A cross-linked porous structure high temperature proton exchange membrane and preparation method thereof
By using polyvalent organic phosphonic acid with both proton conductive function and cross-linking effect in the high-temperature proton exchange membrane, a dense double skin layer is formed, which solves the problems of hydrogen cross-penetration and phosphoric acid loss, and achieves high proton conductivity and low hydrogen penetration. The cross-linked porous structure improves the stability and performance of the fuel cell.
Patent Information
- Application Number
- CN202211396714.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-09
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2042-11-09
AI Technical Summary
High-temperature proton exchange membrane fuel cells have problems with hydrogen cross-penetration and phosphoric acid loss under high-temperature conditions. Existing cross-linking agents often sacrifice proton conductivity when improving stability.
Polyvalent organic phosphonic acid with both proton conductive function and cross-linking effect is used to soak the porous polymer membrane to form a dense double skin layer, which enhances the membrane's phosphoric acid retention capacity and reduces hydrogen gas penetration.
A cross-linked porous structure high-temperature proton exchange membrane with high proton conductivity and low hydrogen permeability under high temperature conditions has been achieved, which improves the stability and performance of the fuel cell.
Smart Images

Figure CN115832376B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of fuel cells, and in particular relates to a cross-linked porous high-temperature proton exchange membrane with high proton conductivity and high phosphoric acid retention capacity for fuel cells and a preparation method thereof. Background Art
[0002] Proton exchange membrane fuel cells are currently widely used in portable and fixed power sources due to their high specific power, use of clean energy hydrogen, and flexibility. Research has sprung up in recent years. Compared with traditional low-temperature proton exchange membrane fuel cells, high-temperature proton exchange membrane fuel cells have the advantages of fast electrode reaction kinetics, high CO tolerance, simple water thermal management system, and a wide range of fuel sources (methanol reforming gas, formic acid, industrial by-product hydrogen) under high temperature conditions. Therefore, it has become one of the fastest-growing research directions in the field of fuel cells today.
[0003] Among the many polymers suitable for high-temperature proton exchange membranes, phosphoric acid-doped polybenzimidazole systems have outstanding potential due to their excellent thermal stability and chemical resistance, making them promising candidates for the new generation of high-temperature proton exchange membranes. It is well known that high phosphoric acid doping levels can achieve high proton conductivity of proton exchange membranes. A method generally recognized to increase the phosphoric acid doping level of membranes is to prepare membranes with porous structures. The rich pore structure can store a large amount of phosphoric acid. However, the cross-permeation problem of fuel gas and the loss of phosphoric acid faced during the long-term operation of the battery cannot be ignored due to the rich porosity. The direct exposure of the porous structure to the battery environment is still a challenge to obtain excellent fuel cell stability. A promising solution is to construct a porous membrane structure with a dense skin layer, that is, to use the porous structure to store phosphoric acid and to use the dense skin layer to block the rapid loss of phosphoric acid and hydrogen penetration.
[0004] In view of the above strategy, cross-linking agents are currently commonly used to cross-link polymer membranes to form a dense epidermis, but the cross-linking agents themselves often do not have mass transfer functions. Although the introduction of the cross-linking agent into the membrane improves the stability of the membrane, it sacrifices some proton conduction performance. A multi-organic phosphonic acid with both cross-linking and proton conduction functions is used, and it is introduced into a porous polymer membrane to prepare a cross-linked porous polymer membrane with a dense double epidermis. Compared with porous membranes with fast phosphoric acid loss rate and severe hydrogen permeation, the cross-linked porous polymer membrane has a dense epidermis formed by the cross-linking effect of the organic phosphonic acid, which makes phosphoric acid better retained in the porous membrane and significantly reduces hydrogen permeation. In addition, as an organic proton conductor, the multi-organic phosphonic acid has a strong hydrogen bonding effect with phosphoric acid, which enhances the synergistic mass transfer ability and further increases the retention capacity of phosphoric acid in the membrane. Summary of the invention
[0005] In view of the above problems, the present invention aims to introduce the use of a cross-linking agent, an organic phosphonic acid, which has both proton conduction function and cross-linking effect, to form a cross-linked porous high-temperature proton exchange membrane with a dense double skin layer. The porous high-temperature proton exchange membrane prepared by this method alleviates hydrogen cross-permeation and phosphoric acid loss in water / anhydrous environments, and does not sacrifice the proton conduction performance of the membrane due to cross-linking, thereby enhancing the stability of the porous proton exchange membrane.
