Graphene-coated metal particles and preparation method thereof
Through high-temperature heat treatment and instantaneous high current treatment, graphene-coated metal particles were successfully prepared, solving the problems of long-term operation of high temperatures and difficulty in deposition of carbon in the prior art, and achieving the improvement of high conductivity and mechanical strength. At the same time, energy consumption and risk are reduced.
Patent Information
- Application Number
- CN202211513562.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-29
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2042-11-29
AI Technical Summary
In the existing preparation method of graphene-coated metal particles, the chemical vapor deposition method requires long-term operation at high temperature, which is time-consuming and energy-consuming, and is difficult to avoid agglomeration between metal particles and difficulty in deposition of carbon at low temperatures.
Carbon-coated metal particles are obtained by high-temperature heat treatment, and the high temperature generated by instantaneous high current is used to convert carbon into graphene in a short time to prepare graphene-coated metal particles.
It avoids the inconvenience of long-term heating of high temperatures, improves the electrical conductivity and mechanical strength of the product, and reduces the energy consumption and danger of the preparation process.
Smart Images

Figure CN115815592B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of graphene metal materials, and in particular to a graphene-coated metal particle and a preparation method thereof. Background Art
[0002] Metal particles (such as copper particles) have broad application prospects in the fields of electronics, electrical appliances, and defense industry due to their high electrical and thermal conductivity. However, single metal particles are often limited in application due to their own shortcomings (such as copper particles are easily oxidized).
[0003] Graphene is a carbon atom in the form of sp 2 Two-dimensional carbon nanomaterials with hybrid orbitals forming hexagonal honeycomb lattices have excellent properties such as extremely high mechanical strength and ultra-high carrier mobility, and are believed to have broad application prospects in many fields.
[0004] Graphene-coated metal particles can solve the above problems (for example, graphene-coated copper particles can solve the easy oxidation of copper, improve its conductivity, increase its heat dissipation, and improve its mechanical strength). Currently, graphene-coated metal particles mainly use chemical vapor deposition to grow graphene layers on the surface of metal particles. The preparation involves gaseous carbon sources and high-temperature furnaces that are used at high temperatures for a long time, which is time-consuming and energy-consuming, and the use of gaseous carbon sources is relatively dangerous. In addition, high temperatures easily cause metal particles to agglomerate into blocks. At low temperatures, the cracking temperature of the carbon source often cannot be reached, making it difficult for carbon to deposit on the metal particles, or the carbon source cracked at low temperatures only exists on the metal surface in the form of amorphous carbon, and it is impossible to truly obtain graphene-coated metal particles.
[0005] In the prior art, a carbon layer / graphene layer is coated on the surface of metal particles by chemical vapor deposition (CVD); or metal particles and a carbon source are heated in an ordinary high-temperature furnace to prepare graphene-coated metal particles.
[0006] For CVD, a gaseous carbon source is generally used. The cracking temperature of the gaseous carbon source is high, such as methane. The temperature must be above 1000K to obtain a large cracking rate, close to the melting point of copper. The metal copper melts and no longer has a particle morphology. Or it can be operated through a high-temperature furnace, but this method can only obtain carbon-coated metal particles, and the product has low conductivity. The advantages of the present invention are: 1) It avoids high-temperature and long-term heating of CVD and avoids metal melting (such as Cu), 2) The product has better conductivity than the product obtained by high-temperature furnace treatment. Summary of the invention
[0007] The present invention utilizes high-temperature heat treatment to obtain carbon-coated metal particles (metal particles @ carbon), and converts the carbon on the surface of the metal particles into graphene in a short time through the high temperature (>2000°C) generated by instantaneous large current, thereby obtaining graphene-coated metal particles (metal particles @ graphene).
[0008] To achieve the above-mentioned purpose of the invention, the technical solution of the present invention is as follows:
[0009] A method for preparing graphene-coated metal particles comprises the following steps:
[0010] (1) Preparation of carbon-coated metal micro- or nanoparticles: a carbon source and a metal salt are mixed, the mass ratio of the metal salt to the carbon source being 1:(0.5-3), the two are mixed evenly by grinding or ball milling, and then heat-treated in a high-temperature furnace at 200-900°C for 30-240 minutes to obtain a metal particle@carbon material, which is a carbon-based material with carbon-coated metal micro- or nanoparticles grown on it;
[0011] (2) Preparation of graphene-coated metal particles: The metal particles@carbon material are placed in a quartz tube, both ends of which are blocked with copper wire or carbon cloth and then placed in a reaction chamber for treatment. The two ends of the reactant are connected to the positive and negative electrodes of the power supply, the reaction chamber is evacuated, and the sample is discharged at a voltage of 30-220V for 50-1000ms to obtain a graphene-coated metal particle material.
