaxial wafer is about 2700us for 350 runs; and the MCLT value of the epitaxial wafer is about 2800us for 400 runs. After adopting the technical solution of this embodiment, corresponding to 50 runs, the MCLT value of the epitaxial wafer is greater than 500us; corresponding to 100 runs, the MCLT value of the epitaxial wafer is greater than 2000us; corresponding to 200 runs, the MCLT value of the epitaxial wafer is approximately 3000us; corresponding to 250 runs, the MCLT value of the epitaxial wafer is greater than 3000us; corresponding to 300 runs, the MCLT value of the epitaxial wafer is approximately 3100us.

[0069] Compared with the prior art, this embodiment can effectively shorten the time for the reaction chamber MCLT to reach the set value by designing the flow rate and time of the etching gas HCL and the silicon source gas TCS. If the above operation is not performed, the MCLT reaches about 2800us at about 400Runs, and the epitaxial furnace meets the restart condition. However, if the above operation of this embodiment is performed, the MCLT can reach about 3000us at about 200Runs, which greatly shortens the restart time of the epitaxial furnace.

[0070] Figure 4 The figure shows the time and temperature required for each process when the epitaxial furnace of this embodiment is restarted, and each operation is completed. It can be seen that the embodiment completes one operation in about 330 seconds, which can greatly shorten the time for restarting the epitaxial furnace.

[0071] It should be noted that, in this article, the terms "comprise", "include" or any other variant thereof are intended to cover non-exclusive inclusion, so that the process, method, article or device including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise one..." do not exclude the presence of other identical elements in the process, method, article or device including the element. In addition, it should be pointed out that the scope of the methods and devices in the embodiments of the present application is not limited to performing functions in the order shown or discussed, and may also include performing functions in a substantially simultaneous manner or in reverse order according to the functions involved, for example, the described method may be performed in an order different from that described, and various steps may also be added, omitted, or combined. In addition, the features described with reference to certain examples may be combined in other examples.

[0072] The embodiments of the present application are described above in conjunction with the accompanying drawings, but the present application is not limited to the above-mentioned specific implementation methods. The above-mentioned specific implementation methods are merely illustrative and not restrictive. Under the guidance of the present application, ordinary technicians in this field can also make many forms without departing from the purpose of the present application and the scope of protection of the claims, all of which are within the protection of the present application.

Claims

1. A method for restarting an epitaxial growth device, It is characterized in that include: Injecting hydrogen into a reaction chamber disposed in the epitaxial growth device and purging the hydrogen for a predetermined time; placing a wafer on a susceptor inside the reaction chamber; Introducing an etching gas into the reaction chamber at a first temperature with a flow rate of 15 SLM to 20 SLM for a duration of 30 to 40 seconds, etching the base in the reaction chamber to remove moisture, pollutants, metal substances and various residues on the base; At a second temperature, silicon source gas is introduced into the reaction chamber at a flow rate of 20 SLM to 30 SLM for a duration of 40 to 60 seconds to form a silicon film on the base; After the epitaxial wafer is grown, the minority carrier MCLT of the epitaxial wafer is measured, and when the MCLT reaches a predetermined value, the epitaxial growth equipment is restarted.

2. The epitaxial growth equipment restart method according to claim 1, It is characterized in that After placing the wafer on the susceptor inside the reaction chamber, the method further includes: The reaction chamber is heated to a predetermined first temperature and then the reaction chamber is stabilized.

3. The method for restarting the epitaxial growth device according to claim 1 or 2, It is characterized in that The first temperature is 1100°C-1200°C.

4. The epitaxial growth equipment restart method according to claim 1, It is characterized in that The second temperature is 1075°C-1175°C.

5. The epitaxial growth equipment restart method according to claim 1, It is characterized in that The silicon source gas is trichlorosilane gas; The etching gas is HCL.

6. The epitaxial growth equipment restart method according to claim 1, It is characterized in that The step of measuring the MCLT of the epitaxial wafer after growing the epitaxial wafer further includes repeatedly performing the steps of removing the epitaxial wafer from the reaction chamber and cleaning the reaction chamber after manufacturing the epitaxial wafer until the MCLT reaches a predetermined value.

7. The epitaxial growth equipment restart method according to claim 1, It is characterized in that The step of measuring the MCLT of the epitaxial wafer is performed while a plurality of runs are performed, wherein the process of manufacturing one epitaxial wafer is referred to as one run.

8. The epitaxial growth equipment restart method according to claim 7, It is characterized in that Epitaxial wafers corresponding to 50, 100, 150, 200, 250, 300, 350 and 400 runs were taken as sample wafers and the MCLT values ​​were measured.