[0006] The technical solution of the present invention is as follows:
[0007] A method for preparing a cross-linked porous high-temperature proton exchange membrane comprises the following steps:
[0008] (1) Preparation of porous membrane substrate
[0009] Dissolving a high molecular polymer containing a nitrogen heterocycle in a main chain in an organic solvent of the polymer to obtain a first polymer solution; using the first polymer solution to form a film by casting with a porogen, or casting to form a liquid film and preparing a porous base film by a water vapor induced phase inversion method;
[0010] (2) Formation of a cross-linked dense double skin layer
[0011] The porous polymer membrane obtained in step (1) is immersed in a polybasic organic phosphonic acid aqueous solution of a certain concentration at a certain temperature, wherein the polybasic organic phosphonic acid has a proton conduction function; the polybasic organic phosphonic acid and the polymer membrane are cross-linked to form a dense double skin layer with a cross-linked structure on the surface of the porous membrane;
[0012] (3) Acid doping post-treatment
[0013] The cross-linked porous structure membrane obtained in step (2) is saturated with acid and then the residual acid is removed to obtain the cross-linked porous structure high-temperature proton exchange membrane.
[0014] Furthermore, in step (1), the polymer whose main chain contains nitrogen heterocycles is polybenzimidazole (OPBI, ABPBI, mPBI, etc.), polyaromatic piperidine (polyterphenyl piperidine, polybiphenyl piperidine, etc.) or polyaromatic pyridine (polyterphenyl pyridine, polybiphenyl pyridine, etc.); and the organic solvent is N,N-dimethylformamide, N,N-dimethylacetamide, etc.
[0015] Furthermore, the step (1) of using a porogen to cast a film is specifically as follows: under stirring conditions, a certain amount of a porogen is added to a first polymer solution to obtain a second polymer solution; the second polymer solution is cast on a clean substrate to form a film, and the solvent is heated to volatilize the solvent to obtain a composite film; and the composite film is immersed in a solvent to dissolve the porogen in the film, thereby obtaining a porous base film. Furthermore, the composite film is immersed in a solvent to dissolve the porogen in the film, and for inorganic additives, the solvent is a strong acid (hydrofluoric acid, hydrochloric acid) or a strong base (such as NaOH or KOH) aqueous solution; for organic additives, the solvent is a combination of one or more of deionized water, anhydrous ethanol, methanol, isopropanol, acetone, etc. The preferred additive addition amount is 30 to 60% by weight.
[0016] Furthermore, the step (1) of casting to form a liquid film and preparing a porous base film by a water vapor induced phase inversion method is specifically as follows: casting the first polymer solution on a clean substrate to form a liquid film, and placing the liquid film in a water vapor environment with a certain temperature and humidity, and preparing the porous base film by a water vapor induced phase inversion method. Furthermore, the water vapor temperature and humidity ranges are 20 to 80° C. and 20 to 100% RH, respectively.
[0017] Furthermore, the step (3) is specifically as follows: the cross-linked porous structure membrane obtained in step (2) is immersed in an 85wt% concentrated phosphoric acid solution until the membrane reaches acid absorption saturation, and the residual attached acid on the surface is removed after removal to obtain the cross-linked porous structure high-temperature proton exchange membrane. Furthermore, the cross-linked porous structure high-temperature proton exchange membrane is immersed in an 85wt% phosphoric acid aqueous solution for 48-96 hours at a temperature of 60-100°C.
[0018] Furthermore, the porogen in step (1) is an inorganic nanopowder (the inorganic nanopowder may be SiO 2 、Al 2 O 3 , ZnO and other inorganic nanopowders that are easily dissolved by acid and alkali), or a combination of one or more of organic liquid dibutyl phthalate, low molecular weight polyethylene glycol or polyacrylic acid.
