Surface bonding method of metal pipeline and fiber-reinforced ceramic matrix composite material
By performing hydrophobizing pretreatment of the metal pipeline and heating treatment with silica sol brush coating, combined with high-temperature adhesive, and using fiber braided sleeves as medium, the metal pipeline and fiber-reinforced ceramic matrix composite materials are solved under high temperature environments. The problem of debonding achieves a firm bonding effect under thermal shock conditions.
Patent Information
- Application Number
- CN202211542946.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-02
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-12-02
AI Technical Summary
In the prior art, metal pipes and fiber-reinforced ceramic matrix composites are prone to debonding due to insufficient bonding temperature resistance in high temperature environments, which limits the actual application temperature range of sensor products.
The metal pipe is pre-treated by hydrophobizing and pre-treating, and then passing it through the fiber braided sleeve and brushing the silica sol. After heating, it forms a composite material. Then, the metal pipe and fiber are used to use a high-temperature adhesive. Reinforced ceramic matrix composite bonding, connecting both through a fiber braided sleeve as an intermediate medium.
It effectively avoids the debonding problem caused by mismatch in thermal expansion coefficients, improves the high temperature strength of the connection, and allows the metal pipes and fiber-reinforced ceramic matrix composites to be firmly bonded after multiple thermal shocks.
Smart Images

Figure CN115805747B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite materials, and in particular to a surface bonding method of a metal pipeline and a fiber-reinforced ceramic-based composite material. Background Art
[0002] Fiber-reinforced ceramic-based composite materials are widely used in wave-transmitting and heat-insulating products such as antenna covers and antenna windows due to their excellent mechanical strength and temperature resistance. The metal pipes of sensors are often laid on the surfaces of the above-mentioned products to measure ambient air pressure, temperature and other parameters.
[0003] In the prior art, in order to avoid structural damage caused by grooving or punching the surface of ceramic-based composite materials, metal pipes are often fixed to the surface of ceramic-based composite materials by adhesive bonding. However, in actual applications, metal pipes and fiber-reinforced ceramic-based composite materials are prone to debonding due to insufficient bonding temperature resistance under thermal shock conditions, which seriously restricts the actual application temperature range of sensor products. Therefore, it is necessary to study a high-temperature resistant surface bonding method for metal pipes and fiber-reinforced ceramic-based composite materials. Summary of the invention
[0004] The present invention provides a surface bonding method for a metal pipeline and a fiber-reinforced ceramic-based composite material, which can ensure that the metal pipeline and the fiber-reinforced ceramic-based composite material are not prone to debonding in a high-temperature environment and can still be firmly bonded after undergoing multiple thermal shocks.
[0005] The present invention provides a surface bonding method for a metal pipeline and a fiber-reinforced ceramic matrix composite material, the bonding method comprising:
[0006] (1) using a release agent to perform hydrophobic pretreatment on the surface of the metal pipeline to obtain a pretreated metal pipeline;
[0007] (2) after passing the pretreated metal pipeline through a fiber braided sleeve, brushing silica sol on the surface of the fiber braided sleeve to obtain a first metal pipeline;
[0008] (3) heating the first metal pipeline to obtain a second metal pipeline;
[0009] (4) Adhesive is used to bond the surface of the second metal pipeline to the surface of the fiber-reinforced ceramic matrix composite material, thereby completing the surface bonding of the metal pipeline and the fiber-reinforced ceramic matrix composite material.
[0010] Preferably, in step (1), the metal pipeline is a stainless steel metal pipeline or a high temperature resistant alloy pipeline.
[0011] Preferably, in step (1): the release agent is at least one of polytetrafluoroethylene, methyl silicone oil or liquid paraffin.
[0012] Preferably, in step (2), the fiber braided sleeve is a quartz fiber braided sleeve, a high silica fiber braided sleeve or an alumina fiber braided sleeve.
[0013] Preferably, in step (2), in step (1), the inner diameter of the fiber braided sleeve is 1 to 2 mm larger than the diameter of the metal pipe.
[0014] Preferably, in step (2), the fiber braided sleeve has a braiding mesh number greater than 25 meshes and a thickness of 0.4 to 0.6 mm.
[0015] Preferably, in step (2), the density of the silica sol is 1.13-1.15 g / cm 3 ; The silica sol is applied 6 to 9 times.