[0012] As a preferred embodiment, the mass ratio of the metal salt to the carbon source in step (1) is 1:1 or 1:2 or 2:1.
[0013] Among them, when the mass ratio of metal salt to carbon source is 2:1, the metal proportion is the largest and the product conductivity is the best;
[0014] When the mass ratio of metal salt to carbon source is 1:1, the metal ratio is in the middle;
[0015] When the mass ratio of metal salt to carbon source is 1:2, the metal accounts for the smallest proportion, the cheap carbon accounts for a large proportion, and the product is the cheapest; although the conductivity is worse than 2:1, because the Joule heat treatment converts carbon into graphene, the conductivity of the final product will not be too bad;
[0016] As a preferred embodiment, the carbon source is selected from glucose, sucrose, and a polymer;
[0017] And / or the metal salt is selected from basic copper carbonate, copper acetate, basic nickel carbonate.
[0018] As a preferred embodiment, in step (1), the content of metal particles in the metal particles@carbon material is adjusted by adjusting the ratio of the carbon source to the metal salt;
[0019] By increasing the mass proportion of metal salt in the raw materials, the metal proportion in the final product is increased, and the conductivity of the final product is increased.
[0020] As a preferred embodiment, when the heat treatment temperature in step (1) is 750°C, the number of discharges in step (2) is 2 times, the first time being a low voltage pretreatment with a voltage less than or equal to 110V to reduce the resistance of the reactants to a few ohms; the second time being a formal Joule heat treatment with a voltage greater than 110V. In the first discharge pretreatment, the resistance of the sample is reduced to a few ohms, so that the instantaneous current in the second discharge can be maximized, the instantaneous Joule heat generated can be maximized, and the carbon layer on the surface of the metal particles can be more fully transformed into graphene.
[0021] As a preferred embodiment, in step (2), the sample is discharged at a voltage of 150 V for a period of 400 ms.
[0022] The reason for this setting is: if the voltage is too high, energy will be wasted. If the voltage is too low, the energy will be too little to fully transform carbon into graphene. If the discharge time is too short, the voltage cannot be completely reduced to 0V, and there will be residual voltage, wasting energy. If the discharge time is too long, time will be wasted. Under 150V voltage, 400ms time is the preferred solution. The transformation of metal particles @ carbon to metal particles @ graphene is very sufficient without wasting too much electricity.
[0023] In step (2), when the discharge time is appropriate (300-1000 ms), the greater the discharge voltage, the smaller the resistance of the sample, the greater the instantaneous current during the reaction, and the more complete the final transformation of metal particles @ carbon to metal particles @ graphene.
[0024] As a preferred embodiment, the heat treatment in step (1) is carried out in different temperature sections in a step-by-step manner. In the first temperature section, heat pretreatment is carried out to first react the metal salt with the carbon source; after the temperature is raised, heat treatment is carried out in the second temperature section to achieve the graphitization transformation process of the carbon.
[0025] And / or the heat treatment in step 1, by increasing the heat treatment temperature in the second temperature section, to improve the conductivity of the intermediate product metal particles @ carbon.
[0026] As a preferred embodiment, step (1) is specifically:
[0027] Weigh 6.66 g of glucose and 3.33 g of monohydrated copper carbonate, grind for 15 min to mix the two evenly, and perform heat pretreatment before heat treatment. The heat pretreatment is as follows: heat from room temperature to 335°C at a heating rate of 5°C / min, with 200 sccm argon as protective gas, and heat treatment for 60 min;
[0028] Then, heat treatment was performed: the temperature was raised from 335°C to 750°C at a heating rate of 5°C / min, 200 sccm argon was used as the protective gas, and the treatment lasted for 60 minutes.
