A method for preparing high-strength graphene material
Through metal ion solution swelling and coordination crosslinking treatment, combined with chemical reduction, the problem of structural defects in graphene fibers and membranes is solved, and its mechanical properties are significantly improved, achieving high-strength and high elasticity graphene material preparation.
Patent Information
- Application Number
- CN202211461157.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-21
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-11-21
AI Technical Summary
There are structural defects in the existing graphene fiber and membrane preparation methods, such as irregular folds and pores, which affect their mechanical properties, making it difficult to completely eliminate micron folds, hindering the transmission of excellent performance of two-dimensional graphene sheets to macroscopic materials.
The graphene oxide was swelled by metal ion solution, and the interlayer force and orientation degree were enhanced by coordination cross-linking. Combined with chemical reduction treatment, the interlayer slip and micro-wrinkles were reduced, and graphite with high orientation and regular structure was obtained. ene material.
The modulus and elastic properties of graphene materials are significantly improved, and their ability to withstand tensile loads is enhanced, achieving excellent performance of high strength and high elasticity.
Smart Images

Figure CN115748234B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of nano materials, and in particular to a method for preparing a high-strength graphene material. Background Art
[0002] In 2004, Andre Geim and Konstantin Novoselov, physicists at the University of Manchester in the UK, successfully separated graphene from graphite using a micromechanical exfoliation method. Graphene is a two-dimensional single-atomic layer honeycomb periodic lattice structure crystal composed of carbon atoms in sp2 hybrid orbitals, with a thickness of only 0.35nm. The unique structure of graphene gives it excellent properties, including excellent mechanical properties, large specific surface area, large carrier mobility, and extremely high thermal conductivity. Graphene fibers assembled from graphene nanosheets can realize the transfer of graphene's excellent properties at the nanoscale to the macroscale. With the gradual optimization of the material system and the improvement of the preparation process, graphene fibers are expected to develop into fiber materials with integrated structure and function and be applied in a wider range of fields.
[0003] As an important derivative of graphene, graphene oxide has attracted the attention of the industry due to its easy large-scale preparation and unique solution processability. In 2011, Professor Gao Chao's team at Zhejiang University prepared graphene oxide fibers by wet spinning based on the lyotropic liquid crystal phenomenon of graphene oxide. At present, wet spinning has become the most commonly used method for preparing graphene fibers due to its simple operation, high efficiency, and scalability. However, the primary fibers obtained by liquid crystal wet spinning will inevitably introduce structural defects such as irregular wrinkles during the coagulation stage. Large-sized wrinkles in the fibers are prone to stress concentration during the stretching process, while small-sized wrinkles are numerous and of different sizes, which are often difficult to control. In the past, under the weak plasticization system, the interlayer spacing of graphene oxide was limited, and the deformation ability under stress was weak, making it difficult to completely eliminate micron-level wrinkles. These structural defects will always exist inside the fiber, and will eventually be inherited to the graphene fiber after chemical reduction and heat treatment, which greatly affects the comprehensive performance of graphene fiber materials. In addition, for graphene oxide membranes, most of the existing methods are based on scraping and filtration. These two methods will cause a large number of wrinkles and pores on the surface and inside of the membrane, which will damage its mechanical properties. This is a major problem that hinders the transfer of the excellent properties of two-dimensional graphene sheets to macroscopic materials. Summary of the invention
[0004] In order to overcome the above-mentioned existing technical defects, the purpose of the present invention is to provide a method for preparing a high-strength graphene material. The present invention is based on the swelling of graphene oxide by metal ion solution and provides coordination cross-linking to greatly enhance the interlayer force and orientation, thereby obtaining a highly oriented graphene oxide material with few wrinkles; further, a high-performance graphene functional material with uniform wrinkles is obtained through chemical reduction post-treatment.
[0005] The present invention adopts the following technical scheme: a method for preparing graphene oxide material, comprising the following process: placing a macroscopic graphene oxide material in a metal salt solution for immersion treatment for 1 to 5 seconds and then stretching it to obtain a graphene oxide hydrogel; wherein the concentration of the metal salt is 0.2 to 2 mol / L, and the solvent of the metal salt can be water, acetic acid, ethanol, methanol, isopropanol, ethylene glycol, propylene glycol, glycerol, triethylene glycol, tetraethylene glycol, pentaethylene glycol or other mixed solvents; the stretching rate is 40-60%, and the stretching is continued for 3-5 seconds to keep the oxide The graphene sheets are arranged straight; in this step, a uniform external force is maintained to keep the graphene sheets arranged straight, and the interlayer spacing is reduced. At the same time, the metal ions in the plasticizing bath will coordinate and cross-link the carboxyl functional groups on the upper edges of the graphene oxide sheets, transforming the viscous slip flow structure into an elastic structure, greatly reducing the interlayer slip, thereby providing a stronger interlayer force, and giving the graphene oxide sheets the ability to withstand a larger load; under large load stretching, the micro-wrinkles of the graphene sheets are stretched, and the graphene sheets are arranged straight, and after drying, a wrinkle-free graphene oxide material is obtained.