[0016] Preferably, in step (3), the heating treatment is carried out at a temperature of 240 to 260° C. and for a time of 0.8 to 1.2 h.
[0017] Preferably, in step (3), the adhesive is at least one of KH-PSON-1 high temperature adhesive and KH-PSNBA-1 high temperature adhesive.
[0018] Preferably, in step (3), the fiber-reinforced ceramic matrix composite material is at least one of a quartz fiber-reinforced ceramic matrix composite material, an alumina fiber-reinforced ceramic matrix composite material or a silicon nitride fiber-reinforced ceramic matrix composite material.
[0019] Compared with the prior art, the present invention has at least the following beneficial effects:
[0020] (1) The present invention firstly uses a fiber braided tube sleeve to wrap the metal pipe after surface hydrophobic pretreatment, and brushes silica sol on the surface of the wrapped fiber braided tube sleeve. After heating treatment, the fiber braided tube sleeve can form a composite material with the silica sol on the surface of the metal pipe. Finally, an adhesive is used to bond the fiber braided tube sleeve wrapped with the metal pipe and the fiber reinforced ceramic matrix composite material together. The presence of the fiber braided tube sleeve can serve as an intermediate medium to connect the metal pipe and the fiber reinforced ceramic matrix composite material together, preventing the metal pipe and the composite material substrate from being directly connected through the adhesive, thereby avoiding the debonding problem caused by the mismatch of thermal expansion coefficients between the metal pipe and the fiber reinforced ceramic matrix composite material under thermal shock conditions. After the fiber braided tube forms a composite material, the high-temperature strength of the tube is significantly improved, thereby enabling the connected metal pipe and the fiber reinforced ceramic matrix composite material to remain firmly bonded after undergoing multiple thermal shocks;
[0021] (2) In some preferred embodiments of the present invention, the inner diameter of the fiber braided sleeve is larger than the diameter of the metal pipe, which is beneficial for the metal pipe to expand freely in the fiber braided sleeve under high temperature environment, thereby further ensuring the bonding performance between the metal pipe and the fiber reinforced ceramic matrix composite material under thermal shock conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0023] Figure 1 The present invention provides a flow chart of a surface bonding method for a metal pipeline and a fiber-reinforced ceramic matrix composite material. DETAILED DESCRIPTION
[0024] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0025] In the prior art, the metal pipe of the sensor is usually directly bonded to the fiber-reinforced ceramic matrix composite material by glue. However, the thermal expansion coefficient of the metal pipe as a metal material is relatively large, while the thermal expansion coefficient of the fiber-reinforced ceramic matrix composite material is relatively small. Therefore, under high temperature environment or thermal shock conditions, the metal pipe and the fiber-reinforced ceramic matrix composite material as the substrate are prone to debonding due to the mismatch in thermal expansion coefficients, which greatly limits the practical use of the sensor. In view of this, if Figure 1 As shown, an embodiment of the present invention provides a surface bonding method for a metal pipeline and a fiber-reinforced ceramic matrix composite material, the bonding method comprising:
[0026] (1) using a release agent to perform hydrophobic pretreatment on the surface of the metal pipeline to obtain a pretreated metal pipeline;
[0027] (2) after passing the pretreated metal pipeline through a fiber braided sleeve, brushing silica sol on the surface of the fiber braided sleeve to obtain a first metal pipeline;
[0028] (3) heating the first metal pipeline to obtain a second metal pipeline;
[0029] (4) Adhesive is used to bond the surface of the second metal pipeline to the surface of the fiber-reinforced ceramic matrix composite material, thereby completing the surface bonding of the metal pipeline and the fiber-reinforced ceramic matrix composite material.
[0030] The present invention firstly uses a fiber braided tube sleeve to wrap the metal pipe after surface hydrophobic pretreatment, and brushes silica sol on the surface of the wrapped fiber braided tube sleeve. After heating treatment, the fiber braided tube sleeve can form a composite material with the silica sol on the surface of the metal pipe. Finally, an adhesive is used to bond the fiber braided tube sleeve wrapped with the metal pipe and the fiber reinforced ceramic-based composite material. The presence of the fiber braided tube sleeve can serve as an intermediate medium to connect the metal pipe and the fiber reinforced ceramic-based composite material together, thereby isolating the metal pipe and the fiber reinforced ceramic-based composite material with a large difference in thermal expansion coefficient from being directly bonded by the adhesive, thereby effectively avoiding the debonding problem caused by the mismatch of thermal expansion coefficients between the metal pipe and the fiber reinforced ceramic-based composite material under thermal shock conditions, and enabling the connected metal pipe and the fiber reinforced ceramic-based composite material to still be firmly bonded after undergoing multiple thermal shocks; at the same time, by brushing silica sol on the surface of the fiber braided tube sleeve and heating it to form a composite material, the disadvantage of the simple fiber braided tube having serious performance attenuation in a high temperature environment is effectively overcome.
