By preparing a denitration catalyst with a regular structure and using a combination of rare earth and group IIA metal components and non-noble metal components, the problem of low NOx emission reduction activity during the catalytic cracking process is solved, and efficient NOx removal is achieved.
Patent Information
- Application Number
- CN202111054722.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-09
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-09-09
AI Technical Summary
The existing methods for reducing NOx emissions during the catalytic cracking process have low activity and are difficult to effectively reduce NOx pollutant emissions in the catalytic cracking regeneration flue gas.
A denitrification catalyst with a regular structure is used. The preparation method includes preparing a solution of a rare earth and IIA metal component precursor and a non-noble metal component precursor to form a sol, and coating the active component through drying, roasting, beating, and coating. layer and impregnation treatment, and finally reduction treatment in a reducing atmosphere to prepare an efficient NOx removal catalyst.
The NOx removal capability in the gas is significantly improved, and the NOx conversion rate of the catalyst reaches more than 70%, which is better than the existing technology, and the process is simple and the cost is relatively low.
Smart Images

Figure BDA0003254133470000201 
Figure BDA0003254133470000202 
Figure BDA0003254133470000211
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of catalyst preparation, and in particular to a denitration catalyst with a regular structure, a preparation method and application thereof, and gas denitration x method. Background Art
[0002] During the catalytic cracking reaction, the reaction of hydrocarbons causes coke to deposit on the catalyst, which reduces the activity of the catalyst. The catalyst containing coke is sent to the regenerator after the hydrocarbons adsorbed on the catalyst are removed in the stripping section. In the regenerator, the catalyst containing coke is fully contacted with air at high temperature, and the coke on the catalyst surface is burned off, so that the catalyst activity can be restored, and catalytic cracking flue gas is generated at the same time.
[0003] In the catalytic cracking process, some nitrogen compounds in the raw materials enter the coke during the reaction in the riser and are deposited on the spent catalyst. When the spent catalyst enters the regenerator for coking and regeneration, the nitrogen compounds in the coke are oxidized to generate NO. x Flue gas pollutants such as chlorine and chlorine must be purified and meet the standards before they can be discharged.
[0004] At present, the main technical measures to reduce the emission of catalytic cracking regeneration flue gas pollutants include: regenerator optimization, the use of additives and flue gas post-treatment. Post-treatment such as SCR has high removal efficiency, but the investment and operation costs of the equipment are high, and there is ammonia slip problem. The method of adding additives is flexible in operation and does not require investment in facilities, but it is difficult to achieve a high removal efficiency. NO is neither water-soluble nor acidic and alkaline, so it is difficult to remove. In flue gas, NO x The proportion of NO in the gas is usually around 95%, so NO x The key to the removal of iodine is the removal of NO.
[0005] CN1688508A discloses a method for reducing NO in flue gas from fluidized catalytic cracking x The invention discloses a composition for reducing CO emissions and its application, wherein the composition comprises copper and / or cobalt and a carrier, wherein the carrier is selected from hydrotalcite compounds, spinel, alumina, zinc titanate, zinc aluminate, and zinc titanate / zinc aluminate.
[0006] US20050100494 discloses a method for reducing NO in a catalytic cracking process. x Composition for reducing NOx emissions, said composition comprising a cracking catalyst component, preferably comprising Y-type zeolite, and a particulate NOx reduction x Emission components, the reduction of NO x The emission components contain ferrierite.
[0007] Existing FCC process for reducing NO x The emission method has low activity and needs to be improved. Summary of the invention
[0008] The purpose of the present invention is to overcome the existing problems in the prior art in reducing NO in the FCC process. x The method for emission has the problem of low activity, provides a denitration catalyst with a regular structure and its preparation method and application, gas deNO x The method of preparing the denitration catalyst with a regular structure is simple and can effectively reduce NO in the gas x emissions.
[0009] In order to achieve the above object, the first aspect of the present invention provides a method for preparing a denitration catalyst having a regular structure, the method comprising the following steps:
[0010] (1) preparing a solution containing one or more metal component precursors of rare earth group and / or group IIA and one or more non-noble metal component precursors selected from group VB, VIIB, VIII, IB and IIB;
[0011] (2) mixing the solution with an organic acid solution to obtain a sol, and drying and calcining the sol;
[0012] (3) mixing and slurrying the product obtained in step (2), a matrix source, water, and optionally a noble metal active component precursor to obtain an active component coating slurry;
[0013] (4) coating a structured support with the active component coating slurry, drying and calcining the structured support to obtain an active component coating distributed on the inner surface and / or outer surface of the structured support to obtain a first composition;
[0014] The method may further optionally include: (5) impregnating the first composition with a solution containing a noble metal component precursor as an impregnation solution to obtain a solid product, and then drying and / or calcining the solid product to obtain a second composition;
[0015] (6) subjecting the first composition and / or the second composition to a reduction treatment under a reducing atmosphere;
[0016] Among them, the amounts of one or more metal component precursors of rare earth group and / or group IIA, one or more non-precious metal component precursors selected from group VB, VIIB, VIII, IB and IIB, matrix source, precious metal component precursor and regular structure carrier are used so that in the prepared regular structure catalyst, the content of the active component coating is 1-50% by weight based on the total weight of the catalyst, and the active component coating contains matrix and active metal components, wherein, based on the total weight of the active component coating, the content of the matrix is 10-90% by weight, the content of the active metal component is 10-90% by weight, and the active metal component contains: 1) 45-95% by weight of one or more metal components selected from group rare earth and / or group IIA, calculated as oxide; 2) 3-55% by weight of one or more non-precious metal components selected from group VB, VIIB, VIII, IB and IIB, calculated as oxide; 3) 0.01-2% by weight of precious metal components, calculated as elements.
[0017] Preferably, the reducing gas is at least one of H2, CO and CH4, more preferably H2.
[0018] Preferably, the reduction treatment conditions include: temperature: 500-700°C, pressure: 0.05-4MPa, time not less than 1min, preferably 2-20min, volume space velocity of reducing gas: 100-5000h -1 .
[0019] The second aspect of the present invention provides a denitration catalyst having a regular structure prepared by the preparation method described in the first aspect.
[0020] The third aspect of the present invention provides the denitration catalyst with a regular structure according to the second aspect for denitration of gas NO x Application in reaction.
[0021] A fourth aspect of the present invention provides a gas deNO x A method comprising:
[0022] Will contain NO x The gas contacts a denitration catalyst, and the denitration catalyst is the denitration catalyst with a regular structure as described in the second aspect.