[0029] As a preferred embodiment, step (2) is specifically:
[0030] Weigh 180 mg of the metal particles@carbon material prepared in step (1) and place them in a quartz tube with a length of 50 mm, an inner diameter of 4 mm, and an outer diameter of 6 mm. After blocking both ends with fine copper wires, place them in a reaction chamber, connect the positive and negative electrodes at both ends, evacuate the reaction chamber, and discharge the sample at a voltage of 150 V for 400 ms. When the voltage drops to 0 V, graphene-coated metal particles are obtained.
[0031] The present invention also provides graphene-coated metal particles obtained by the preparation method.
[0032] The inventive principle of the present invention is:
[0033] In the first step, the carbon source and the metal salt are heat-treated, and the carbon source reduces the metal oxide decomposed by the metal salt into metal particles, thereby obtaining metal particles @ carbon. At the same time, the heat treatment increases the graphitization degree of the carbon layer on the surface of the metal particles, increases the conductivity of the metal particles @ carbon, and is beneficial to the discharge treatment.
[0034] In the second step, the energy generated by the instantaneous large current causes the carbon atoms on the surface of the metal particles @ carbon to rearrange to form graphene, and allows the incompletely reduced metal oxides to be further reduced to metal particles, and finally metal particles @ graphene are obtained.
[0035] The beneficial effects of the present invention are:
[0036] (1) The raw materials are metal salts and carbon sources, which are low in cost and can be mass-produced.
[0037] (2) By adjusting the ratio of metal salt and carbon source, products with different metal proportions can be obtained, which are suitable for different application scenarios.
[0038] (3) Compared with chemical vapor deposition, it takes less time.
[0039] (4) The Joule heat generated during discharge directly acts on the reactants, resulting in high energy utilization.
[0040] (5) The temperature is high during discharge, and high-quality metal particles@graphene can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 This is an electron microscope image of the carbon-coated metal micro- or nanoparticles prepared in step (1).
[0042] Figure 2 This is an electron microscope image of the graphene-coated metal particles prepared in step (2). DETAILED DESCRIPTION
[0043] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.
[0044] Example 1
[0045] This embodiment provides a method for preparing graphene-coated metal particles, comprising the following steps:
[0046] (1) Preparation of carbon-coated metal micro- or nanoparticles: a carbon source and a metal salt are mixed, with the mass ratio of metal salt to carbon source being 1:0.5, and the two are mixed evenly by grinding or ball milling, and then heat-treated in a high-temperature furnace at 220°C for 30 minutes to obtain a metal particle@carbon material, which is a carbon-based material with carbon-coated metal micro- or nanoparticles grown on it;
[0047] The carbon source is selected from glucose;
[0048] The metal salt is selected from basic copper carbonate.
[0049] In step (1), the content of metal particles in the metal particles@carbon material is adjusted by adjusting the ratio of the carbon source to the metal salt;
[0050] By increasing the mass proportion of metal salt in the raw materials, the metal proportion in the final product is increased, and the conductivity of the final product is increased.
[0051] The heat treatment in step (1) is carried out in different temperature sections in a step-by-step manner. In the first temperature section, heat pretreatment is carried out to first react the metal salt with the carbon source; after the temperature is raised, heat treatment is carried out in the second temperature section to achieve the graphitization transformation process of the carbon.
[0052] The heat treatment in step 1 improves the conductivity of the intermediate product metal particles@carbon by increasing the heat treatment temperature in the second temperature section.
[0053] (2) Preparation of graphene-coated metal particles: The metal particles@carbon material are placed in a quartz tube, both ends of which are blocked with copper wire or carbon cloth and then placed in a reaction chamber for treatment. The two ends of the reactant are connected to the positive and negative electrodes of the power supply, the reaction chamber is evacuated, and the sample is discharged at a voltage of 30 V for 50 ms to obtain the graphene-coated metal particle material.
[0054] Example 2
[0055] This embodiment provides a method for preparing graphene-coated metal particles, comprising the following steps:
[0056] (1) Preparation of carbon-coated metal micro- or nanoparticles: a carbon source and a metal salt are mixed, with the mass ratio of metal salt to carbon source being 1:1, and the two are mixed evenly by grinding or ball milling, and then heat-treated in a high-temperature furnace at 900°C for 240 minutes to obtain a metal particle@carbon material, which is a carbon-based material with carbon-coated metal micro- or nanoparticles grown on it;
[0057] The carbon source is selected from glucose;
[0058] The metal salt is selected from basic copper carbonate.