[0031] According to some preferred embodiments, in step (1), the metal pipeline is a stainless steel metal pipeline or a high temperature resistant alloy pipeline.
[0032] In the present invention, the metal pipeline includes but is not limited to the above-mentioned types of metal materials, and may also be other types of high-temperature resistant alloy pipelines. At the same time, the shape of the metal pipeline is not limited to a circle, for example, it may also be a square tube or other shapes of metal materials.
[0033] According to some preferred embodiments, in step (1), the release agent is at least one of polytetrafluoroethylene, methyl silicone oil or liquid paraffin.
[0034] Before the fiber braided tube sleeve is used to wrap the metal pipe, the present invention firstly applies a release agent on the surface of the metal pipe. The present invention has no specific requirements on the coating thickness of the release agent, which is generally less than 0.1 mm. After the release agent is applied to the surface of the metal pipe, the release agent coating can form a hydrophobic surface for the metal pipe, thereby effectively preventing the silica sol or adhesive from passing through the gap of the fiber braided tube sleeve to bond the metal pipe and the fiber braided tube sleeve together.
[0035] According to some preferred embodiments, in step (2), the fiber braided sleeve is a quartz fiber braided sleeve, a high silica fiber braided sleeve or an alumina fiber braided sleeve.
[0036] According to some preferred embodiments, in step (2), the inner diameter of the fiber braided sleeve is 1 to 2 mm larger than the diameter of the metal pipe (for example, it may be 1 mm, 1.2 mm, 1.5 mm, 1.8 mm or 2 mm).
[0037] In the present invention, a fiber braided sleeve is first used to wrap the metal pipe. On the one hand, the fiber braided sleeve can play the role of fixing the metal pipe, and on the other hand, it can act as an intermediate medium to bond with the fiber-reinforced ceramic-based composite material. Because the thermal expansion coefficient of the fiber braided sleeve is slightly different from that of the fiber-reinforced ceramic-based composite material, it can avoid the direct contact between the metal pipe with a large difference in thermal expansion coefficient and the fiber-reinforced ceramic-based composite material, thereby effectively avoiding the debonding problem caused by the mismatch of thermal expansion coefficients under thermal shock environment. The fiber braided sleeve should have good mechanical properties and high temperature resistance. In the present invention, the fiber braided sleeve is preferably a quartz fiber braided sleeve; at the same time, the inner diameter of the fiber braided sleeve in the present invention should be greater than 1 to 2 mm of the diameter of the metal pipe, so that the fiber braided sleeve can not only better fix the metal pipe, but also enable the metal pipe in the fiber braided sleeve to expand freely under high temperature environment or thermal shock conditions, thereby further ensuring the excellent bonding performance between the fiber braided sleeve and the fiber-reinforced ceramic-based composite material. It should be noted that the diameter of the metal pipe is the maximum distance between the two edges of the metal pipe.
[0038] According to some preferred embodiments, in step (2), the fiber braided sleeve has a braiding mesh greater than 25 (for example, 25, 30, 35 or 40 mesh) and a thickness of 0.4 to 0.6 mm (for example, 0.4, 0.5 or 0.6 mm).
[0039] In the present invention, the mesh number and thickness of the fiber tube sleeve are controlled within the above range, which can ensure that the fiber braided tube sleeve has certain mechanical properties and high temperature resistance. At the same time, the mesh number of the fiber braided tube sleeve can prevent the silica sol from penetrating into the surface of the metal pipe in large quantities when spraying the silica sol, so that the metal pipe and the fiber braided tube sleeve are bonded together, thereby ensuring that the metal pipe can expand freely in the fiber braided tube sleeve under high temperature environment.