[0023] The inventors of the present invention found during the research that the NO removal x After the active components with high capacity are loaded on the regular structure carrier, they are then reduced to reduce the NO in the gas. x The removal capacity is greatly improved. DETAILED DESCRIPTION
[0024] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0025] In the present invention, the term "regular structure catalyst" used refers to a catalyst comprising a regular structure carrier and an active component coating distributed on the inner surface and / or outer surface of the carrier; a "regular structure carrier" is a carrier with a regular structure.
[0026] The first aspect of the present invention provides a method for preparing a denitration catalyst having a regular structure, the method comprising the following steps:
[0027] (1) preparing a solution containing one or more metal component precursors of rare earth group and / or group IIA and one or more non-noble metal component precursors selected from group VB, VIIB, VIII, IB and IIB;
[0028] (2) mixing the solution with an organic acid solution to obtain a sol, and drying and calcining the sol;
[0029] (3) mixing and slurrying the product obtained in step (2), a matrix source, water, and optionally a noble metal active component precursor to obtain an active component coating slurry;
[0030] (4) coating a structured support with the active component coating slurry, drying and calcining the structured support to obtain an active component coating distributed on the inner surface and / or outer surface of the structured support to obtain a first composition;
[0031] The method may further optionally include: (5) impregnating the first composition with a solution containing a noble metal component precursor as an impregnation solution to obtain a solid product, and then drying and / or calcining the solid product to obtain a second composition;
[0032] (6) subjecting the first composition and / or the second composition to a reduction treatment under a reducing atmosphere;
[0033] Among them, the amounts of one or more metal component precursors of rare earth group and / or group IIA, one or more non-precious metal component precursors selected from group VB, VIIB, VIII, IB and IIB, matrix source, precious metal component precursor and regular structure carrier are used so that in the prepared regular structure catalyst, the content of the active component coating is 1-50% by weight based on the total weight of the catalyst, and the active component coating contains matrix and active metal components, wherein, based on the total weight of the active component coating, the content of the matrix is 10-90% by weight, the content of the active metal component is 10-90% by weight, and the active metal component contains: 1) 45-95% by weight of one or more metal components selected from group rare earth and / or group IIA, calculated as oxide; 2) 3-55% by weight of one or more non-precious metal components selected from group VB, VIIB, VIII, IB and IIB, calculated as oxide; 3) 0.01-2% by weight of precious metal components, calculated as elements.
[0034] Preferably, the amounts of one or more metal component precursors of rare earth group and / or group IIA, one or more non-precious metal component precursors selected from groups VB, VIIB, VIII, IB and IIB, matrix source, precious metal component precursor and regular structure carrier are such that in the prepared regular structure catalyst, the content of the active component coating is 10-35% by weight based on the total weight of the catalyst, and the active component coating contains a matrix and an active metal component, wherein, based on the total weight of the active component coating, the content of the matrix is 50-80% by weight, the content of the active metal component is 20-50% by weight, and the active metal component contains: 1) 60-80% by weight of one or more metal components selected from rare earth group and / or group IIA, calculated as oxide; 2) 20-30% by weight of one or more non-precious metal components selected from groups VB, VIIB, VIII, IB and IIB, calculated as oxide; 3) 0.03-1.2% by weight of precious metal components, calculated as elements.
[0035] According to the present invention, conventionally defined rare earth noble metal components can be used in the present invention. In order to further improve the deNOx of the catalyst with a regular structure, x The rare earth metal component is preferably selected from one or more of lanthanum, cerium, praseodymium and neodymium, more preferably lanthanum and / or cerium, and most preferably lanthanum.
[0036] According to the present invention, the Group IIA metal component is selected from one or more of beryllium, magnesium, calcium, strontium and barium, and more preferably magnesium.
[0037] According to the present invention, the VB group non-precious metal component can be selected from at least one of vanadium, niobium and tantalum; the VIII group non-precious metal component can be selected from at least one of iron, cobalt and nickel; the IB group non-precious metal component can be copper; the IIB group non-precious metal component can be selected from at least one of zinc, cadmium and mercury.
[0038] Preferably, the one or more non-precious metal components of groups VB, VIIB, VIII, IB, and IIB are selected from one or more of manganese, iron, cobalt, nickel, copper, zinc, and vanadium, more preferably at least one of manganese, cobalt, and iron, and most preferably cobalt and manganese.
[0039] Preferably, the noble metal component is selected from one or more of ruthenium, rhodium, rhenium, platinum, palladium, silver, iridium and gold, more preferably one or more of platinum, palladium and rhodium, most preferably palladium.
[0040] According to the present invention, the matrix source is a substance that can be converted into a matrix under the calcination conditions in step (4).
[0041] Preferably, the matrix is selected from at least one of alumina, spinel, perovskite, silicon oxide-alumina, zeolite, kaolin, diatomite and perlite, preferably selected from at least one of alumina, spinel and perovskite, and more preferably alumina. In the present invention, the spinel can be various commonly used spinels. When the matrix is preferably alumina, the matrix source can be a precursor of alumina, for example, the matrix source is selected from at least one of gibbsite, diaspore, gibbsite, diaspore, boehmite and pseudo-boehmite.
[0042] In the present invention, the alumina may be at least one selected from γ-alumina, δ-alumina, η-alumina, ρ-alumina, κ-alumina and χ-alumina, and the present invention has no particular limitation on this.
[0043] According to the preparation method provided by the present invention, when the inorganic oxide matrix of the present invention is aluminum oxide, preferably, before slurrying, the inorganic oxide matrix and / or the precursor of the inorganic oxide matrix is subjected to an acidification treatment, and the acidification treatment can be carried out according to conventional technical means in the art. Further preferably, the acid used for the acidification treatment is hydrochloric acid.
[0044] The present invention has a wide range of selection of conditions for the acidification treatment. Preferably, the conditions for the acidification treatment include: an acid-aluminum ratio of 0.12-0.22:1, and a time of 20-40 min.
[0045] In the present invention, unless otherwise specified, the acid-to-aluminum ratio refers to the mass ratio of hydrochloric acid calculated as 36 wt % concentrated hydrochloric acid to the alumina precursor calculated on a dry basis.
[0046] According to the present invention, the structured carrier can be used for the catalyst bed provided in the fixed bed reactor. The structured carrier can be a whole carrier block, the interior of which is hollow and provided with a pore structure, a catalyst coating can be distributed on the inner wall of the pore, and the pore space can be used as a flow space for the fluid. Preferably, the structured carrier is selected from a monolithic carrier having a parallel pore structure with openings at both ends.
[0047] Preferably, the pore density of the cross section of the regular structure carrier is 10-300 pores / square inch, preferably 20-300 pores / square inch; the open porosity of the cross section of the regular structure carrier is 20-80%, preferably 50-80%. The pores may be regular or irregular in shape, and the shapes of the pores may be the same or different, and each pore may be independently one of a square, an equilateral triangle, an equilateral hexagon, a circle, and a corrugated shape.