[0059] In step (1), the content of metal particles in the metal particles@carbon material is adjusted by adjusting the ratio of the carbon source to the metal salt;
[0060] By increasing the mass proportion of metal salt in the raw materials, the metal proportion in the final product is increased, and the conductivity of the final product is increased.
[0061] The heat treatment in step (1) is carried out in different temperature sections in a step-by-step manner. In the first temperature section, heat pretreatment is carried out to first react the metal salt with the carbon source; after the temperature is raised, heat treatment is carried out in the second temperature section to achieve the graphitization transformation process of the carbon.
[0062] The heat treatment in step 1 improves the conductivity of the intermediate product metal particles@carbon by increasing the heat treatment temperature in the second temperature section.
[0063] Step (1) is specifically as follows:
[0064] Weigh 5 g of glucose and monohydrated copper carbonate, grind for 15 min to mix the two evenly, and perform heat pretreatment before heat treatment. The heat pretreatment is as follows: heat from room temperature to 335°C at a heating rate of 5°C / min, with 200 sccm argon as the protective gas, and heat treat for 60 min.
[0065] Then, heat treatment was performed: the temperature was raised from 335°C to 900°C at a heating rate of 5°C / min, 200sccm argon was used as a protective gas, and the metal particle@carbon material was obtained after treatment for 60 minutes.
[0066] (2) Preparation of graphene-coated metal particles: The metal particles@carbon material are placed in a quartz tube, both ends of which are blocked with copper wire or carbon cloth and then placed in a reaction chamber for treatment. The two ends of the reactant are connected to the positive and negative electrodes of the power supply, the reaction chamber is evacuated, and the sample is discharged for 1000 ms at a voltage of 220 V to obtain a graphene-coated metal particle material.
[0067] Example 3
[0068] This embodiment provides a method for preparing graphene-coated metal particles, comprising the following steps:
[0069] (1) Preparation of carbon-coated metal micro- or nanoparticles: a carbon source and a metal salt are mixed, with the mass ratio of metal salt to carbon source being 1:2, and the two are mixed evenly by grinding or ball milling, and then heat-treated in a high-temperature furnace at 750°C for 100 minutes to obtain a metal particle@carbon material, which is a carbon-based material with carbon-coated metal micro- or nanoparticles grown on it;
[0070] The carbon source is selected from sucrose;
[0071] The metal salt is selected from copper acetate.
[0072] In step (1), the content of metal particles in the metal particles@carbon material is adjusted by adjusting the ratio of the carbon source to the metal salt;
[0073] By increasing the mass proportion of metal salt in the raw materials, the metal proportion in the final product is increased, and the conductivity of the final product is increased.
[0074] The heat treatment in step (1) is carried out in different temperature sections in a step-by-step manner. In the first temperature section, heat pretreatment is carried out to first react the metal salt with the carbon source; after the temperature is raised, heat treatment is carried out in the second temperature section to achieve the graphitization transformation process of the carbon.
[0075] The heat treatment in step 1 improves the conductivity of the intermediate product metal particles@carbon by increasing the heat treatment temperature in the second temperature section.
[0076] (2) Preparation of graphene-coated metal particles: The metal particles@carbon material are placed in a quartz tube, both ends of which are blocked with copper wire or carbon cloth and then placed in a reaction chamber for treatment. The two ends of the reactant are connected to the positive and negative electrodes of the power supply, the reaction chamber is evacuated, and the sample is discharged at a voltage of 150 V for 400 ms to obtain graphene-coated metal particle material.
[0077] When the heat treatment temperature in step (1) is 750°C, the number of discharges in step (2) is 2 times. The first time is a low voltage pretreatment with a voltage less than or equal to 110V to reduce the resistance of the reactants to a few ohms; the second time is a formal Joule heat treatment with a voltage greater than 110V.
[0078] Step (2) is specifically as follows:
[0079] Weigh 180 mg of the metal particles@carbon material prepared in step (1) and place them in a quartz tube with a length of 50 mm, an inner diameter of 4 mm, and an outer diameter of 6 mm. After blocking both ends with fine copper wires, place them in a reaction chamber, connect the positive and negative electrodes at both ends, evacuate the reaction chamber, and discharge the sample at a voltage of 150 V for 400 ms. When the voltage drops to 0 V, graphene-coated metal particles are obtained.