[0040] According to some preferred embodiments, in step (2), the density of the silica sol is 1.13-1.15 g / cm 3 (For example, it can be 1.13 g / cm3 , 1.14g / cm 3 or 1.15g / cm 3 ); the number of times the silica sol is brushed is 6 to 9 times (for example, 6 times, 7 times, 8 times or 9 times).
[0041] In the present invention, by brushing silica sol on the surface of the fiber braided sleeve and performing heat treatment, on the one hand, the silica sol can form a composite material with the fiber braided sleeve, effectively avoiding the problem of serious strength attenuation of the simple fiber braided sleeve in a high temperature environment, thereby ensuring that the fiber braided sleeve has good mechanical strength in a high temperature environment; on the other hand, the silica sol enables the fiber braided sleeve to be further densified, effectively avoiding the glue in the subsequent bonding process from passing through the gap of the fiber braided sleeve to bond the metal pipe and the fiber reinforced ceramic-based composite material together, so that the metal pipe cannot expand freely under a thermal shock environment, thereby causing debonding.
[0042] The present invention comprehensively controls the surface hydrophilicity and hydrophobicity of the metal pipe, the density of the silica sol, the number of times the silica sol is brushed, the mesh number and thickness of the fiber braided tube sleeve and other parameters, so as to not only ensure that the fiber braided tube sleeve has excellent mechanical properties and high temperature resistance, but also effectively prevent the silica sol or adhesive from bonding the metal pipe and the fiber braided tube sleeve together, so that the metal pipe can expand freely in the fiber braided tube sleeve under high temperature environment, and further ensure that the metal pipe and the fiber reinforced ceramic matrix composite material can still be firmly bonded after being subjected to multiple thermal shocks.
[0043] It should also be noted that in the present invention, each time after the silica sol is brushed on the surface of the fiber braided tube sleeve, the fiber braided tube sleeve wrapping the metal pipeline (ie, the first metal pipeline) can be placed in an oven at 50-80° C. to dry for 1 hour.
[0044] According to some preferred embodiments, in step (3), the heating treatment is carried out at a temperature of 240 to 260°C (for example, 240°C, 245°C, 250°C, 255°C or 260°C), and the heating time is 0.8 to 1.2h (for example, 0.8h, 0.9h, 1.0h, 1.1h or 1.2h).
[0045] The present invention uses high-temperature heating treatment to further dehydrate and densify the silica sol on the surface of the fiber braided tube sleeve, and tightly combine with the fibers of the fiber braided tube sleeve, thereby effectively improving the mechanical strength of the fiber braided tube sleeve.
[0046] According to some preferred embodiments, in step (4), the adhesive is at least one of KH-PSON-1 high temperature adhesive and KH-PSNBA-1 high temperature adhesive. The high temperature adhesive in the present invention is purchased from the Beijing Institute of Chemistry, Chinese Academy of Sciences.
[0047] When using an adhesive to bond the fiber sleeve wrapping the metal pipe to the surface of the fiber-reinforced ceramic-based composite material, the adhesive can be applied to the connecting surface of the fiber braided sleeve and / or the connecting surface of the fiber-reinforced ceramic-based composite material, and the connecting surface of the fiber braided sleeve and the connecting surface of the fiber-reinforced ceramic-based composite material are tightly fitted together and a certain pressure is applied, thereby completing the surface bonding of the metal pipe and the fiber-reinforced ceramic-based composite material.
[0048] It should be noted that the types of adhesives in the present invention include but are not limited to the above-mentioned types of adhesives. In actual application, those skilled in the art can select the corresponding type of adhesive according to the actual environment and bonding strength requirements.
[0049] According to some preferred embodiments, in step (3), the fiber-reinforced ceramic matrix composite material is at least one of a quartz fiber-reinforced ceramic matrix composite material, an alumina fiber-reinforced ceramic matrix composite material, or a silicon nitride fiber-reinforced ceramic matrix composite material. In the present invention, a quartz fiber-reinforced ceramic matrix composite material is preferred.
[0050] In order to more clearly illustrate the technical solution and advantages of the present invention, a surface bonding method of a metal pipeline and a fiber-reinforced ceramic matrix composite material is described in detail below through several embodiments.