[0048] Preferably, the regular structure carrier can be selected from at least one of a cordierite honeycomb carrier, a mullite honeycomb carrier, a diamond honeycomb carrier, a corundum honeycomb carrier, a zirconium corundum honeycomb carrier, a quartz honeycomb carrier, a nepheline honeycomb carrier, a feldspar honeycomb carrier, an alumina honeycomb carrier and a metal alloy honeycomb carrier.
[0049] According to the present invention, preferably, the metal component precursor containing one or more metal components of rare earth group and / or group IIA and one or more non-precious metal component precursors selected from group VB, VIIB, VIII, IB and IIB can be independently selected from water-soluble salts of each metal component, such as nitrate, chloride, chlorate or sulfate, etc., preferably nitrate and / or chloride. In particular, the precursor of manganese can be potassium permanganate and / or manganese chloride.
[0050] According to the present invention, the one or more metal components of the rare earth group and / or the IIA group include rare earth group metal components and the IIA group metal components.
[0051] Preferably, based on the total amount of the active metal component, the content of the rare earth metal component is 30-80% by weight, more preferably 35-75% by weight; the content of the IIA group metal component is 5-40% by weight, more preferably 10-30% by weight.
[0052] Preferably, the one or more non-precious metal components selected from groups VB, VIIB, VIII, IB and IIB include one or more non-precious metal components selected from groups VB, VIII, IB, IIB and group VIIB non-precious metal components.
[0053] Preferably, based on the total amount of the active metal components, the content of one or more non-precious metal components of groups VB, VIII, IB, and IIB is 3-30% by weight, and more preferably 5-20% by weight; the content of the non-precious metal components of group VIIB is 3-20% by weight, and more preferably 5-15% by weight.
[0054] According to a preferred embodiment of the present invention, the amount of one or more metal component precursors of rare earth group and / or group IIA, one or more non-precious metal component precursors selected from group VB, VIIB, VIII, IB and IIB, matrix source, precious metal component precursor and regular structure carrier is such that in the prepared regular structure catalyst, the content of the active component coating is 13-20% by weight based on the total weight of the catalyst, and the active component coating contains a matrix and an active metal component, wherein Based on the total weight of the active component coating, the content of the matrix is 50-80% by weight, the content of the active metal component is 20-50% by weight, and the active metal component contains: 1) 11-28% by weight of lanthanum in terms of oxide; 2) 4-6% by weight of magnesium in terms of oxide; 3) 2-10% by weight of cobalt in terms of oxide; 4) 2-8% by weight of manganese in terms of oxide; 5) 0.015-0.04% by weight of palladium in terms of element, and the molar ratio of lanthanum to cobalt is (0.4-6):1. In this particularly preferred embodiment, La, Co, Mg, Mn and precious metals are used in combination as metal elements, which can greatly improve NO x ability.
[0055] The method for preparing active metal precursors provided by the present invention is a sol-gel method. The method for obtaining the solution in step (1) is not particularly limited in the present invention, as long as the precursors of each metal component are mixed uniformly. For example, the precursors of each metal component are dissolved in water and stirred thoroughly.
[0056] The present invention has no particular limitation on the type and amount of the organic acid in step (2), as long as the sol-gel reaction proceeds smoothly. The type of the organic acid can be conventionally selected in the art, preferably, the organic acid is selected from citric acid and / or acetic acid, more preferably citric acid.
[0057] According to a preferred embodiment of the present invention, the molar ratio of the organic acid to the solution calculated as metal ions is (1-10):1.
[0058] According to a preferred embodiment of the present invention, the concentration of the organic acid solution is 0.01-3 mol / L.
[0059] There is no particular limitation on the method for obtaining the sol in step (2), and it can be carried out, for example, under heating conditions in a water bath.
[0060] According to a preferred embodiment of the present invention, the mixing conditions in step (2) include: under stirring, pH is 4-7, and temperature is 50-90°C; preferably, pH is 5-6, and temperature is 65-80°C.
[0061] According to a preferred embodiment of the present invention, the pH can be adjusted by adding acid and / or base, and there is no particular limitation on the specific type thereof, for example, it can be aqueous ammonia.
[0062] Preferably, the stirring rate of the mixing in step (2) is 120-1000 rpm.
[0063] According to the present invention, step (2) further comprises drying and calcining the sol.
[0064] According to the method provided by the present invention, there is no restriction on the order of adding the product obtained in step (2), the matrix source, water and optionally the precursor of the precious metal active component in step (3), as long as the product obtained in step (2), the matrix source, optionally the precursor of the active metal component and water are contacted to obtain the active component coating slurry. Similarly, there is no specific restriction on the method of mixing and slurrying the product obtained in step (2), the matrix source and optionally the precursor of the precious metal active component.
[0065] According to the present invention, preferably, the solid content of the slurry in step (3) is 5-40% by weight.
[0066] The coating described in the method provided by the present invention can be to coat the active component coating slurry on the inner surface and / or outer surface of the regular structure carrier by various coating methods; the coating method can be a water coating method, an immersion method or a spraying method. The specific operation of coating can be carried out with reference to the method described in CN1199733C. In a preferred case, the coating adopts a water coating method, during the coating process, one end of the regular structure carrier is immersed in the active component coating slurry, and a vacuum is applied to the other end, so that the active component coating slurry passes through the pores of the regular structure carrier continuously. The volume of the active component coating slurry passing through the pores of the regular structure carrier can be 2-20 times the volume of the regular structure carrier, the vacuum pressure applied can be -0.1MPa (megapascals) to -0.01MPa (megapascals), the coating temperature can be 10-70°C, and the coating time can be 0.1-300 seconds. The regular structure carrier coated with the active component coating slurry is dried and / or calcined to obtain the active component coating distributed on the inner surface and / or outer surface of the regular structure carrier, and obtain the first composition. It should be noted that in the present invention, the precious metal can be introduced during the mixing and beating process in step (3), can be introduced during the impregnation process in step (5), or can be introduced partially in both steps simultaneously. When the method of the present invention further includes introducing the precious metal in step (5), the active component coating of the first composition obtained in step (4) is only a partial active component coating, and the entire active component coating also includes the precious metal introduced in the subsequent step (5).
[0067] Preferably, the method provided by the present invention includes step (5). That is, preferably, the noble metal component precursor is introduced through step (5), and the use of this preferred embodiment is more conducive to the dispersion of the noble metal elements.
[0068] According to the present invention, preferably, in step (5), the noble metal component precursor is hydrolyzed in an acid solution to provide the impregnation solution. Specifically, after the hydrolysis, dilution (water may be added) or concentration (evaporation may be performed) may be performed, and then the impregnation may be performed to provide a denitration catalyst with a regular structure and a specific noble metal component loading amount.