[0006] Furthermore, in step (1), the metal salt is calcium chloride, magnesium chloride, copper sulfate, ferric chloride, aluminum chloride, etc. The metal salt provides coordination and cross-linking effects between graphene oxide sheets.
[0007] The graphene oxide macroscopic material of the present invention is graphene oxide fiber (not limited to graphene oxide fiber monofilament, but also can be used for graphene oxide fiber bundle) and graphene oxide film.
[0008] Furthermore, the stretching bath has a polarity at least greater than that of ethyl acetate, including but not limited to acetic acid, ethanol, methanol, isopropanol, ethylene glycol, propylene glycol, glycerol, triethylene glycol, tetraethylene glycol, pentaethylene glycol or other mixed solvents.
[0009] Furthermore, the method further comprises subjecting the wrinkled graphene oxide material to a reduction treatment, wherein the reduction is a chemical reduction, and the reagents used for the chemical reduction are hydroiodic acid, hydrazine hydrate, sodium ascorbate, stannous chloride, and the like.
[0010] The beneficial effect of the present invention is that the graphene oxide hydrogel is plasticized and stretched in a plasticizing bath containing metal ions. Based on the coordination and crosslinking characteristics of the metal salt between the graphene oxide sheets, the metal salt can coordinate and crosslink with the carboxyl functional groups at the edges of the graphene oxide sheets, thereby enhancing the interlayer force, so that the internal sheets can withstand a large tensile load so that the graphene oxide sheets are arranged straight, and a highly oriented and regularly micro-wrinkled structure is obtained, thereby giving it excellent properties of high modulus and high elasticity. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Figure 1 It is the SEM and the comparison of strength and modulus of the products of Example 1 and Comparative Example 1, a1 and a2 are the surface and cross-section of the graphene fiber in Example 1, respectively; b1 and b2 are the surface and cross-section of the graphene fiber in Comparative Example 1, respectively; the left dotted line in c represents the strength comparison of the graphene fibers of Example 1 and Comparative Example 1, and the right dotted line in c represents the modulus comparison of the graphene fibers of Example 1 and Comparative Example 1.
[0012] Figure 2 This is a SEM comparison of the products of Example 2 and Comparative Example 2, where a is the surface of the graphene fiber bundle in Example 2; b is the surface of the graphene fiber bundle in Comparative Example 2.
[0013] Figure 3 The SEM and strength comparison of the products of Example 3 and Comparative Example 3, a1 and a2 are the surface and fracture surface of the graphene film in Example 3, respectively; b1 and b2 are the surface and fracture surface of the graphene film in Comparative Example 3, respectively; c is the graphene film (GP-Ca) of Example 3 2+ ) and the strength of graphene films (GP-Ethanol);
[0014] Figure 4 This is a comparison of the maximum elongation of graphene oxide fibers by ions in different plasticizing baths in Example 4, where the ordinate is the elongation. DETAILED DESCRIPTION
[0015] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation mode, structure, characteristics and effects of the present invention are described in detail below in combination with the accompanying drawings and preferred embodiments.
[0016] Embodiment 1:
[0017] (1) extruding 8 mg / g DMF-phase graphene oxide spinning solution into an ethyl acetate coagulation bath, and obtaining primary graphene oxide fibers through wet liquid crystal spinning;
[0018] (2) immersing the primary graphene oxide fiber in step 1 in a 1M CaCl2 solution (the solvent is water and ethanol in a volume ratio of 1:1) and plasticizing it for 1 second. At this stage, the interlayer spacing of the graphene oxide sheets increases to 2.1 nm;
[0019] (3) stretching the graphene oxide fiber in step 2 with a stretching rate of 55% and maintaining the stretching for 5 seconds;
[0020] (4) The graphene oxide fiber after plasticization and stretching in step 3 is immersed in a water bath containing water and ethanol in a volume ratio of 3:1 to perform Ca 2+ The fiber is washed and removed. During this stage, the fiber needs to maintain its original tension;
[0021] (5) The washed graphene oxide fiber in step 4 is heat-set and subjected to a fumigation reduction treatment at 85° C. with hydroiodic acid and acetic acid (1:3) to obtain a high-strength graphene fiber.