[0019] Furthermore, the polybasic organic phosphonic acid in step (2) is a combination of one or more of hydroxyethylidene diphosphonic acid (HEDP), aminotrimethylene phosphonic acid (ATMP), ethylenediaminetetramethylenephosphonic acid (EDTMPA), diethylenetriaminepentamethylenephosphonic acid (DTPMPA), hexamethylenediaminetetramethylenephosphonic acid (HDTMPA), and dihexylenetriaminepentamethylenephosphonic acid (BHMTPMPA); the concentration of the polybasic organic phosphonic acid is 5 to 50 wt%, and the preferred concentration of the polybasic organic phosphonic acid is 10 to 30 wt%.
[0020] A cross-linked porous high-temperature proton exchange membrane obtained by the method comprises an intermediate porous layer and a cross-linked dense double surface layer; the intermediate porous layer stores free phosphate to obtain high proton conductivity, and the cross-linked dense double surface layer has a proton conduction function.
[0021] Furthermore, the conductivity of the exchange membrane at 160°C is 0.112S cm -1 The hydrogen permeation current density of the hydrogen-oxygen single cell assembled using the exchange membrane at 160°C is 0.99 mA cm -2 , the output power is 0.98W cm -2 .
[0022] Furthermore, the high temperature proton exchange membrane is used as an electrolyte diaphragm material for a high temperature proton exchange membrane fuel cell or a diaphragm material for a flow battery, a water electrolyzer, or an electrochemical device.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] (1) The cross-linked porous high-temperature proton exchange membrane prepared by the present invention has a dense double skin layer and a porous internal structure. The internal porous structure can store a large amount of free phosphoric acid to obtain high proton conductivity. The dense double skin layer can greatly reduce phosphoric acid loss and hydrogen permeation, and at the same time has high mechanical strength.
[0025] (2) The present invention uses an organic phosphonic acid, a cross-linking agent having both proton conduction function and cross-linking effect, to ensure cross-linking without sacrificing the proton conduction performance of the membrane.
[0026] (3) The preparation method of the present invention is simple, and the thickness of the dense skin layer can be regulated by cross-linking time, concentration of organic phosphonic acid solution, immersion temperature, etc., so as to achieve the optimal performance of the cross-linked porous structure high-temperature proton exchange membrane. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the technical solution of the present invention, the drawings required for use in the embodiments are briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0028] Figure 1 Schematic diagram of the porous proton exchange membrane and the cross-linked porous proton exchange membrane with a dense double skin layer according to the present invention.
[0029] Figure 2 Schematic diagram of the cross-linked structure of the dense double skin layer of the porous proton exchange membrane of the present invention.
[0030] Figure 3Proton conductivity curves of the high-temperature proton exchange membranes prepared in Example 1 of the present invention and Comparative Example 1 at different temperatures.
[0031] Figure 4 Internal resistance stability of the high temperature proton exchange membranes prepared in Example 1 of the present invention and Comparative Example 1 at 80° C. and 40% humidity.
[0032] Figure 5 Single cell performance of the high temperature proton exchange membranes prepared in Example 1 of the present invention and Comparative Example 1 at 160°C.
[0033] Figure 6 The high temperature proton exchange membrane prepared in Example 1 of the present invention and Comparative Example 1 was 160°C and 0.4A cm -2 Battery discharge stability under . DETAILED DESCRIPTION
[0034] The present invention provides a method for preparing a cross-linked porous high-temperature proton exchange membrane for a fuel cell. The preparation method is simple and controllable, and the prepared high-temperature proton exchange membrane has excellent phosphoric acid retention performance, low hydrogen permeation and high proton conductivity.