[0069] Preferably, the acid is selected from water-soluble inorganic acids and / or organic acids, preferably at least one selected from hydrochloric acid, nitric acid, phosphoric acid and acetic acid.
[0070] According to the present invention, preferably, the acid is used in an amount such that the pH value of the impregnation solution is less than 6.0, preferably 2 to 5. This preferred embodiment is more conducive to uniform dispersion of active components and improvement of the wear resistance of the finished catalyst.
[0071] The present invention can obtain the solid product by filtering the mixture obtained after the immersion. The filtration can be performed according to conventional technical means in the art.
[0072] According to the method provided by the present invention, the "drying and / or roasting" means that the solid product can be dried, the solid product can be roasted, or the solid product can be dried first and then roasted. The present invention does not particularly limit the conditions for the roasting in step (5), and it can be carried out according to conventional technical means in the art. For example, the roasting in step (5) can be carried out in air or an inert atmosphere (such as nitrogen).
[0073] In steps (2), (4) and (5) of the present invention, the respective products may be dried, calcined or dried before calcining. The present invention has no particular limitation on this. Preferably, the respective products are dried before calcining. The present invention has no particular limitation on the conditions for drying and calcining, which may be carried out according to conventional technical means in the art. For example, the drying conditions may include: a temperature of 100-150°C and a time of 1-5h. The present invention has no particular limitation on the conditions for calcining, which may be carried out in an atmosphere containing air or an inert atmosphere. The conditions for calcining in step (2), the calcining in step (4) for preparing the first composition and the calcining in step (5) for preparing the second composition each independently include: being carried out in an oxygen-containing atmosphere, at a temperature of 350-750°C and a time of 0.1-6h.
[0074] According to the present invention, in step (6), the first composition in step (4) and / or the second composition in step (5) may be subjected to a reduction treatment.
[0075] Preferably, the reducing atmosphere can be provided by reducing gas, and the concentration of the reducing gas is 1-20% by volume. In addition to the reducing gas, the reducing atmosphere can also contain an inert gas, such as nitrogen, helium, neon and argon.
[0076] Preferably, the reducing gas is at least one of H2, CO and CH4, more preferably H2. The advantage of using H2 is that the reduction depth is higher and it is more conducive to shortening the reduction time.
[0077] Preferably, the reduction treatment conditions include: temperature: 500-700°C, pressure: 0.05-4MPa, time not less than 1min, preferably 2-20min, volume space velocity of reducing gas: 100-5000h -1 .
[0078] Further preferably, the reduction treatment conditions include: temperature: 550-650°C, pressure: 0.05-2MPa, time: 2-15min, volume space velocity of reducing gas: 400-4000h -1 .
[0079] The second aspect of the present invention provides a denitration catalyst having a regular structure prepared by the preparation method described in the first aspect.
[0080] According to the structured catalyst of the present invention, the structured carrier can be used for the catalyst bed provided in a fixed bed reactor.
[0081] The catalyst provided by the present invention is particularly suitable for removing NO from gas. x Based on this, the third aspect of the present invention provides the denitration catalyst with a regular structure as described in the second aspect for deNOx in gas. x Application in reaction.
[0082] A fourth aspect of the present invention provides a gas deNO x A method comprising:
[0083] Will contain NO x The gas contacts a denitration catalyst, and the denitration catalyst is the denitration catalyst with a regular structure as described in the second aspect.
[0084] The NO x The gas is not particularly limited and can be any gas containing NO x A gas such as flue gas.
[0085] The present invention treats NO in the gas x The content of NO is preferably selected in a wide range. x The content of NO is 0.001-3% by volume; further preferably, in the gas, NO x The content is 0.01-2 volume %.
[0086] In the present invention, the gas may also contain NO x Gases other than oxygen, including but not limited to O2, CO, CO2 and H2O.
[0087] When the gas contains oxygen, it is preferred to remove the oxygen first and then perform the contact. The present invention has no particular limitation on the method for removing oxygen, and the method can be performed according to conventional techniques in the art.
[0088] The catalyst provided by the present invention is particularly suitable for catalytic cracking regeneration of NO in flue gas. x Preferably, the gas is catalytic cracking regeneration flue gas.
[0089] According to the method provided by the present invention, preferably, the contact is carried out in a flue gas channel arranged after the cyclone separator and / or after the CO incinerator. xHigh concentration and less catalyst fine powder particles, high temperature is conducive to improving the reaction conversion rate, and less particles are not easy to block the pores. However, during the regeneration process with low residual oxygen content, the CO concentration is high. In the CO incinerator used for energy recovery, if it is fully oxidized, it is easy to generate NO x Based on this, preferably, the contact between the regenerated flue gas and the catalyst is carried out in the CO incinerator and / or the flue gas channel arranged after the CO incinerator to catalytically convert NO x .
[0090] The present invention has no particular limitation on the CO incinerator, and various CO incinerators conventionally used in the art, such as a vertical CO incinerator or a horizontal CO incinerator, may be used.
[0091] In the present invention, the cyclone separator is preferably a three-stage cyclone separator.
[0092] Preferably, the regular structure catalyst exists in the form of a catalyst bed. In the method provided by the present invention, the regular structure catalyst can be arranged as a fixed catalyst bed in a flue gas channel arranged after a cyclone separator and / or after a CO incinerator, and the flowing flue gas can flow through the regular structure catalyst bed, that is, it can flow through the pores in the regular structure carrier and react with the active component coating distributed on the pore wall.
[0093] The present invention has a wide range of contact conditions, as long as the NO in the gas can be removed. x According to the method provided by the present invention, preferably, the contact conditions include: temperature of 300-1000°C, reaction pressure of 0-0.5MPa, gas volume space velocity of 100-5000h -1 The reaction pressure in the present invention is measured in gauge pressure.
[0094] According to the present invention, preferably, a small amount of hydrogen can be introduced during the contacting process. This preferred embodiment is more conducive to extending the service life of the catalyst. The present invention has a wide range of selection for the amount of hydrogen introduced, which is based on the ability to achieve safe production.
[0095] In the present invention, unless otherwise specified, ppm refers to volume concentration.
[0096] The present invention will be described in detail below through specific examples. The component content parameters in the following examples are measured by X-ray fluorescence spectroscopy (XRF) method; the raw materials used: lanthanum nitrate (analytical grade, Aladdin Biochemical Company), magnesium nitrate (analytical grade, Sinopharm Chemical Reagent Co., Ltd.), manganese chloride (analytical grade, Beijing Chemical Plant), cobalt nitrate (analytical grade, Beijing Inokai Technology Co., Ltd.), citric acid (analytical grade, Sinopharm Chemical Reagent Co., Ltd.), ammonia water (analytical grade, 25%, Tianjin Damao Chemical Plant), palladium chloride (Beijing Purchasing and Supply Station of China Pharmaceutical Company), hydrochloric acid (Beijing Chemical Plant), OX50-SiO2 (Sinopec Catalyst Company).
