A colorless and transparent soldering flux with post-welding residue and preparation method thereof
By using a combination of high softening point rosin and low softening point rosin, compound halogen, antioxidant and whitening agent in the lead-free LED solder paste, the problem of color and corrosiveness of the post-soldering residue is solved and achieved Colorless, transparent and non-corrosive soldering effect, suitable for lead-free LED soldering.
Patent Information
- Application Number
- CN202310058961.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-14
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-01-14
AI Technical Summary
The post-soldering residues of existing lead-free LED solder pastes are mostly yellow or light yellow, which affects the color temperature of the LED lamp, and most colorless and transparent lead-free solder pastes are highly corrosive to fiberglass boards and aluminum substrates, causing short circuits and use Lifespan is reduced.
A combination system of high softening point and low softening point rosin compound, compound halogen, antioxidant, whitening agent and thixotropic agent is used, and the active agent is selected through high temperature tests to prepare a non-corrosive fiberglass board and aluminum substrate. Color-transparent flux ensures weldability and residue color. The post-soldering residue is colorless and transparent.
It achieves colorless and transparent post-soldering residue, maintains weldability and correction, avoids corrosion of the LED board, meets the corrosiveness and surface insulation resistance requirements of IPC standards, and is suitable for lead-free LED welding.
Smart Images

Figure BDA0004060940430000011 
Figure BDA0004060940430000031 
Figure BDA0004060940430000041
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of soldering flux and preparation method thereof, and particularly relates to a colorless and transparent soldering flux with post-welding residue and a preparation method thereof. Background Art
[0002] As a new type of green lighting fixture, LED lamps are widely used and promoted. At present, the production of LED products is mostly based on surface mount technology (SMT), with tin-lead (Sn-Pb) alloy as the main solder paste. With the concern of human beings for environmental protection, the widely used LED product mounting is also increasingly tending to be lead-free. Compared with Sn-Pb alloy reflow soldering, lead-free reflow soldering has the disadvantages of high solder melting point, poor wettability, and yellow residue color. At present, the lead-free solder paste with better weldability has a higher welding temperature than lead solder paste, and the residue after soldering is mostly yellow or light yellow, which has a certain impact on the color temperature of LED lamps. In order to ensure the quality of LED lamps, the requirements for LED lamp solder paste are not only limited to welding performance, but also have higher requirements for the color of the residue.
[0003] At present, there are relatively few colorless, transparent, lead-free solder pastes for LEDs on the market. Most of the colorless, transparent, lead-free solder pastes use an activator system of organic acid plus organic amine, which makes the flux highly corrosive to glass fiber boards and aluminum substrates. On the premise of ensuring weldability and residue, a large area of tin drilling (tin liquid spreads on the metal substrate through the coating) is formed, which causes defects such as short circuit and reduced service life of the LED board after welding and makes it unusable. The activator system using organic acid plus halogen will also have a certain degree of influence on the color of the residue. Therefore, the present invention conducts high temperature tests on materials such as halogen, organic acid, antioxidant and brightener in the flux formula, and optimizes the activator system that can take into account both weldability and residue color. Summary of the invention
[0004] The present invention aims to solve the shortcomings of the existing lead-free LED solder paste technology and provide a lead-free LED soldering flux with colorless and transparent residue, no corrosion to glass fiber boards and aluminum substrates, good weldability, deviation correction, and no tin beads. The present invention also provides a preparation method of the soldering flux.