[0080] Example 4
[0081] This embodiment provides a method for preparing graphene-coated metal particles, comprising the following steps:
[0082] (1) Preparation of carbon-coated metal micro- or nanoparticles: a carbon source and a metal salt are mixed, with the mass ratio of metal salt to carbon source being 2:1, and the two are mixed evenly by grinding or ball milling, and then heat-treated in a high-temperature furnace at 200°C for 150 minutes to obtain a metal particle@carbon material, which is a carbon-based material with carbon-coated metal micro- or nanoparticles grown on it;
[0083] The carbon source is selected from polymers;
[0084] The metal salt is selected from basic nickel carbonate.
[0085] In step (1), the content of metal particles in the metal particles@carbon material is adjusted by adjusting the ratio of the carbon source to the metal salt;
[0086] By increasing the mass proportion of metal salt in the raw materials, the metal proportion in the final product is increased, and the conductivity of the final product is increased.
[0087] The heat treatment in step (1) is carried out in different temperature sections in a step-by-step manner. In the first temperature section, heat pretreatment is carried out to first react the metal salt with the carbon source; after the temperature is raised, heat treatment is carried out in the second temperature section to achieve the graphitization transformation process of the carbon.
[0088] The heat treatment in step 1 improves the conductivity of the intermediate product metal particles@carbon by increasing the heat treatment temperature in the second temperature section.
[0089] (2) Preparation of graphene-coated metal particles: The metal particles@carbon material are placed in a quartz tube, both ends of which are blocked with copper wire or carbon cloth and then placed in a reaction chamber for treatment. The two ends of the reactant are connected to the positive and negative electrodes of the power supply, the reaction chamber is evacuated, and the sample is discharged at a voltage of 150 V for 400 ms to obtain graphene-coated metal particle material.
[0090] Example 5
[0091] This embodiment provides a method for preparing graphene-coated metal particles, comprising the following steps:
[0092] (1) Preparation of carbon-coated metal micro- or nanoparticles: a carbon source and a metal salt are mixed, with the mass ratio of metal salt to carbon source being 1:3, and the two are mixed evenly by grinding or ball milling, and then heat-treated in a high-temperature furnace at 750°C for 90 minutes to obtain a metal particle@carbon material, which is a carbon-based material with carbon-coated metal micro- or nanoparticles grown on it;
[0093] The carbon source is selected from glucose;
[0094] The metal salt is selected from basic copper carbonate monohydrate.
[0095] In step (1), the content of metal particles in the metal particles@carbon material is adjusted by adjusting the ratio of the carbon source to the metal salt;
[0096] By increasing the mass proportion of metal salt in the raw materials, the metal proportion in the final product is increased, and the conductivity of the final product is increased.
[0097] The heat treatment in step (1) is carried out in different temperature sections in a step-by-step manner. In the first temperature section, heat pretreatment is carried out to first react the metal salt with the carbon source; after the temperature is raised, heat treatment is carried out in the second temperature section to achieve the graphitization transformation process of the carbon.
[0098] The first temperature section is subjected to heat pretreatment, wherein the heat pretreatment is specifically as follows: heating from room temperature to 335°C at a heating rate of 5°C / min, using 200 sccm argon as a protective gas, and heat treating for 60 minutes;
[0099] Then, heat treatment was performed in the second temperature section, with the temperature rising from 335°C to 750°C at a heating rate of 5°C / min, 200 sccm argon as the protective gas, and the treatment lasted for 60 min;
[0100] The heat treatment in step (1) improves the conductivity of the intermediate product metal particles@carbon by increasing the heat treatment temperature in the second temperature section.
[0101] (2) Preparation of graphene-coated metal particles: The metal particles@carbon material are placed in a quartz tube, and the two ends are blocked with copper wire or carbon cloth and then placed in a reaction chamber for treatment. The two ends of the reactant are connected to the positive and negative electrodes of the power supply, and the reaction chamber is evacuated. The discharge times are 2 times. The first time is a low voltage pretreatment with a voltage less than or equal to 110V to reduce the resistance of the reactant to a few ohms; the second time is a formal Joule heat treatment with a voltage greater than 110V to obtain the graphene-coated metal particle material.