[0097] Example 1
[0098] Weigh 480mL of deionized water in a beaker, add 20g of lanthanum nitrate based on the mass of La2O3, 4g of magnesium nitrate based on the mass of MgO, 7g of cobalt nitrate based on the mass of Co2O3, and 4g of manganese chloride based on the mass of MnO under stirring until completely dissolved. According to the molar ratio of metal ions to citric acid of 1:2, weigh citric acid and dissolve it in deionized water to prepare a solution with a concentration of 1.04mol / L, and stir continuously until fully dissolved. While stirring, mix the above solutions, add ammonia water to adjust the pH value of the solution to 6, and then evaporate to a sol state in a water bath at 80°C with stirring. Then dry at 120°C, roast at 700°C in an air atmosphere for 6 hours, and grind to obtain an active metal precursor.
[0099] Weigh 30 g of aluminum ore in terms of Al2O3 mass, add 120 mL of water and 4.5 g of 36 wt% concentrated hydrochloric acid, and slurry. Weigh 20 g of active metal precursor, add it to the acidified inorganic oxide matrix, mix and stir, and obtain active component coating slurry.
[0100] The active component coating slurry obtained above is coated on 300 g of a cordierite structured carrier with 200 pores / square inch and dried and calcined to obtain an active component coating distributed on the inner surface and / or outer surface of the structured carrier. The obtained component is dried at 120°C and then calcined at 700°C in an air atmosphere for 4 hours to obtain a structured catalyst semi-finished product.
[0101] Weigh a palladium precursor and dissolve it in dilute hydrochloric acid at a mass ratio of 1:1, add deionized water to dilute it, and prepare a palladium chloride solution with a concentration of 5.6 g / L and a pH of 2. Weigh a certain amount of palladium chloride solution based on a palladium mass of 0.009 g, and use the palladium-containing solution as an impregnation liquid to impregnate the above-mentioned catalyst semi-finished product to obtain a solid product, and then dry the solid product at 120° C. and calcine it at 700° C. in an air atmosphere for 4 hours to obtain Catalyst A. Among them, based on the total weight of the regular structure catalyst, the content of the active component coating is 14.3% by weight.
[0102] The concentration of 8% by volume of H2 / N2 was selected as the reducing atmosphere, and the temperature was 650°C, the pressure was 0.05 MPa, the time was 5 min, and the volume space velocity was 1000 h -1 Catalyst D was reduced under the conditions of .
[0103] Example 2
[0104] Weigh 180mL of deionized water in a beaker, add 10g of lanthanum nitrate based on the mass of La2O3, 4g of magnesium nitrate based on the mass of MgO, 2g of cobalt nitrate based on the mass of Co2O3, and 2g of manganese chloride based on the mass of MnO under stirring until completely dissolved. Weigh citric acid and dissolve it in deionized water according to the molar ratio of metal ions to citric acid of 1:2 to prepare a solution with a concentration of 1.04mol / L, and stir continuously until fully dissolved. While stirring, mix the above solutions, add ammonia water to adjust the pH value of the solution to 6, and then stir and evaporate to a sol state in a water bath at 80°C. Then dry at 120°C, roast at 700°C in an air atmosphere for 6 hours, and grind to obtain an active metal precursor.
[0105] Weigh 40 g of aluminum ore in terms of Al2O3 mass, add 160 mL of water and 6 g of 36 wt% concentrated hydrochloric acid, and slurry. Weigh 10 g of active metal precursor, add it to the acidified inorganic oxide matrix, mix and stir, and obtain active component coating slurry.
[0106] The active component coating slurry obtained above is coated on 300 g of a cordierite structured carrier with 200 pores / square inch and dried and calcined to obtain an active component coating distributed on the inner surface and / or outer surface of the structured carrier. The obtained component is dried at 120°C and then calcined at 700°C in an air atmosphere for 4 hours to obtain a structured catalyst semi-finished product.
[0107] Weigh a palladium precursor and dissolve it in dilute hydrochloric acid at a mass ratio of 1:1, add deionized water to dilute it, and prepare a palladium chloride solution with a concentration of 5.6 g / L and a pH of 2. Weigh a certain amount of palladium chloride solution based on a palladium mass of 0.018 g, and use the palladium-containing solution as an impregnation liquid to impregnate the above-mentioned catalyst semi-finished product to obtain a solid product, and then dry the solid product at 120° C. and calcine it at 700° C. in an air atmosphere for 4 hours to obtain Catalyst B. Wherein, based on the total weight of the regular structure catalyst, the content of the active component coating is 15.5% by weight.
[0108] The concentration of 8% by volume of H2 / N2 was selected as the reducing atmosphere, and the temperature was 650°C, the pressure was 0.05 MPa, the time was 10 min, and the volume space velocity was 1000 h -1 Catalyst D was reduced under the conditions of .
[0109] Example 3
[0110] Weigh 540mL of deionized water in a beaker, add 30g of lanthanum nitrate based on the mass of La2O3, 6g of magnesium nitrate based on the mass of MgO, 10g of cobalt nitrate based on the mass of Co2O3, and 8g of manganese chloride based on the mass of MnO under stirring until completely dissolved. Weigh citric acid and dissolve it in deionized water according to the molar ratio of metal ions to citric acid of 1:2 to prepare a solution with a concentration of 1.04mol / L, and stir continuously until fully dissolved. While stirring, mix the above solutions, add ammonia water to adjust the pH value of the solution to 6, and then stir and evaporate to a sol state in a water bath at 80°C. Then dry at 120°C, roast at 700°C in an air atmosphere for 6 hours, and grind to obtain an active metal precursor.
[0111] Weigh 25 g of aluminum ore in terms of Al2O3 mass, add 120 mL of water and 3.8 g of 36 wt% concentrated hydrochloric acid, and slurry. Weigh 25 g of active metal precursor, add it to the acidified inorganic oxide matrix, mix and stir, and obtain active component coating slurry.
[0112] The active component coating slurry obtained above is coated on 300 g of a cordierite structured carrier with 200 pores / square inch and dried and calcined to obtain an active component coating distributed on the inner surface and / or outer surface of the structured carrier. The obtained component is dried at 120°C and then calcined at 700°C in an air atmosphere for 4 hours to obtain a structured catalyst semi-finished product.
