Conductive copper paste for solar cells capable of being sprayed by aerosol and preparation method thereof

By adjusting the distribution ratio and process flow of conductive copper paste, especially the application of diluted atomizer, the aerosol performance and adhesion strength problems of conductive copper paste in aerosol spraying process are solved, and efficient spraying effect is achieved and Simplify the process.

CN115762849BActive Publication Date: 2024-11-26韩亚半导体材料(贵溪)有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211416928.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-14
Publication Date
2024-11-26
Estimated Expiration
2042-11-14

AI Technical Summary

Technical Problem

The existing conductive copper slurry has poor aerosol performance in the aerosol spraying process, resulting in poor spraying effect, and low conductivity and adhesion strength, which increases the difficulty of the process.

Method used

Through the adjustment of the component distribution ratio in the preparation method and the optimization of process flow, especially the preparation and application of dilution atomizer, as well as the treatment of copper powder and glass powder, conductive copper slurry with good aerosolization performance and high adhesion strength are formed. .

Benefits of technology

The excellent aerosol atomization performance, high conductivity and high adhesion strength of conductive copper paste are achieved, the spraying process and preparation process are simplified, and the aerosol spraying effect is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115762849B_ABST
    Figure CN115762849B_ABST
Patent Text Reader

Abstract

The present invention is applicable to the technical field of conductive pastes, and provides a conductive copper paste for solar cells that can be sprayed by aerosol and a preparation method thereof. The conductive paste comprises spherical copper powder, glass powder, organic solvent, thickener, coupling agent, dispersant, defoaming agent and diluent atomizer, and is matched with a specific component ratio and a preparation process flow to finally prepare a conductive copper paste having the advantages of excellent aerosolization performance, high conductivity, high adhesion strength, simple spraying process, simple preparation process, etc., so that the requirements of the aerosol spraying process can be well met in the end.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of conductive pastes, and specifically provides a conductive copper paste for solar cells that can be sprayed by aerosols and a preparation method thereof for an aerosol spraying process. Background Art

[0002] In crystalline silicon solar cells, conductive silver paste is widely used in positive electrode materials. However, as the price of silver continues to rise, the cost of conductive silver paste also continues to rise. In addition, the problem of electron migration in metallic silver makes the performance of silver paste unstable. Copper has no electron migration and also has good conductivity. Therefore, copper paste is regarded as a new material that can replace conductive silver paste for solar cells, making the research on conductive copper paste very valuable.

[0003] Aerosol spraying technology has excellent performance, high degree of equipment automation, suitable for long-term work, conducive to industrial application, high printing resolution, low ink requirements, and has been widely used. Therefore, the feasibility of applying conductive copper paste in aerosol spraying technology has been gradually studied.

[0004] However, when the current conductive copper paste is used in the aerosol spraying process, its atomization performance is poor, which affects the final spraying effect. At the same time, the conductivity and adhesion strength of the paste are relatively low, which will increase the difficulty of the spraying process. Summary of the invention

[0005] The purpose of the embodiments of the present invention is to provide a conductive copper paste for solar cells that can be sprayed by aerosol and a preparation method thereof, aiming to solve the problem of atomization of the conductive copper paste for solar cells in the aerosol spraying process.

[0006] The present invention is achieved by a method for preparing a conductive copper paste for solar cells that can be sprayed by aerosol, comprising the following steps:

[0007] Step 1: Take a certain amount of organic solvent, thickener, coupling agent, dispersant and defoamer into a beaker, and heat them at a constant temperature of 80° C. in a water bath until they are completely dissolved to prepare an organic carrier as a non-conductive phase for standby use;

[0008] Step 2: Put anhydrous formic acid and anhydrous ethanol in a certain mass ratio into a beaker and mix them evenly to prepare dilute formic acid;

[0009] Step 3: Take a certain amount of commercial spherical copper powder and the dilute formic acid in step 2 and put them into a beaker, stir and centrifuge to wash until the supernatant is colorless and the pH value is neutral, then put the washed copper micron particles into a vacuum drying oven at 50°C to dry, and put the dried copper micron particles into an agate mortar for grinding and dispersion for later use;

[0010] Step 4: Take a certain proportion of commercial Bi2O3-B2O3-ZnO glass powder and the spherical copper powder treated in step 3 and place them in a beaker, add an appropriate amount of anhydrous ethanol, stir by ultrasonic, and dry in a vacuum drying oven at 50°C to obtain a uniformly mixed powder;