[0022] After mechanical testing, the strength of the graphene fiber reached 1.82GPa.
[0023] Comparative Example 1
[0024] (1) extruding 8 mg / g DMF-phase graphene oxide spinning solution into an ethyl acetate coagulation bath, and obtaining primary graphene oxide fibers through wet liquid crystal spinning;
[0025] (2) immersing the primary graphene oxide fiber in step 1 in a solution of water and ethanol in a volume ratio of 1:1 and plasticizing it for 1 second. At this stage, the interlayer spacing of the graphene oxide sheets increases to 1.5 nm;
[0026] (3) stretching the graphene oxide fiber in step 2 with a maximum stretching rate of 20% and maintaining the stretching for 5 seconds;
[0027] (4) The graphene oxide fiber in step 3 is heat-set, and then subjected to a fumigation reduction treatment at 85° C. with hydroiodic acid and acetic acid (1:3) to obtain graphene fiber.
[0028] After mechanical testing, the strength of the graphene fiber reached 0.78GPa.
[0029] The SEM images of the products of Example 1 and Comparative Example 1 are shown in Figure 1 a1~a2 and b1~b2. It can be seen from the figure that as the stretching rate increases, the wrinkles on the fiber surface become smoother, the cross section becomes denser and more regular, and it has a very excellent effect on mechanical conduction. The mechanical properties diagrams are shown in Figure 1 c. It can be seen from the figure that the strength of the ion-crosslinked graphene fiber is increased by 133% and the modulus is increased by 192% compared with the uncrosslinked graphene fiber.
[0030] Embodiment 2:
[0031] (1) extruding a 20 mg / g DMF-phase graphene oxide spinning solution through a spinneret with 100 holes and a pore size of 120 μm into an ethyl acetate coagulation bath, and obtaining a primary graphene oxide fiber bundle by wet liquid crystal spinning;
[0032] (2) pulling 100 graphene oxide fiber bundles in step 1 into a 2M MgCl2 solution (the solvent is water and ethanol in a volume ratio of 1:1) and soaking for 5 seconds to allow the fiber bundles to swell and crosslink;
[0033] (3) performing positive stretching on the graphene oxide fiber tow in step 2, with a stretching rate of 10%, and maintaining the stretching for 5 seconds;
[0034] (4) The graphene oxide fiber tow in step 3 is pulled out and immersed in a water bath containing water and ethanol in a volume ratio of 3:1 to clean the surface of the graphene oxide fiber. 2+ The fiber is washed and removed. During this stage, the fiber needs to maintain its original tension;
[0035] (5) The graphene oxide fiber bundles prepared in step 4 are dried, collected and chemically reduced to obtain uniformly oriented graphene fiber bundles.
[0036] Comparative Example 2:
[0037] (1) extruding a 20 mg / g DMF-phase graphene oxide spinning solution through a spinneret with 100 holes and a pore size of 120 μm into an ethyl acetate coagulation bath, and obtaining a primary graphene oxide fiber bundle by wet liquid crystal spinning;
[0038] (2) pulling the 100 graphene oxide fiber bundles in step 1 into a solution having a volume ratio of water to ethanol of 1:1 and soaking them for 5 seconds to allow the fiber bundles to swell;
[0039] (3) performing positive stretching on the graphene oxide fiber bundle in step 2, with a stretching rate of 5%, and maintaining the stretching for 5 seconds;
[0040] (5) The graphene oxide fiber bundle in step 3 is dried, collected and chemically reduced to obtain a graphene fiber bundle.
[0041] The SEM images of the products of Example 2 and Comparative Example 2 are shown in Figure 2 a and 2b. It can be seen from the figures that the surface of the cross-linked graphene fiber bundle is more uniform, with fewer defects, and thus has better strength.
[0042] Embodiment 3:
[0043] (1) obtaining a graphene oxide film by a film laying and drying method, and cutting the film into strips with a length of 10 mm and a width of 4 mm;
[0044] (2) immersing the graphene oxide film in step 1 into a 2M AlCl3 solution (the solvent is: water and ethanol in a volume ratio of 1:1) for 2 seconds to allow the solution to fully penetrate into the interlayer of the graphene oxide macrofilm;
[0045] (3) applying axial tension to both ends of the swollen graphene oxide film in step 2, and under the action of the above-mentioned plasticizing stretching bath, the graphene oxide macroscopic film material has a stretching rate of 13%;
[0046] (4) The graphene oxide macro-membrane material stretched in step 3 is fixed and washed with water and ethanol in a volume ratio of 3:1 to remove Al 3+ The membrane is removed by washing, during which the membrane is always in a taut state, and then dried naturally. During the drying process, external force is applied to maintain the current length;
[0047] (5) The film of step 4 is chemically reduced with hydroiodic acid and ethanol (1:3) to obtain a high-strength graphene film.