[0113] Weigh a palladium precursor and dissolve it in dilute hydrochloric acid at a mass ratio of 1:1, add deionized water to dilute it, and prepare a palladium chloride solution with a concentration of 5.6 g / L and a pH of 2. Weigh a certain amount of palladium chloride solution based on a palladium mass of 0.009 g, and use the palladium-containing solution as an impregnation liquid to impregnate the above-mentioned catalyst semi-finished product to obtain a solid product, and then dry the solid product at 120° C. and calcine it at 700° C. in an air atmosphere for 4 hours to obtain Catalyst C. Wherein, based on the total weight of the regular structure catalyst, the content of the active component coating is 16.7% by weight.
[0114] The concentration of 8% by volume of H2 / N2 was selected as the reducing atmosphere, and the temperature was 650°C, the pressure was 0.05 MPa, the time was 10 min, and the volume space velocity was 1000 h -1 Catalyst D was reduced under the conditions of .
[0115] Example 4
[0116] Weigh 350mL of deionized water in a beaker, add 20g of lanthanum nitrate based on the mass of La2O3, 4g of magnesium nitrate based on the mass of MgO, 7g of cobalt nitrate based on the mass of Co2O3, and 4g of manganese chloride based on the mass of MnO under stirring until completely dissolved. Weigh citric acid and dissolve it in deionized water according to the molar ratio of metal ions to citric acid of 1:2 to prepare a solution with a concentration of 1.04mol / L, and stir continuously until fully dissolved. While stirring, mix the above solutions, add ammonia water to adjust the pH value of the solution to 6, and then stir and evaporate to a sol state in a water bath at 80°C. Then dry at 120°C, roast at 700°C in an air atmosphere for 6 hours, and grind to obtain an active metal precursor.
[0117] Weigh 30 g of aluminum ore in terms of Al2O3 mass, add 120 mL of water and 4.5 g of 36 wt% concentrated hydrochloric acid, and slurry. Weigh 20 g of active metal precursor, add it to the acidified inorganic oxide matrix, mix and stir, and obtain active component coating slurry.
[0118] The active component coating slurry obtained above is coated on 300 g of a cordierite structured carrier with 200 pores / square inch and dried and calcined to obtain an active component coating distributed on the inner surface and / or outer surface of the structured carrier. The obtained component is dried at 120°C and then calcined at 700°C in an air atmosphere for 4 hours to obtain a structured catalyst semi-finished product.
[0119] Weigh a palladium precursor and dissolve it in dilute hydrochloric acid at a mass ratio of 1:1, add deionized water to dilute it, and prepare a palladium chloride solution with a concentration of 5.6 g / L and a pH of 2. Weigh a certain amount of palladium chloride solution based on a palladium mass of 0.009 g, and use the palladium-containing solution as an impregnation liquid to impregnate the above-mentioned catalyst semi-finished product to obtain a solid product, and then dry the solid product at 120° C. and calcine it at 700° C. in an air atmosphere for 4 hours to obtain catalyst D. Wherein, based on the total weight of the regular structure catalyst, the content of the active component coating is 14.3% by weight.
[0120] The concentration of 8% by volume of H2 / N2 was selected as the reducing atmosphere, the temperature was 650°C, the pressure was 0.05 MPa, the time was 5 min, and the volume space velocity was 2000 h -1 Catalyst D was reduced under the conditions of .
[0121] Example 5
[0122] Weigh 430mL of deionized water in a beaker, add 30g of lanthanum nitrate based on the mass of La2O3, 4g of magnesium nitrate based on the mass of MgO, 5g of cobalt nitrate based on the mass of Co2O3, and 4g of manganese chloride based on the mass of MnO under stirring until completely dissolved. According to the molar ratio of metal ions to citric acid of 1:2, weigh citric acid and dissolve it in deionized water to prepare a solution with a concentration of 1.04mol / L, and stir continuously until fully dissolved. While stirring, mix the above solutions, add ammonia water to adjust the pH value of the solution to 6, and then stir and evaporate to a sol state in a water bath at 80°C. Then dry at 120°C, roast at 700°C in an air atmosphere for 6 hours, and grind to obtain an active metal precursor.
[0123] Weigh 30 g of aluminum ore in terms of Al2O3 mass, add 180 mL of water and 6 g of 36 wt% concentrated hydrochloric acid, and slurry. Weigh 30 g of active metal precursor, add it to the acidified inorganic oxide matrix, mix and stir, and obtain active component coating slurry.
[0124] The active component coating slurry obtained above is coated on 300 g of a cordierite structured carrier with 200 pores / square inch and dried and calcined to obtain an active component coating distributed on the inner surface and / or outer surface of the structured carrier. The obtained component is dried at 120°C and then calcined at 700°C in an air atmosphere for 4 hours to obtain a structured catalyst semi-finished product.
[0125] The palladium precursor was weighed and dissolved in dilute hydrochloric acid at a mass ratio of 1:1, and deionized water was added to dilute it to prepare a palladium chloride solution with a concentration of 5.6 g / L and a pH of 2. A certain amount of palladium chloride solution was weighed according to the palladium mass of 0.009 g, and the palladium-containing solution was used as an impregnation liquid to impregnate the above-mentioned catalyst semi-finished product to obtain a solid product, and then the solid product was dried at 120° C. and calcined at 700° C. in an air atmosphere for 4 hours to obtain Catalyst E. Among them, based on the total weight of the regular structure catalyst, the content of the active component coating was 16.7% by weight.
[0126] Select H2 / N2 with a concentration of 8 vol% as the reducing atmosphere, at a temperature of 680°C, a pressure of 0.05 MPa, a time of 10 min, and a volume space velocity of 1000 h -1 Catalyst D was reduced under the conditions of .
[0127] Example 6
[0128] The method of Example 1 is followed, except that the reducing gas is replaced by CO / N2 with a volume concentration of 8%.
[0129] Example 7
[0130] The method of Example 1 is followed, except that the palladium chloride solution is replaced by a ruthenium chloride solution of equal concentration, and the content of precious metals in the prepared catalyst remains unchanged.
[0131] Example 8
[0132] The method of Example 1 is followed, except that, calculated as oxide, lanthanum nitrate is replaced by an equal mass of cerium nitrate; calculated as oxide, cobalt nitrate is replaced by an equal mass of iron nitrate.
[0133] Comparative Example 1
[0134] A certain amount of palladium chloride solution prepared in Example 1 was weighed according to the palladium mass of 0.009 g. The palladium chloride solution was coated on 300 g of a cordierite structured carrier with 200 pores / square inch, dried and calcined to obtain an active component coating distributed on the inner surface and / or outer surface of the structured carrier, and the obtained component was dried at 120°C and then calcined at 700°C in an air atmosphere to obtain a structured catalyst, namely, catalyst D1.