[0005] The technical solution adopted by the present invention is as follows:
[0006] A colorless and transparent soldering flux with post-welding residue, the raw materials of which are as follows by weight percentage:
[0007]
[0008] The compound rosin of the present invention is a compound of two or more of high softening point rosin and low softening point rosin, wherein the high softening point rosin is one or more of KE-604 rosin, 125 rosin, ice white rosin, 150 rosin, and RHR-604; the low softening point rosin is one or more of KE-100 rosin, KE-311 rosin, and 100D rosin;
[0009] The composite organic acid of the present invention is two or more of succinic acid, glutaric acid, 10-hydroxy-2-decenoic acid, 2,2-dihydroxymethylpropionic acid, pyruvic acid, itaconic acid, p-methylcinnamic acid, and suberic acid;
[0010] The composite halogen of the present invention is two or more of o-iodobenzoic acid, 1-bromo-N-phenylcarbazole, α,α-dibromo-p-xylene, N-n-butylaniline HBr, 2,3-dichloropyrazine, and N,N-dimethyl-p-phenylenediamine dihydrochloride;
[0011] The thixotropic agent of the present invention is one or more of polyamide modified hydrogenated castor oil, dust-proof thixotropic agent SH, thixotropic agent MONORAL8800, polyamide wax thixotropic agent J-530, Arkema thixotropic agent Crayvallac Ultra, and thixotropic agent CRAYVALLAC SF;
[0012] The composite antioxidant of the present invention is prepared by mixing 2,4-di(dodecylthiomethyl)-6-methylphenol and 1,2,3-benzotriazole in a mass ratio of 3:1;
[0013] The compound brightener of the present invention is prepared by mixing brightener 3030 and fluorescent brightener CBS-X in a mass ratio of 1:1;
[0014] The compound solvent of the present invention is compounded from alcohol solvents and alcohol ether solvents in high boiling point solvents; the alcohol solvent is one or more of ethylene glycol, glycerol, 2-ethyl-1,3-hexanediol, n-octanol, and isooctadecanol; the alcohol ether solvent is one or more of propylene glycol phenyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dibutyl ether, and diethylene glycol hexyl ether.
[0015] The preparation method of the colorless and transparent soldering flux with post-welding residue of the present invention is as follows:
[0016] (1) Adding compound rosin, compound thixotropic agent and part of solvent into a reactor, heating at a heating rate of 150-170° C., and stirring until completely melted;
[0017] (2) heating the compounded antioxidant, brightener and remaining solvent to 150° C., stirring and melting them completely to obtain a compounded solution;
[0018] (3) cooling the completely melted liquid of step (1) to 150° C., adding the composite solution of step (2), and stirring the composite organic acid until it is completely melted;
[0019] (4) Cool the liquid to 130-140° C., add the compound halogen, stir and melt completely, and obtain a colorless transparent liquid, which is the colorless transparent flux residue after welding. Heat the liquid to 125-135° C. and place it in a refrigerator at 2-10° C. for later use.
[0020] The colorless and transparent soldering flux with post-weld residue of the present invention has the following advantages:
[0021] (1) The rosin used in the present invention is hydrogenated rosin compounded with high softening point rosin and low softening point rosin, which can ensure the excellent film-forming property of the flux and is not easy to turn yellow under high temperature welding.
[0022] (2) The compound halogen used in the present invention has good activity and can remain yellow for 5 minutes at 250°C, ensuring that the residue after welding is colorless and transparent, and providing sufficient activity during welding to ensure the wettability of the solder joint.
[0023] (3) The present invention uses a whitening agent compounded with N-methyl-4-methoxy-1,8-naphthalene diimide and a fluorescent whitening agent CBS-X, which can increase the transparency of the flux during the preparation process of the flux and inhibit the yellowing of the flux residue under high-temperature welding conditions.
[0024] (4) The present invention adopts an antioxidant compounded with 2,4-di(dodecylthiomethyl)-6-methylphenol and 1,2,3-benzotriazole, which can prevent the residue from oxidizing and turning yellow and black during the welding process, and protect the solder joints from secondary oxidation during a long reflow time. Benzotriazole can be adsorbed on the metal surface to form a very thin film to protect metals such as tin and copper from corrosion by acidic vapor and residual activity.
[0025] (5) The thixotropic agent used in the present invention is a high-temperature thixotropic agent, which is not easily oxidized and yellowed at high temperatures and has good thixotropic properties, ensuring that the solder paste is fine and shiny, has good deviation correction and collapse properties, and does not produce tin beads after soldering.
[0026] (6) The compound solvent and compound organic acid raw materials used in the present invention are high-temperature raw materials, which are not easily oxidized and discolored at high temperatures. The oxides generated during the welding process can also be cleaned up in time by the active substances to prevent the formation of oxide slag, thereby ensuring wettability and the color of the residue.
[0027] (7) The flux component of the present invention does not corrode the glass fiber board and the aluminum substrate under the condition of providing sufficient welding activity, and is not easy to oxidize and turn yellow at high temperature (lead-free soldering temperature 250°C), thereby ensuring excellent weldability and colorless and transparent residues. DETAILED DESCRIPTION
[0028] The present invention is further described in detail below by way of examples, but the protection scope of the present invention is not limited to the contents described in the examples.