[0011] Step 5: Take a certain proportion of the non-conductive phase in step 1 and mix it with the powder in step 4 to prepare a primary copper slurry;

[0012] Step 6: Mix a certain proportion of anhydrous ethanol and acetone with the powder of hexadecyltrimethylammonium bromide to prepare a diluted atomizer;

[0013] Step 7: within half an hour before aerosol spraying, add a certain proportion of the diluting atomizer of step 6 to the primary copper paste of step 5 and mix thoroughly to obtain a conductive copper paste for solar cells that can be sprayed by aerosol.

[0014] In a preferred technical solution, in step 1, the organic solvent is terpineol, the thickener is ethyl cellulose, the coupling agent is KH-570 silane coupling agent, and the dispersant is ethyl acetate.

[0015] In a preferred technical solution, the total weight of the organic solvent is used as the basis in step 1, wherein the mass percentages of the raw materials are 76wt%-88wt% of the organic solvent, 0wt%-12wt% of the thickener, 3wt% of the coupling agent, 6wt% of the dispersant, and 3wt% of the defoaming agent.

[0016] In a preferred technical solution, the mass ratio of anhydrous formic acid to anhydrous ethanol in step 2 is 1:39.

[0017] In a preferred technical solution, the commercial spherical copper powder in step three has an average particle size of 1 μm.

[0018] In a preferred technical solution, the mass ratio of the commercial spherical copper powder in step three to the dilute formic acid in step two is 1:10.

[0019] In a preferred technical solution, the mass ratio of the spherical copper powder and the glass powder after treatment in step 4 is 22-24:1-3.

[0020] In a preferred technical solution, the mass ratio of the non-conductive phase to the powder in step five is 1:1.

[0021] In a preferred technical solution, the total weight of the diluted atomizer is used as a reference in step six, wherein the mass percentages of the raw materials are 85wt%-97wt% for liquid and 3wt%-15wt% for powder.

[0022] In a preferred technical solution, the mass ratio of anhydrous ethanol to acetone in step six is ​​3:1.

[0023] In a preferred technical solution, the mass ratio of the primary copper slurry to the diluent atomizer in step seven is 1:5.

[0024] Another aspect of the present invention further provides a conductive copper paste for solar cells that can be sprayed by aerosol, which is prepared by any of the above-mentioned methods for preparing a conductive copper paste for solar cells that can be sprayed by aerosol.

[0025] The method for preparing a conductive copper paste for solar cells that can be aerosol-sprayed provided in the embodiment of the present invention studies the components of the conductive copper paste, different proportions of each component, especially the preparation of a diluting atomizer and its application in the overall conductive copper paste preparation system, and the influence of the preparation process on the performance of the conductive copper paste that can be atomized and aerosol-sprayed. The conductive copper paste finally prepared has the advantages of excellent aerosolization performance, high conductivity and high adhesion strength, and achieves the purposes of simple spraying process, simple preparation process, and good aerosol spraying effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 A graph showing the result of spraying a conductive copper paste sample for solar cells using an aerosol sprayable method according to an embodiment of the present invention once. DETAILED DESCRIPTION

[0027] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific implementation cases described herein are only used to explain the present invention and are not used to limit the present invention.

[0028] In order to solve the problem that the current conductive copper paste has poor atomization performance when used in the aerosol spraying process, which affects the final spraying effect, and the conductivity and adhesion strength of the slurry are also relatively low, which will increase the difficulty of the spraying process. The present invention proposes a conductive copper paste for solar cells that can be aerosol sprayed and a preparation method thereof, so as to study the influence of the conductive copper paste components, different proportions of each component, and the preparation process on the performance of the conductive copper paste that can be atomized and sprayed by aerosol, so as to prepare a conductive copper paste with excellent atomization performance, high conductivity, high adhesion strength, simple spraying process, simple preparation process and the like, so that it can finally meet the requirements of the aerosol spraying process. The technical solution of the present invention is as follows:

[0029] A method for preparing a conductive copper paste for solar cells that can be sprayed by aerosol, comprising the following steps:

[0030] Step 1: Take a certain amount of organic solvent, thickener, coupling agent, dispersant and defoamer into a beaker, and heat them at a constant temperature of 80° C. in a water bath until they are completely dissolved to prepare an organic carrier as a non-conductive phase for standby use;

[0031] Step 2: Put anhydrous formic acid and anhydrous ethanol in a certain mass ratio into a beaker and mix them evenly to prepare dilute formic acid;

[0032] Step 3: taking a certain amount of commercial spherical copper powder and the dilute formic acid in step 2 and putting them into a beaker, stirring and centrifuging and washing them until the supernatant is colorless and the pH value is neutral, and then obtaining copper micron particles after washing, and then drying the washed copper micron particles in a vacuum drying oven at 50° C., and grinding and dispersing the dried copper micron particles in an agate mortar to obtain the treated spherical copper powder for later use;

[0033] Step 4: Take a certain proportion of commercial Bi2O3-B2O3-ZnO glass powder and the spherical copper powder treated in step 3 and place them in a beaker, add an appropriate amount of anhydrous ethanol, stir by ultrasonic, and dry in a vacuum drying oven at 50°C to obtain a uniformly mixed powder;

[0034] Step 5: Take a certain proportion of the non-conductive phase in step 1 and mix it with the powder in step 4 to prepare a primary copper slurry;

[0035] Step 6: Mix a certain proportion of anhydrous ethanol and acetone with the powder of hexadecyltrimethylammonium bromide to prepare a diluted atomizer;

[0036] Step 7: within half an hour before aerosol spraying, add a certain proportion of the diluting atomizer of step 6 to the primary copper paste of step 5 and mix thoroughly to obtain a conductive copper paste for solar cells that can be sprayed by aerosol.

[0037] During specific use, the required graphics can be drawn on the control panel of the aerosol spray printer, and the conductive copper paste prepared in step seven is placed in the atomization bottle of the aerosol spray printer. By adjusting the carrier gas, good atomization can be achieved, thereby realizing the desired graphic effect of automatic printing.

[0038] Preferably, in step 1, the organic solvent is terpineol, the thickener is ethyl cellulose, the coupling agent is KH-570 silane coupling agent, and the dispersant is ethyl acetate.

[0039] Preferably, in step 1, the total weight of the organic solvent is used as a reference, wherein the mass percentages of the raw materials are 76wt%-88wt% of the organic solvent, 0wt%-12wt% of the thickener, 3wt% of the coupling agent, 6wt% of the dispersant, and 3wt% of the defoaming agent.

[0040] Preferably, in step 2, the mass ratio of anhydrous formic acid to anhydrous ethanol is 1:39.

[0041] Preferably, the commercial spherical copper powder in step 3 has an average particle size of 1 μm.

[0042] Preferably, the mass ratio of the commercial spherical copper powder in step 3 to the dilute formic acid in step 4 is 1:10.

[0043] Preferably, the mass ratio of the spherical copper powder and the glass powder after treatment in step 4 is 22-24:1-3;

[0044] Preferably, in the step five, the mass ratio of the non-conductive phase to the powder is 1:1, in the step six, the mass ratio of anhydrous ethanol to acetone is 3:1, and in the step seven, the mass ratio of the primary copper slurry to the diluting atomizer is 1:5.

[0045] Preferably, in step six, the total weight of the diluted atomizer is used as a reference, wherein the mass percentages of the raw materials are 85wt%-97wt% for liquid and 3wt%-15wt% for powder.

[0046] The specific implementation of the present invention is described in detail below in conjunction with specific embodiments.

[0047] Embodiment 1

[0048] A method for preparing a conductive copper paste for solar cells that can be sprayed by aerosol, comprising the following steps:

[0049] Step 1: Take a certain amount of organic solvent, thickener, coupling agent, dispersant and defoamer, put them into a beaker and heat them at a constant temperature of 80°C in a water bath until they are completely dissolved to prepare an organic carrier, which is used as a non-conductive phase. The mass percentages of the raw materials in the non-conductive phase are 88wt% of organic solvent, 0wt% of thickener, 3wt% of coupling agent, 6wt% of dispersant and 3wt% of defoamer, respectively. The organic solvent is specifically terpineol, the thickener is specifically ethyl cellulose, and the coupling agent is specifically KH-570. The silane coupling agent and dispersant are specifically ethyl acetate; step 2, taking anhydrous formic acid and anhydrous ethanol in a certain mass ratio and putting them into a beaker, mixing them evenly, and preparing dilute formic acid, wherein the mass ratio of anhydrous formic acid to anhydrous ethanol is 1:39; step 3, taking a certain amount of commercial spherical copper powder and the dilute formic acid in step 3 and putting them into a beaker, stirring and centrifuging and washing until the supernatant is colorless and the pH value is neutral, and then putting the washed copper micron particles into a vacuum drying oven at 50°C to dry, and the dried The copper micron particles are ground and dispersed in an agate mortar for later use. The specification of the commercial spherical copper powder is an average particle size of about 1 μm, and the mass ratio with the dilute formic acid in step 2 is 1:10; step 4, take a certain proportion of commercial Bi2O3-B2O3-ZnO glass powder and the treated spherical copper powder in step 3 and place them in a beaker, add an appropriate amount of anhydrous ethanol, stir by ultrasound, and dry in a vacuum drying oven at 50°C to obtain a uniformly mixed powder, wherein the mass ratio of glass powder to copper powder is 24:1; Step 5, take a certain proportion of the non-conductive phase in step 1 and mix it with the powder in step 4 to prepare a primary copper paste, wherein the mass ratio of the non-conductive phase to the powder is 1:1; Step 6, take a certain proportion of anhydrous ethanol, acetone and an appropriate amount of hexadecyltrimethylammonium bromide powder and mix and stir to prepare a dilution atomizer, wherein the mass ratio of anhydrous ethanol to acetone is 3:1, wherein the mass ratio of liquid to powder is 97wt%:3wt% based on the total weight of the dilution atomizer. Step 7, within half an hour before aerosol spraying, add a certain proportion of the dilution atomizer in step 6 to the primary copper paste in step 5 and mix thoroughly to prepare a conductive copper paste for solar cells that can be sprayed by aerosol, wherein the mass ratio of the primary copper paste to the dilution atomizer is 1:5. Step 8. Draw the required graphics on the control panel of the aerosol spray printer, and put the conductive copper paste prepared in step 7 into the atomizer bottle of the aerosol spray printer. By adjusting the carrier gas, better atomization can be achieved, and the required graphics effect of automatic printing can be achieved. The square resistance is 5.37mΩ / □.

[0050] Embodiment 2

[0051] A method for preparing a conductive copper paste for solar cells that can be sprayed by aerosol, comprising the following steps:

[0052] Step 1: Take a certain amount of organic solvent, thickener, coupling agent, dispersant and defoamer, put them into a beaker and heat them at a constant temperature of 80°C in a water bath until they are completely dissolved to prepare an organic carrier, which is used as a non-conductive phase. The mass percentages of the raw materials in the non-conductive phase are 82wt% of organic solvent, 6wt% of thickener, 3wt% of coupling agent, 6wt% of dispersant and 3wt% of defoamer, respectively. The organic solvent is specifically terpineol, the thickener is specifically ethyl cellulose, and the coupling agent is specifically KH-570. The silane coupling agent and dispersant are specifically ethyl acetate; step 2, taking anhydrous formic acid and anhydrous ethanol in a certain mass ratio and putting them into a beaker, mixing them evenly, and preparing dilute formic acid, wherein the mass ratio of anhydrous formic acid to anhydrous ethanol is 1:39; step 3, taking a certain amount of commercial spherical copper powder and the dilute formic acid in step 3 and putting them into a beaker, stirring and centrifuging and washing until the supernatant is colorless and the pH value is neutral, and then putting the washed copper micron particles into a vacuum drying oven at 50°C to dry, and the dried The copper micron particles are ground and dispersed in an agate mortar for later use. The specification of the commercial spherical copper powder is an average particle size of about 1 μm, and the mass ratio with the dilute formic acid in step 2 is 1:10; step 4, take a certain proportion of commercial Bi2O3-B2O3-ZnO glass powder and the treated spherical copper powder in step 3 and place them in a beaker, add an appropriate amount of anhydrous ethanol, stir by ultrasound, and dry in a vacuum drying oven at 50°C to obtain a uniformly mixed powder, wherein the mass ratio of glass powder to copper powder is 22:3; Step 5, take a certain proportion of the non-conductive phase in step 1 and mix it with the powder in step 4 to prepare a primary copper paste, wherein the mass ratio of the non-conductive phase to the powder is 1:1; Step 6, take a certain proportion of anhydrous ethanol, acetone and an appropriate amount of hexadecyltrimethylammonium bromide powder and mix and stir to prepare a dilution atomizer, wherein the mass ratio of anhydrous ethanol to acetone is 3:1, wherein the mass ratio of liquid to powder is 90wt%:10wt% based on the total weight of the dilution atomizer. Step 7, within half an hour before aerosol spraying, add a certain proportion of the dilution atomizer in step 6 to the primary copper paste in step 5 and mix thoroughly to prepare a conductive copper paste for solar cells that can be sprayed with aerosols, wherein the mass ratio of the primary copper paste to the dilution atomizer is 1:5. Step 8. Draw the required graphics on the control panel of the aerosol spray printer, and put the conductive copper paste prepared in step 7 into the atomizer bottle of the aerosol spray printer. By adjusting the carrier gas, good atomization can be achieved to achieve the desired graphics effect of automatic printing, and the square resistance is 2.46mΩ / □.