[0135] Comparative Example 2
[0136] The catalyst prepared by the method described in CN102658155A is prepared by dissolving ferric nitrate and cerium nitrate in water to obtain a mixed solution, stirring the solution evenly by magnetic force, adding a certain titanium dioxide carrier to the solution, controlling the molar ratio of Fe:Ce:TiO2 to be 19:1:100, applying the above slurry to 300g of a 200 pores / square inch cordierite structured carrier according to a solid content of 100g, drying and calcining to obtain an active component coating distributed on the inner surface and / or outer surface of the structured carrier, drying the obtained components at 120°C, and then calcining at 700°C in an air atmosphere to obtain a catalyst D2.
[0137] Performance Testing
[0138] (I) Determination of component content: The deNOx prepared in Examples 1-8 x The component contents of the catalysts were all determined by X-ray fluorescence spectroscopy (XRF), see for details the Petrochemical Analysis Method (RIPP Experimental Method), edited by Yang Cuiding et al., published by Science Press in 1990. The specific results are shown in the following table.
[0139] Table 1 Removal of NO in Examples 1-8 x Content of each catalyst component (wt%)
[0140]
[0141] The content of each component in Table 1 is based on the total amount of the active metal component coating.
[0142] (II) Activity evaluation: The catalyst activity evaluation standard in the present invention is based on the NO content in the reaction product. x As a measure of the concentration change, the NO x The content is measured by FT-IR Fourier infrared flue gas analyzer and evaluated by fixed bed microreactor experimental device. x The catalyst activity evaluation results are expressed as conversion rate.
[0143] Conversion rate calculation method:
[0144]
[0145] Among them, C (inlet) Refers to the experimental device inlet NO x The concentration of C (outlet) Refers to the experimental device outlet NO x concentration.
[0146] For the removal of NO provided in the above embodiments and comparative examples xThe catalytic cracking reaction-regeneration evaluation was carried out on a small fixed bed simulated flue gas device, with a catalyst loading of 20 g, a reaction temperature of 680°C, a pressure of 0.03 MPa, a feed gas volume flow rate (standard condition) of 1000 mL / min, and a volume space velocity of about 3000 h -1 The raw gas contained 1200 ppm of NO, and the balance was N2. The gas product was analyzed by an online infrared analyzer to obtain the NO concentration after the reaction. The results of the evaluation time of 0.5 h are listed in Table 2, and the results of the evaluation time of 1 h are listed in Table 3.
[0147] Table 2 Different NO removal within 0.5h x Comparison of Catalytic Conversion of NO by Catalysts
[0148]
[0149] As can be seen from the table above, within the first 0.5 h, the NO reduction x Compared with the catalyst prepared by the prior art under the same evaluation conditions, the catalyst provided by the present invention has a significant effect on NO x The removal effect can be as high as 70% or more, which is significantly better than the evaluation results of other catalysts.
[0150] Table 3 Different NO removal within 1 h x Comparison of Catalytic Conversion of NO by Catalysts
[0151]
[0152] As can be seen from the above table, within 1 hour, the NO reduction provided by the present invention x Compared with the catalyst prepared by the prior art under the same evaluation conditions, the catalyst provided by the present invention has a significant effect on NO x The removal effect can reach up to more than 50%, which is significantly better than the comparative catalyst.
[0153] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing a denitration catalyst having a regular structure, the method comprising the following steps: (1) preparing a solution containing one or more metal component precursors of rare earth group and / or group IIA and one or more non-precious metal component precursors selected from group VB, VIIB, VIII, IB and IIB; the rare earth metal component is selected from one or more of lanthanum, cerium, praseodymium and neodymium; the IIA group metal component is selected from one or more of beryllium, magnesium, calcium, strontium and barium; the one or more non-precious metal components of group VB, VIIB, VIII, IB and IIB are selected from one or more of manganese, iron, cobalt, nickel, copper, zinc and vanadium; (2) mixing the solution with an organic acid solution to obtain a sol, and drying and calcining the sol; (3) mixing and slurrying the product obtained in step (2), a matrix source and water to obtain an active component coating slurry; (4) coating a structured support with the active component coating slurry, and drying and calcining the coating to obtain an active component coating distributed on the inner surface and / or outer surface of the structured support, thereby obtaining a first composition; (5) impregnating the first composition with a solution containing a precursor of a precious metal component as an impregnation liquid to obtain a solid product, and then drying and / or roasting the solid product to obtain a second composition; the precious metal component is selected from one or more of ruthenium, rhodium, rhenium, platinum, palladium, silver, iridium and gold; (6) subjecting the second composition to a reduction treatment under a reducing atmosphere; The amounts of one or more metal component precursors of rare earth group and / or group IIA, one or more non-precious metal component precursors selected from group VB, VIIB, VIII, IB and IIB, matrix source, precious metal component precursor and regular structure carrier are such that in the prepared regular structure catalyst, the content of the active component coating is 1-50% by weight based on the total weight of the catalyst, and the active component coating contains a matrix and an active metal component, wherein, based on the total weight of the active component coating, the content of the matrix is 10-90% by weight, the content of the active metal component is 10-90% by weight, and the active metal component contains: 1) 45-95% by weight of one or more metal components selected from group rare earth group and / or group IIA, calculated as oxide; 2) 3-55% by weight of one or more non-precious metal components selected from group VB, VIIB, VIII, IB and IIB, calculated as oxide; 3) 0.01-2% by weight of precious metal components, calculated as elements.
2. The preparation method according to claim 1, wherein The amounts of one or more metal component precursors of rare earth group and / or group IIA, one or more non-precious metal component precursors selected from group VB, VIIB, VIII, IB and IIB, matrix source, precious metal component precursor and regular structure carrier are such that in the prepared regular structure catalyst, the content of the active component coating is 5-40% by weight based on the total weight of the catalyst, and the active component coating contains matrix and active metal components, wherein, based on the total weight of the active component coating, the content of the matrix is 40-90% by weight, the content of the active metal component is 10-60% by weight, and the active metal component contains: 1) 50-90% by weight of one or more metal components selected from group rare earth group and / or group IIA, calculated as oxide; 2) 7-50% by weight of one or more non-precious metal components selected from group VB, VIIB, VIII, IB and IIB, calculated as oxide; 3) 0.02-1.5% by weight of precious metal components, calculated as elements.
3. The preparation method according to claim 2, wherein Based on the total weight of the catalyst, the content of the active component coating is 10-35% by weight, and the active component coating contains a matrix and an active metal component, wherein, based on the total weight of the active component coating, the content of the matrix is 50-80% by weight, the content of the active metal component is 20-50% by weight, and the active metal component contains: 1) calculated as oxide, 60-80% by weight of one or more metal components selected from rare earth group and / or group IIA; 2) calculated as oxide, 20-30% by weight of one or more non-precious metal components selected from groups VB, VIIB, VIII, IB and IIB; 3) calculated as elements, 0.03-1.2% by weight of precious metal components.