[0102] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical ideas disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A method for preparing graphene-coated metal particles, characterized in that: The following steps are involved: (1) Preparation of carbon-coated metal micro- or nanoparticles: a carbon source and a metal salt are mixed, the mass ratio of the metal salt to the carbon source being 1:(0.5-3), the two are mixed evenly by grinding or ball milling, and then heat-treated in a high-temperature furnace at 200-900°C for 30-240 minutes to obtain a metal particle@carbon material, which is a carbon-based material with carbon-coated metal micro- or nanoparticles grown on it; (2) Preparation of graphene-coated metal particles: metal particles@carbon material are placed in a quartz tube, both ends of which are blocked with copper wire or carbon cloth and then placed in a reaction chamber for treatment. The two ends of the reactant are connected to the positive and negative electrodes of the power supply, the reaction chamber is evacuated, and the sample is discharged at a voltage of 30-220V for 50-1000ms to obtain a graphene-coated metal particle material; The carbon source is selected from one of glucose, sucrose and polymer; The metal salt is selected from basic copper carbonate, copper acetate and basic nickel carbonate.
2. The method for preparing graphene-coated metal particles according to claim 1, characterized in that: In step (1), the mass ratio of the metal salt to the carbon source is 1:1 or 1:2 or 2:
1.
3. The method for preparing graphene-coated metal particles according to claim 1, characterized in that: In step (1), the content of metal particles in the metal particles@carbon material is adjusted by adjusting the ratio of the carbon source to the metal salt; By increasing the mass proportion of metal salt in the raw materials, the metal proportion in the final product is increased, and the conductivity of the final product is increased.
4. The method for preparing graphene-coated metal particles according to claim 1, characterized in that: When the heat treatment temperature in step (1) is 750°C, the number of discharges in step (2) is 2 times. The first time is a low voltage pretreatment with a voltage less than or equal to 110V to reduce the resistance of the reactants to a few ohms; the second time is a formal Joule heat treatment with a voltage greater than 110V.
5. The method for preparing graphene-coated metal particles according to claim 1, characterized in that: In step (2), the sample is discharged at a voltage of 150 V for 400 ms.
6. The method for preparing graphene-coated metal particles according to claim 1, characterized in that: The heat treatment in step (1) is carried out in different temperature sections in a step-by-step manner. A heat pretreatment is carried out in the first temperature section to first react the metal salt with the carbon source. After the temperature is raised, a heat treatment is carried out in the second temperature section to achieve a graphitization transformation process of the carbon. And / or the heat treatment in step 1, by increasing the heat treatment temperature in the second temperature section, to improve the conductivity of the intermediate product metal particles @ carbon.
7. The method for preparing graphene-coated metal particles according to claim 1, characterized in that: Step (1) is specifically as follows: Weigh 6.66 g of glucose and 3.33 g of monohydrated copper carbonate, grind for 15 min to mix the two evenly, and perform heat pretreatment before heat treatment. The heat pretreatment is as follows: heat from room temperature to 335°C at a heating rate of 5°C / min, with 200 sccm argon as protective gas, and heat treatment for 60 min; Then, heat treatment was performed: the temperature was raised from 335°C to 750°C at a heating rate of 5°C / min, 200 sccm argon was used as the protective gas, and the treatment lasted for 60 minutes.
8. The method for preparing graphene-coated metal particles according to claim 1, characterized in that: Step (2) is specifically as follows: Weigh 180 mg of the metal particles@carbon material prepared in step (1) and place them in a quartz tube with a length of 50 mm, an inner diameter of 4 mm, and an outer diameter of 6 mm. After blocking both ends with fine copper wires, place them in a reaction chamber, connect the positive and negative electrodes at both ends, evacuate the reaction chamber, and discharge the sample at a voltage of 150 V for 400 ms. When the voltage drops to 0 V, graphene-coated metal particles are obtained.
9. Graphene-coated metal particles obtained by the preparation method according to any one of claims 1 to 8.
Citation Information
Patent Citations
Processing method of ultrahigh-thermal-conductivity and high-toughness device
CN112521146A
Processes for manufacture of coated metallic particles and composite material, and installation for carrying out these processes
EP1462539A1