[0051] Embodiment 1:
[0052] (1) Spraying polytetrafluoroethylene coating on the surface of a stainless steel metal pipeline with a length of 1 m and a diameter of 2 mm, and curing at 250° C. for 30 min to obtain a pretreated stainless steel metal pipeline;
[0053] (2) The pretreated stainless steel metal pipe is passed through a quartz fiber braided sleeve with an inner diameter of 3 mm and a density of 1.14 g / cm 3 The industrial-grade silica sol is brushed on the surface of the quartz fiber braided sleeve for 8 times, and the sleeve is placed in an oven at 60° C. and dried for 1 hour to obtain a first metal pipeline; wherein the quartz fiber braided sleeve has a braiding mesh number of 30 meshes and a thickness of 0.5 mm;
[0054] (3) heating the first metal pipeline at 250° C. for 1 h to obtain a second metal pipeline;
[0055] (4) Apply KH-PSON-1 high temperature adhesive to the connection surface of the second metal pipe, and then tightly fit the connection surface of the second metal pipe and the connection surface of the quartz fiber reinforced composite material together and apply a pressure of 1 KPa to complete the surface bonding of the metal pipe and the fiber reinforced composite material.
[0056] The metal pipe and the fiber-reinforced ceramic-based composite material bonded together in Example 1 were placed at 800°C and kept warm for 10 minutes without falling off, and the metal pipe and the fiber-reinforced ceramic-based composite material were still firmly bonded after undergoing 5 heating-cooling thermal shock cycles; wherein the temperature was increased from room temperature (25°C) to 800°C at a rate of 10°C / s, maintained for 10 minutes, and then naturally cooled from 800°C to room temperature (25°C), which is one heating-cooling thermal shock cycle.
[0057] Embodiment 3:
[0058] (1) Spraying a release agent polytetrafluoroethylene coating on the surface of a high-temperature resistant alloy metal pipeline with a length of 1 m and a diameter of 3 mm, and curing it at 250° C. for 30 min to obtain a pretreated high-temperature resistant alloy metal pipeline;
[0059] (2) After the pretreated high-temperature resistant alloy metal pipe is passed through a quartz fiber braided sleeve with an inner diameter of 4 mm, a density of 1.15 g / cm 3 The industrial-grade silica sol is brushed on the surface of the quartz fiber braided sleeve for 7 times, and the sleeve is placed in an oven at 80° C. and dried for 1 hour to obtain a first metal pipeline; wherein the braiding mesh number of the quartz fiber braided sleeve is 35 meshes and the thickness is 0.4 mm;
[0060] (3) heating the first metal pipeline at 240° C. for 1.2 h to obtain a second metal pipeline;
[0061] (4) Apply KH-PSNBA-1 high temperature adhesive to the connection surface of the second metal pipe, and then fit the connection surface of the second metal pipe and the connection surface of the quartz fiber reinforced composite material tightly together and apply pressure to complete the surface bonding of the metal pipe and the fiber reinforced ceramic matrix composite material.
[0062] The metal pipe and the fiber-reinforced ceramic-based composite material bonded together in Example 2 were placed at 800°C and kept warm for 10 minutes without falling off, and the metal pipe and the fiber-reinforced ceramic-based composite material were still firmly bonded after undergoing 5 heating-cooling thermal shock cycles; wherein the temperature was increased from room temperature (25°C) to 800°C at a rate of 10°C / s, maintained for 10 minutes, and then naturally cooled from 800°C to room temperature (25°C), which is a heating-cooling thermal shock cycle.
[0063] Embodiment 3:
[0064] Example 3 is basically the same as Example 1, except that in step (1), the release agent sprayed on the surface of the metal pipe is methyl silicone oil, and the fiber braided sleeve is an alumina fiber braided sleeve.
[0065] The metal pipe and the fiber-reinforced ceramic-based composite material bonded together in Example 3 were placed at 800°C and kept warm for 10 minutes without falling off, and the metal pipe and the fiber-reinforced ceramic-based composite material were still firmly bonded after undergoing 5 heating-cooling thermal shock cycles; wherein, heating from room temperature (25°C) to 800°C at a rate of 10°C / s, maintaining for 10 minutes, and then naturally cooling from 800°C to room temperature (25°C) is one heating-cooling thermal shock cycle.
[0066] Embodiment 4:
[0067] Example 4 is basically the same as Example 1, except that in step (1), the inner diameter of the quartz fiber braided sleeve is 4.5 mm.