[0029] Example 1
[0030] The colorless and transparent flux residue after welding is composed of the following raw materials by weight percentage:
[0031] KE-604 20% KE-311 15% Thixotropic agent MONORAL 8800 2% Anti-settling thixotropic agent SH 4% 2,2-Dimethylolpropionic acid 5% Glutaric acid 4% p-Methylcinnamic acid 5% N,N-Dimethyl-p-phenylenediamine dihydrochloride 0.3% α,α-Dibromo-p-xylene 0.2% 1,2,3-Benzotriazole 0.25% 2,4-Di(dodecylthiomethyl)-6-methylphenol 0.75% Brightener 3030 3.5% Fluorescent brightener CBS-X 3.5% 2-Ethyl-1,3-hexanediol 11.5% Tetraethylene glycol dimethyl ether 25%
[0032] The preparation method of colorless and transparent flux with post-soldering residue is as follows:
[0033] (1) KE-604 rosin, KE-311 rosin, MONORAL 8800 thixotropic agent, anti-settling thixotropic agent SH, and tetraethylene glycol dimethyl ether were added to a reactor at the same time, heated to 160° C. at a heating rate of 8-9° C. / min, stirred and melted completely, and cooled to 150° C. to obtain solution A;
[0034] (2) 1,2,3-benzotriazole, 2,4-di(dodecylthiomethyl)-6-methylphenol, brightener 3030, fluorescent brightener CBS-X, and 2-ethyl-1,3-hexanediol were heated to 150° C. for 15 minutes and stirred thoroughly to obtain a composite solution;
[0035] (3) The compound solution, 2,2-dihydroxymethylpropionic acid, glutaric acid, and p-methylcinnamic acid are sequentially added to solution A and stirred until completely melted. The mixture is cooled to 135° C., N,N-dimethyl-p-phenylenediamine dihydrochloride and α,α-dibromo-p-xylene are added and stirred until completely melted. When the temperature reaches 130° C., the mixture is removed from the pan and placed in a refrigerator at 2-8° C. for 4 hours to obtain a colorless and transparent flux residue after welding.
[0036] Example 2
[0037] A colorless and transparent lead-free LED soldering flux with residue, the raw materials of which are as follows by weight percentage:
[0038] RHR-604 20% KE-100 15% 100D 5% Polyamide modified hydrogenated castor oil 3% Anti-settling thixotropic agent SH 3% 2,2-Dimethylolpropionic acid 6% p-Methylcinnamic acid 6% 2-Iodobenzoic acid 0.2% α,α-Dibromo-p-xylene 0.2% 1,2,3-Benzotriazole 0.3% 2,4-Di(dodecylthiomethyl)-6-methylphenol 0.9% Brightener 3030 3% Fluorescent brightener CBS-X 3% n-Octanol 14.4% Tetraethylene glycol dimethyl ether 20%
[0039] The preparation method of colorless and transparent flux with post-soldering residue is as follows:
[0040] (1) RHR-604 rosin, KE-100 rosin, 100D rosin, polyamide-modified hydrogenated castor oil, anti-settling thixotropic agent SH, tetraethylene glycol dimethyl ether, and 4% n-octanol were added to a reactor at the same time, heated to 163° C. at a heating rate of 8-9° C. / min, stirred and melted completely, and cooled to 150° C. to obtain solution B;
[0041] (2) 1,2,3-benzotriazole, 2,4-di(dodecylthiomethyl)-6-methylphenol, brightener 3030, fluorescent brightener CBS-X, and the remaining n-octanol were heated to 150° C. for 15 minutes and stirred thoroughly to obtain a composite solution;
[0042] (3) Add the compound solution, 2,2-dihydroxymethylpropionic acid, and p-methylcinnamic acid to solution B in sequence and stir until completely melted. Cool to 135°C, add o-iodobenzoic acid and α,α-dibromo-p-xylene and stir until completely melted. When the temperature reaches 125°C, remove from the pan and place in a refrigerator at 2-10°C for at least 4 hours to obtain a colorless and transparent flux residue after welding.