4. The preparation method according to claim 1, wherein The rare earth metal component is lanthanum and / or cerium; The Group IIA metal component is magnesium; One or more non-precious metal components of the VB, VIII, IB, and IIB groups are cobalt and / or iron; The Group VIIB non-noble metal component is manganese; The noble metal component is selected from one or more of platinum, palladium and rhodium; The matrix source is a substance that can be converted into a matrix under the calcination conditions of step (4); The matrix is selected from at least one of alumina, spinel, perovskite, silica-alumina, zeolite, kaolin, diatomaceous earth and perlite.
5. The preparation method according to claim 4, wherein The noble metal component is palladium.
6. The preparation method according to claim 4, wherein The matrix is selected from at least one of alumina, spinel and perovskite.
7. The preparation method according to claim 6, wherein: The matrix is alumina.
8. The preparation method according to claim 1, wherein The regular structure carrier is selected from a monolithic carrier having a parallel pore structure with openings at both ends.
9. The preparation method according to claim 8, wherein: The cross-section pore density of the regular structure carrier is 10-300 pores / square inch, and the open porosity is 20-80%.
10. The preparation method according to claim 1, wherein: The regular structure carrier is selected from at least one of cordierite honeycomb carrier, mullite honeycomb carrier, diamond honeycomb carrier, corundum honeycomb carrier, zirconium corundum honeycomb carrier, quartz honeycomb carrier, nepheline honeycomb carrier, feldspar honeycomb carrier, alumina honeycomb carrier and metal alloy honeycomb carrier.
11. The preparation method according to claim 1, wherein: The rare earth metal component precursor, the IIA group metal component precursor, one or more non-precious metal component precursors selected from groups VB, VIII, IB, and IIB, the VIIB group non-precious metal component precursor, and the precious metal component precursor are each independently selected from the nitrate and / or chloride of each metal component.
12. The preparation method according to claim 1, wherein: The one or more metal components of the rare earth group and / or the IIA group include rare earth group metal components and the IIA group metal components.
13. The preparation method according to claim 12, wherein: Based on the total amount of the active metal components, the content of the rare earth metal component is 30-80% by weight; the content of the IIA group metal component is 5-40% by weight.
14. The preparation method according to claim 13, wherein: Based on the total amount of the active metal components, the content of the rare earth metal component is 35-75% by weight; the content of the IIA group metal component is 10-30% by weight.
15. The preparation method according to claim 1, wherein: The one or more non-precious metal components selected from groups VB, VIIB, VIII, IB and IIB include one or more non-precious metal components selected from groups VB, VIII, IB, IIB and group VIIB non-precious metal components.
16. The preparation method according to claim 15, wherein: Based on the total amount of the active metal components, the content of one or more non-precious metal components of groups VB, VIII, IB, and IIB is 3-30% by weight; the content of the non-precious metal components of group VIIB is 3-20% by weight.
17. The preparation method according to claim 16, wherein: Based on the total amount of the active metal components, the content of one or more non-precious metal components of groups VB, VIII, IB, and IIB is 5-20% by weight; the content of the non-precious metal components of group VIIB is 5-15% by weight.
18. The preparation method according to claim 1, wherein: The organic acid is selected from at least one of citric acid and acetic acid.
19. The preparation method according to claim 18, wherein: The organic acid is citric acid.
20. The preparation method according to claim 1, wherein: The molar ratio of the organic acid to the solution calculated as metal ions is (1-10):
1.
21. The preparation method according to claim 1, wherein: The concentration of the organic acid solution is 0.01-3 mol / L.
22. The preparation method according to claim 1, wherein: The mixing conditions in step (2) include: stirring, pH 4-7, and temperature 50-90°C.
23. The preparation method according to claim 22, wherein: The mixing conditions in step (2) include: stirring, pH 5-6, and temperature 65-80°C.
24. The preparation method according to claim 1, wherein The solid content of the slurry in step (3) is 5-40% by weight.
25. The preparation method according to claim 1, wherein: In step (5), the noble metal component precursor is hydrolyzed in an acid solution to provide the impregnation solution.
26. The preparation method according to claim 25, wherein: In step (5), the acid is selected from inorganic acids and / or organic acids soluble in water.
27. The preparation method according to claim 26, wherein: In step (5), the acid is selected from at least one of hydrochloric acid, nitric acid, phosphoric acid and acetic acid.
28. The preparation method according to claim 25, wherein: In step (5), the amount of the acid used is such that the pH value of the impregnation solution is less than 6.
0.
29. The preparation method according to claim 28, wherein In step (5), the amount of acid used is such that the pH value of the impregnation solution is 2-5.
30. The preparation method according to claim 1, wherein: The conditions for the calcination in step (2), the calcination in step (4) for preparing the first composition, and the calcination in step (5) for preparing the second composition each independently include: The process is carried out in an oxygen-containing atmosphere at a temperature of 350-750°C and a time of 0.1-6h.
31. The preparation method according to claim 1, wherein The reducing atmosphere is provided by a reducing gas, and the concentration of the reducing gas is 1-20% by volume.
32. The preparation method according to claim 31, wherein The reducing gas is at least one of H2, CO and CH4.
33. The preparation method according to claim 32, wherein: The reducing gas is H2.
34. The preparation method according to claim 1, wherein The reduction treatment conditions include: temperature: 500-700℃, pressure: 0.05-4MPa, time not less than 1min, volume space velocity of reducing gas: 100-5000h -1 .
35. The preparation method according to claim 34, wherein: The conditions for the reduction treatment include: the time is 2-20 minutes.
36. A denitration catalyst with a regular structure prepared by the preparation method according to any one of claims 1 to 35.
37. The denitration catalyst with a regular structure according to claim 36 is used for deNOx in gas x Application in reaction.
38. A gas deNO x A method comprising: Will contain NO x The gas is contacted with a denitration catalyst, and the denitration catalyst is the denitration catalyst with a regular structure as described in claim 36.
39. The method of claim 38, wherein: Among the gases, NO x The content is 0.001-3% by volume.
40. The method of claim 38, wherein: The contact conditions include: temperature of 300-1000°C, reaction pressure of 0-0.5MPa, gas volume space velocity of 100-5000h -1 .
41. The method of claim 38, wherein: The gas is catalytic cracking regeneration flue gas.
42. The method of claim 38, wherein: The contact is carried out in a flue gas channel arranged after the cyclone separator and / or after the CO incinerator.
Citation Information
Patent Citations
Preparation method of supported type denitration catalyst
CN102658155A
Method for coating active component on cellular carrier with two open ends
CN1199733C
Flue gas treatments to reduce NOx and CO emissions
CN1688508A
Ferrierite compositions for reducing NOx emissions during fluid catalytic cracking
US20050100494A1
Catalyst for purifying automobile tail gas and preparation method thereof
CN101632930A