[0068] The metal pipe and the fiber-reinforced ceramic matrix composite material bonded together in Example 5 were placed at 800°C for 10 minutes without falling off. However, the inner diameters of the metal pipe and the quartz fiber braided sleeve were quite different, and the metal pipe was poorly fixed in the fiber braided sleeve.
[0069] Comparative Example 1:
[0070] KH-PSON-1 high-temperature adhesive was applied on the connection surface of a stainless steel metal pipe with a length of 1m and a diameter of 2mm. Then, the connection surface of the stainless steel metal pipe and the connection surface of the quartz fiber reinforced composite material were tightly fitted together and a pressure of 1KPa was applied to complete the surface bonding of the metal pipe and the fiber reinforced ceramic matrix composite material.
[0071] The metal pipe and the fiber-reinforced ceramic matrix composite material bonded together in Comparative Example 1 were heated at 800° C. for 3 minutes and then debonding occurred.
[0072] Comparative Example 2:
[0073] Comparative Example 2 is substantially the same as Example 1, except that, in step (2), after the pretreated stainless steel metal pipe is passed through the quartz fiber braided tube sleeve, the silica sol is not used for brushing, and the first metal pipe is directly obtained; KH-PSON-1 high temperature adhesive is applied to the connecting surface of the first metal pipe, and then the connecting surface of the first metal pipe and the connecting surface of the quartz fiber reinforced composite material are tightly fitted together and a pressure of 1 KPa is applied to complete the surface bonding of the metal pipe and the fiber reinforced composite material.
[0074] After the metal pipe and fiber-reinforced ceramic matrix composite material bonded together in Comparative Example 2 were placed at 800°C for 10 minutes, the quartz fiber braided tube sheath became partially brittle and local debonding occurred. After 5 heating-cooling thermal shock cycles, it was completely debonded.
[0075] Comparative Example 3:
[0076] Comparative Example 3 is substantially the same as Example 1, except that step (1) is omitted, that is, the stainless steel metal pipe that has not been pretreated is directly passed through a quartz fiber braided sleeve with an inner diameter of 3 mm.
[0077] The metal pipe and the fiber-reinforced ceramic matrix composite material bonded together in Comparative Example 3 were placed at 800° C. and heated for 10 minutes, and then fell off.
[0078] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A surface bonding method for a metal pipeline and a fiber-reinforced ceramic matrix composite material, characterized in that: The bonding method comprises: (1) using a release agent to perform hydrophobic pretreatment on the surface of the metal pipeline to obtain a pretreated metal pipeline; (2) After the pretreated metal pipeline passes through a fiber braided sleeve, silica sol is brushed on the surface of the fiber braided sleeve to obtain a first metal pipeline; the braiding mesh number of the fiber braided sleeve is greater than 25 meshes and the thickness is 0.4 to 0.6 mm; the density of the silica sol is 1.13 to 1.15 g / cm 3 ; The number of times the silica sol is brushed is 6 to 9 times; the inner diameter of the fiber braided sleeve is 1 to 2 mm larger than the diameter of the metal pipe; (3) heating the first metal pipeline to obtain a second metal pipeline; the heating treatment temperature is 240 to 260° C., and the time is 0.8 to 1.2 h; (4) Adhesive is used to bond the surface of the second metal pipeline to the surface of the fiber-reinforced ceramic matrix composite material, thereby completing the surface bonding of the metal pipeline and the fiber-reinforced ceramic matrix composite material.
2. The bonding method according to claim 1, characterized in that: In step (1): the metal pipeline is a stainless steel metal pipeline or a high temperature resistant alloy pipeline.
3. The bonding method according to claim 1, characterized in that: In step (1): the release agent is at least one of polytetrafluoroethylene, methyl silicone oil or liquid paraffin.
4. The bonding method according to claim 1, characterized in that: In step (2): the fiber braided sleeve is a quartz fiber braided sleeve, a high silica fiber braided sleeve or an alumina fiber braided sleeve.
5. The bonding method according to claim 1, characterized in that: In step (4): the adhesive is at least one of KH-PSON-1 high temperature adhesive and KH-PSNBA-1 high temperature adhesive.
6. The bonding method according to any one of claims 1 to 5, characterized in that: In step (4): the fiber-reinforced ceramic matrix composite material is at least one of a quartz fiber-reinforced ceramic matrix composite material, an alumina fiber-reinforced ceramic matrix composite material or a silicon nitride fiber-reinforced ceramic matrix composite material.