[0043] Example 3
[0044] The colorless and transparent flux residue after welding is composed of the following raw materials by weight percentage:
[0045]
[0046]
[0047] The preparation method of colorless and transparent flux with post-weld residue is as follows:
[0048] (1) RHR-604 rosin, KE-100 rosin, Arkema thixotropic agent Crayvallac Ultra, anti-settling thixotropic agent SH, tetraethylene glycol dimethyl ether, and 7% 2-ethyl-1,3-hexanediol were added to a reactor at the same time, heated to 165° C. at a heating rate of 8-9° C. / min, stirred and melted completely, and cooled to 150° C. to obtain solution C;
[0049] (2) 1,2,3-benzotriazole, 2,4-di(dodecylthiomethyl)-6-methylphenol, brightener 3030, fluorescent brightener CBS-X, and the remaining 2-ethyl-1,3-hexanediol were heated to 150° C. for 18 minutes and stirred thoroughly to obtain a composite solution;
[0050] (3) The compound solution, 2,2-dihydroxymethylpropionic acid and itaconic acid are added to solution C in sequence and stirred until completely melted. The solution is cooled to 130°C, and o-iodobenzoic acid and N-n-butylaniline HBr are added and stirred until completely melted. When the temperature reaches 125°C, the solution is removed from the pot and placed in a refrigerator at 2-8°C for 4 hours to obtain a colorless and transparent flux residue after welding.
[0051] Example 4
[0052] A colorless and transparent soldering flux with post-welding residue, the raw material composition is as follows by weight percentage:
[0053] Ice White Rosin 23% 100D 15% Thixotropic agent MONORAL 8800 4% Thixotropic agent CRAY VALLAC SF 4% 10-Hydroxy-2-decenoic acid 8% p-Methylcinnamic acid 7% 2-Iodobenzoic acid 0.2% N,N-Dimethyl-p-phenylenediamine dihydrochloride 0.1% 1,2,3-Benzotriazole 0.5% 2,4-Di(dodecylthiomethyl)-6-methylphenol 1.5% Brightener 3030 2.5% Fluorescent brightener CBS-X 2.5% Isostearyl alcohol 15.7% Propylene glycol phenyl ether 16%
[0054] The preparation method of colorless and transparent flux with post-soldering residue is as follows:
[0055] (1) Add ice white rosin, 100D rosin, MONORAL 8800 thixotropic agent, CRAY VALLAC SF thixotropic agent, propylene glycol phenyl ether, and 5% isostearyl alcohol to a reactor at the same time, heat to 170° C. at a heating rate of 8-9° C. / min, stir and melt completely, and cool to 150° C. to obtain solution D;
[0056] (2) 1,2,3-benzotriazole, 2,4-di(dodecylthiomethyl)-6-methylphenol, brightener 3030, fluorescent brightener CBS-X, and the remaining isostearyl alcohol were heated to 150° C. for 18 minutes and stirred thoroughly to obtain a composite solution;
[0057] (3) The compound solution, 10-hydroxy-2-decenoic acid, and p-methylcinnamic acid are sequentially added to solution D and stirred until completely melted. The mixture is cooled to 140°C, and o-iodobenzoic acid and N,N-dimethyl-p-phenylenediamine dihydrochloride are added and stirred until completely melted. When the temperature reaches 135°C, the mixture is removed from the pan and placed in a refrigerator at 8°C for 4 hours to obtain a colorless and transparent flux residue after welding.
[0058] The colorless transparent flux residues after soldering prepared in the above Examples 1, 2, 3, and 4 were taken out and heated to room temperature for 4 hours, and then mixed with SnAgCu solder powders at a mass ratio of 11.6:88.4 to prepare solder pastes. The performance test results are shown in Table 1:
[0059] Table 1 List of colorless and transparent flux performance tests after soldering residue
[0060]
[0061] As can be seen from Table 1, the colorless and transparent soldering flux with post-weld residue of the present invention is made colorless and transparent by optimizing rosin, thixotropic agent, compound halogen activator, solvent system, and using antioxidant and brightener. The optimization of the activator system enables the soldering flux to reduce the corrosion to the LED board while ensuring good solderability, tin bead and deviation correction performance, meet the requirement of non-drilling tin for glass fiber board and aluminum substrate in LED board, meet the requirements of IPC standard for corrosion and surface insulation resistance, and be suitable for lead-free LED welding.