[0053] Embodiment 3

[0054] A method for preparing a conductive copper paste for solar cells that can be sprayed by aerosol, comprising the following steps:

[0055] Step 1: Take a certain amount of organic solvent, thickener, coupling agent, dispersant and defoamer, put them into a beaker and heat them at 80°C in a water bath until they are completely dissolved to prepare an organic carrier, which is used as a non-conductive phase. The mass percentages of the raw materials in the non-conductive phase are 76wt% of organic solvent, 12wt% of thickener, 3wt% of coupling agent, 6wt% of dispersant and 3wt% of defoamer, respectively. The organic solvent is specifically terpineol, the thickener is specifically ethyl cellulose, the coupling agent is specifically KH-570 The silane coupling agent and dispersant are specifically ethyl acetate; step 2, taking anhydrous formic acid and anhydrous ethanol in a certain mass ratio and putting them into a beaker, mixing them evenly, and preparing dilute formic acid, wherein the mass ratio of anhydrous formic acid to anhydrous ethanol is 1:39; step 3, taking a certain amount of commercial spherical copper powder and the dilute formic acid in step 3 and putting them into a beaker, stirring and centrifuging and washing until the supernatant is colorless and the pH value is neutral, and then putting the washed copper micron particles into a vacuum drying oven at 50°C to dry, and the dried The copper micron particles are ground and dispersed in an agate mortar for later use. The specification of the commercial spherical copper powder is an average particle size of about 1 μm, and the mass ratio with the dilute formic acid in step 2 is 1:10; step 4, take a certain proportion of commercial Bi2O3-B2O3-ZnO glass powder and the treated spherical copper powder in step 3 and place them in a beaker, add an appropriate amount of anhydrous ethanol, stir by ultrasound, and dry in a vacuum drying oven at 50°C to obtain a uniformly mixed powder, wherein the mass ratio of glass powder to copper powder is 47:3; Step 5, take a certain proportion of the non-conductive phase in step 1 and mix it with the powder in step 4 to prepare a primary copper paste, wherein the mass ratio of the non-conductive phase to the powder is 1:1; Step 6, take a certain proportion of anhydrous ethanol, acetone and an appropriate amount of hexadecyltrimethylammonium bromide powder and mix and stir to prepare a dilution atomizer, wherein the mass ratio of anhydrous ethanol to acetone is 3:1, wherein the mass ratio of liquid to powder is 85wt%:15wt% based on the total weight of the dilution atomizer. Step 7, within half an hour before aerosol spraying, add a certain proportion of the dilution atomizer in step 6 to the primary copper paste in step 5 and mix thoroughly to prepare a conductive copper paste for solar cells that can be sprayed by aerosol, wherein the mass ratio of the primary copper paste to the dilution atomizer is 1:5. Step 8. Draw the required graphics on the control panel of the aerosol spray printer, and put the conductive copper paste prepared in step 7 into the atomizer bottle of the aerosol spray printer. By adjusting the carrier gas, atomization can be achieved to achieve the desired graphic effect of automatic printing, and the square resistance is 4.44mΩ / □.