[0048] After mechanical properties testing, the strength of the cross-linked graphene film reached 843Mpa.
[0049] Comparative Example 3:
[0050] (1) obtaining a graphene oxide film by a film laying and drying method, and cutting the film into strips with a length of 10 mm and a width of 4 mm;
[0051] (2) immersing the graphene oxide film in step 1 in a plasticizing stretching bath of a solution of water and ethanol in a volume ratio of 1:1 for 2 seconds, so that the solution fully penetrates into the interlayer of the graphene oxide macrofilm;
[0052] (3) applying axial tension to both ends of the swollen graphene oxide film in step 2, and under the action of the above-mentioned plasticizing stretching bath, the graphene oxide macroscopic film material has a stretching rate of 7%;
[0053] (4) The graphene oxide macro-membrane material stretched in step 3 is chemically reduced with hydroiodic acid and ethanol (1:3) to obtain a high-strength graphene film.
[0054] After mechanical properties testing, the strength of the cross-linked graphene film reached 468MPa.
[0055] The SEM images of the products of Example 3 and Comparative Example 3 are shown in Figure 3a1~a2 and b1~b2. It can be seen from the figure that as the stretching rate increases, the random wrinkles on the surface of the graphene film are further eliminated, and it has two important characteristics of plastic fracture, namely, fibrous plastic orientation and nearly 45° shear deformation, which has a very excellent effect on mechanical conduction. The mechanical properties diagrams are shown in Figure 3 c. It can be seen from the figure that the strength of the graphene film after ion cross-linking is increased by 80% compared with the non-cross-linked graphene film.
[0056] Embodiment 4:
[0057] (1) extruding 8 mg / g DMF-phase graphene oxide spinning solution into an ethyl acetate coagulation bath, and obtaining primary graphene oxide fibers through wet liquid crystal spinning;
[0058] (2) The primary graphene oxide fibers in step 1 were immersed in 0.2M FeCl3 solution (the solvent was water and ethanol in a volume ratio of 1:3), 1M AlCl3 solution (the solvent was water and ethanol in a volume ratio of 1:1), 0.5M CuSO4 solution (the solvent was water and ethanol in a volume ratio of 1:3), 2M MgCl2 solution (the solvent was water and ethanol in a volume ratio of 1:1), and 1M CaCl2 solution (the solvent was water and ethanol in a volume ratio of 1:1) and plasticized for 1s.
[0059] (3) stretching the graphene oxide fibers in different plasticizing baths in step 2, with maximum stretching rates reaching 20%, 30%, 33%, 35% and 55%, respectively, and maintaining the stretching for 5 seconds;
[0060] (4) immersing the graphene oxide fiber after plasticization and stretching in step 3 in a water bath containing water and ethanol in a volume ratio of 3:1 to wash and remove metal ions on the surface of the graphene oxide fiber. At this stage, the fiber needs to maintain its original tension;
[0061] (5) The washed graphene oxide fiber in step 4 is heat-set and subjected to a fumigation reduction treatment at 85° C. with hydroiodic acid and acetic acid (1:3) to obtain a high-strength graphene fiber.
[0062] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A method for preparing a high-strength graphene material, characterized in that: The process includes: (1) placing a graphene oxide macroscopic material in a metal salt solution for 1 to 5 seconds of immersion treatment and then stretching treatment to obtain a graphene oxide hydrogel; wherein the concentration of the metal salt is 0.2 to 2 mol / L, and the solvent of the metal salt is a polar solvent; the stretching rate is 20-60%, and the stretching is continued for 3-5 seconds to keep the graphene oxide sheets arranged straight; the metal salt is Ca 2+ Mg 2+ , Cu 2+ , Fe 3+ 、Al 3+ The graphene oxide macroscopic material is graphene oxide fiber or graphene oxide film; (2) After drying, a de-wrinkled graphene oxide material is obtained.
2. The preparation method according to claim 1, characterized in that: The solvent used in the metal salt solution is one of acetic acid, ethanol, methanol, isopropanol, ethylene glycol, propylene glycol, glycerol, triethylene glycol, tetraethylene glycol, pentaethylene glycol or a mixed solvent thereof.
3. The preparation method according to any one of claims 1 to 2, characterized in that: The method also includes subjecting the de-wrinkled graphene oxide material to a reduction treatment.