[0062] The above embodiments are only partial embodiments of the present invention, but not all embodiments. In addition to the halogens listed in the embodiments, the composite halogen of the present invention can also use 1-bromo-N-phenylcarbazole, 2,3-dichloropyrazine, etc. Similarly, the thixotropic agent can also be polyamide wax thixotropic agent J-530, etc. The composite solvent is a composite of an alcohol solvent and an alcohol ether solvent in a high boiling point solvent; the alcohol solvent can also be ethylene glycol, glycerol, etc., and the alcohol ether solvent can also be diethylene glycol dibutyl ether, diethylene glycol hexyl ether, etc. For those skilled in the art, technical solutions replaced by equivalent technical means should all fall within the scope of protection of the present invention.
Claims
1. A colorless and transparent soldering flux with post-weld residue, characterized in that: By weight percentage, the raw material composition is: Compound rosin 35-40%; Compound organic acid 8-15%; Compound halogen 0.3~0.6%; Thixotropic agent 6-8%; Compound antioxidant 1-2%; Compound whitening agent 5~8%; Residue of compounding solvent; The compound antioxidant is prepared by mixing 2,4-di(dodecylthiomethyl)-6-methylphenol and 1,2,3-benzotriazole in a mass ratio of 3:1; The compound brightener is prepared by mixing brightener 3030 and fluorescent brightener CBS-X in a mass ratio of 1:1; The composite halogen is two or more of o-iodobenzoic acid, 1-bromo-N-phenylcarbazole, α,α-dibromo-p-xylene, N-n-butylaniline HBr, 2,3-dichloropyrazine, and N,N-dimethyl-p-phenylenediamine dihydrochloride; The composite organic acid is two or more of succinic acid, glutaric acid, 10-hydroxy-2-decenoic acid, 2,2-dihydroxymethylpropionic acid, pyruvic acid, itaconic acid, p-methylcinnamic acid, and suberic acid; The compound solvent is a compound of an alcohol solvent and an alcohol ether solvent in a high boiling point solvent; the alcohol solvent is one or more of ethylene glycol, glycerol, 2-ethyl-1,3-hexanediol, n-octanol, and isooctadecanol; the alcohol ether solvent is one or more of propylene glycol phenyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dibutyl ether, and diethylene glycol hexyl ether; The compound rosin is a compound of two or more of a high softening point rosin and a low softening point rosin, wherein the high softening point rosin is one or more of KE-604 rosin, 125 rosin, ice white rosin, 150 rosin, and RHR-604; and the low softening point rosin is one or more of KE-100 rosin and KE-311 rosin.
2. A colorless and transparent soldering flux with post-weld residue according to claim 1, characterized in that: The thixotropic agent is one or more of polyamide modified hydrogenated castor oil, anti-settling thixotropic agent SH, thixotropic agent MONORAL 8800, polyamide wax thixotropic agent J-530, Arkema thixotropic agent Crayvallac Ultra, and thixotropic agent CRAY VALLAC SF.
3. The method for preparing the colorless and transparent soldering flux with post-weld residue according to claim 1 or 2, characterized in that: Here’s how: (1) Add high softening point rosin, low softening point rosin, thixotropic agent and part of solvent into the reactor, heat to 150~170℃, and stir until completely melted; (2) heating the compounded antioxidant, brightener and remaining solvent to 150°C, stirring and melting them completely to obtain a compounded solution; (3) Cooling the completely melted liquid in step (1) to 150° C., adding the composite solution described in step (2), and mixing with organic acid, and stirring until completely melted; (4) The liquid obtained in step (3) is cooled to 130-140°C, and the compound halogen is added, and the mixture is stirred and melted completely to obtain a colorless transparent liquid. The mixture is taken out of the pot at 125-135°C and refrigerated in a refrigerator at 2-10°C to obtain the colorless transparent flux as the post-welding residue.
Citation Information
Patent Citations
Lead-free solder thread-use colophony type non-halide cleaning-free scaling powder
CN101157168A
Soldering flux of tin soldering paste and preparation method thereof
CN108526758A
Low residual halogen-free solder paste
CN109262161A
Solder wire soldering flux capable of reducing splashing and preparation method thereof
CN111906472A
High-lead soldering paste soldering flux and preparation method thereof
CN114273820A