[0056] Table 1 below shows the performance parameters of the aerosol sprayable conductive copper paste for solar cells prepared in the above embodiments:

[0057] Table 1:

[0058]

[0059] It can be seen from Table 1 above that the embodiment of the present invention has conducted in-depth research on the components of the conductive copper paste, different proportions of each component, especially the preparation of the diluting atomizer and its application in the overall conductive copper paste preparation system, as well as the influence of the preparation process on the performance of the conductive copper paste that can be atomized and sprayed by aerosol. The conductive copper paste finally prepared has the advantages of excellent aerosolization performance, high conductivity and high adhesion strength, and achieves the purposes of simple spraying process, simple preparation process, good aerosol spraying effect, etc. It can be well applied to the aerosol spraying process, and has made a major breakthrough in the research of conductive copper paste, laying a technological foundation for the subsequent replacement of conductive silver paste for solar cells with conductive copper paste.

[0060] In addition, another aspect of the embodiment of the present invention further provides a conductive copper paste for solar cells that can be sprayed by aerosol, which is prepared by the method for preparing a conductive copper paste for solar cells that can be sprayed by aerosol described in any of the above embodiments.

[0061] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a conductive copper paste for solar cells that can be sprayed by aerosol spraying, It is characterized in that The following steps are involved: Step 1: Take a certain amount of organic solvent, thickener, coupling agent, dispersant and defoamer into a beaker, and heat them at a constant temperature of 80° C. in a water bath until they are completely dissolved to prepare an organic carrier as a non-conductive phase for standby use; Step 2: Put anhydrous formic acid and anhydrous ethanol in a certain mass ratio into a beaker and mix them evenly to prepare dilute formic acid; Step 3: Take a certain amount of commercial spherical copper powder and the dilute formic acid in step 2 and put them into a beaker, stir and centrifuge to wash until the supernatant is colorless and the pH value is neutral, then put the washed copper micron particles into a vacuum drying oven at 50 ° C to dry, and put the dried copper micron particles into an agate mortar for grinding and dispersion for later use; Step 4: Take a certain proportion of commercial Bi 2 O 3 -B 2 O 3 -ZnO glass powder and the spherical copper powder treated in step 3 are placed in a beaker, an appropriate amount of anhydrous ethanol is added, ultrasonically stirred, and dried in a vacuum drying oven at 50 °C to obtain a uniformly mixed powder; Step 5: Take a certain proportion of the non-conductive phase in step 1 and mix it with the powder in step 4 to prepare a primary copper slurry; Step 6: Mix a certain proportion of anhydrous ethanol and acetone with the powder of hexadecyltrimethylammonium bromide to prepare a diluted atomizer; Step 7: within half an hour before aerosol spraying, add a certain proportion of the diluting atomizer in step 6 to the primary copper paste in step 5 and mix thoroughly to obtain a conductive copper paste for solar cells that can be sprayed by aerosol; Wherein, the mass ratio of the non-conductive phase to the powder in the step 5 is 1:1, the mass ratio of anhydrous ethanol to acetone in the step 6 is 3:1, and the mass ratio of the primary copper slurry to the diluent atomizer in the step 7 is 1:5; In step 6, the total weight of the diluted atomizer is used as the basis, wherein the weight percentages of the raw materials are 85wt%-97wt% for liquid and 3wt%-15wt% for powder; In the step 1, the organic solvent is terpineol, the thickener is ethyl cellulose, the coupling agent is KH-570 silane coupling agent, and the dispersant is ethyl acetate; The specification of the commercial spherical copper powder in step 3 is an average particle size of 1 μm; The mass ratio of the spherical copper powder and the glass powder after treatment in the step 4 is 22-24:1-3.

2. The method for preparing the conductive copper paste for solar cells capable of aerosol spraying according to claim 1, It is characterized in that In the step 1, the total weight of the organic solvent is used as the basis, wherein the weight percentages of the raw materials are respectively 76wt%-88wt% of the organic solvent, 0wt%-12wt% of the thickener, 3wt% of the coupling agent, 6wt% of the dispersant, and 3wt% of the defoaming agent.

3. The method for preparing the conductive copper paste for solar cells capable of aerosol spraying according to claim 1, It is characterized in that The mass ratio of anhydrous formic acid to anhydrous ethanol in the step 2 is 1:

39.

4. The method for preparing the conductive copper paste for solar cells capable of aerosol spraying according to claim 1, It is characterized in that The mass ratio of the commercial spherical copper powder in step 3 to the dilute formic acid in step 2 is 1:

10.