[0035] The preparation method of the present invention mainly includes three steps: preparation of porous base membrane, formation of cross-linked dense double skin layer and acid doping post-treatment. The structural schematic diagram of the porous proton exchange membrane and the cross-linked porous proton exchange membrane is shown in FIG. Figure 1 As shown, the details are as follows:
[0036] (1) Preparation of porous substrate membrane
[0037] The polymer containing nitrogen heterocycle in the main chain is dissolved in a suitable organic solvent (such as DMF, DMAc, NMP, DMSO, adjusted according to different polymers) to form a polymer membrane solution, the preferred concentration range of which is 4-10wt%; then a certain amount of porogen (such as dibutyl phthalate, polyethylene glycol, polyacrylic acid) is added, usually the mass proportion of the porogen is 10-70wt%, preferably 50wt%. After the final mixed polymer solution is stirred evenly, a film is formed on a clean substrate, and dried at 80-120°C (according to the different selected solvents, the corresponding film forming temperature is adjusted) for 12-24 hours, and the solvent is completely volatilized, and then the composite membrane is immersed in a solvent (such as deionized water, anhydrous ethanol, methanol, isopropanol, acetone) to dissolve the porogen in the membrane, and then taken out for ultrasonic cleaning, and after drying, a porous membrane substrate is obtained.
[0038] (2) Preparation of cross-linked dense double skin layer
[0039] The porous polymer membrane obtained in step (1) is immersed in a certain concentration of polybasic organic phosphonic acid (such as ATMP, HEDP, EDTMPA) aqueous solution at a certain temperature, wherein the concentration of the organic phosphonic acid aqueous solution is 10-60%, and the ambient temperature is 100° C., so that the polymer membrane matrix and the organic phosphonic acid are fully cross-linked, and a dense double skin layer with a cross-linked structure is formed on both sides of the porous membrane;
[0040] (3) Acid doping post-treatment
[0041] The cross-linked membrane with a dense double skin layer obtained in step (2) is immersed in a phosphoric acid / heteropoly acid solution of a certain concentration for 48-96 hours at a temperature of 60-100°C. After taking out the membrane, the acid remaining on the surface is wiped off to obtain a cross-linked porous structure high-temperature proton exchange membrane with high stability.
[0042] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0043] Example 1
[0044] The high molecular polymer is polybenzimidazole OPBI, the porogen is dibutyl phthalate, and the organic phosphonic acid is aminotrimethylene phosphonic acid. The specific preparation process is as follows:
[0045] Polybenzimidazole OPBI with chemical corrosion resistance and thermal stability is dissolved in N,N-dimethylacetamide (DMAc) to form a polymer membrane solution with a concentration of 4.67wt%; after stirring evenly, dibutyl phthalate is added thereto, with a mass proportion of 50wt%. The mixed system is fully stirred at 40°C for 5 hours, and the final mixed polymer solution is subjected to film-forming treatment on a clean substrate, and dried at 80°C for 24 hours. After the solvent is completely evaporated, the composite membrane is immersed in anhydrous ethanol to dissolve the dibutyl phthalate in the membrane. The immersion temperature is 60°C and the immersion time is 72 hours. After the dibutyl phthalate is completely dissolved, the polymer membrane is taken out for ultrasonic cleaning. After drying, a porous OPBI membrane is obtained.
[0046] The porous OPBI membrane was immersed in an aqueous solution of aminotrimethylenephosphonic acid (ATMP), the optimal concentration of which was 50%, and the immersion temperature was 100°C, so that OPBI and ATMP reacted as follows. Figure 2 The cross-linking reaction is carried out as shown, and the water is dried to obtain a cross-linked porous OPBI proton exchange membrane with a dense double skin layer.
[0047] Then, a protonation treatment is performed, and the obtained cross-linked porous OPBI polymer membrane is immersed in a phosphoric acid solution (85wt%) at 60°C for 48h. After the membrane is taken out, the acid remaining on the surface is wiped off to obtain a cross-linked porous high-temperature proton exchange membrane with high stability.
[0048] The obtained cross-linked porous high-temperature proton exchange membrane has good proton conductivity, phosphoric acid retention performance and low hydrogen permeation current density. Figure 3 As shown, at 160°C, the conductivity is 0.112 S cm -1 The result is the conductivity in the direction perpendicular to the membrane plane measured by the AC impedance spectroscopy technique, and the instrument used is the IVIUMsat electrochemical workstation. The output peak power density of the hydrogen-oxygen single cell assembled with this membrane is 0.98W cm at 160℃ -2 , and the hydrogen permeation current density is only 0.99 mA cm -2 ( Figure 5 ).
[0049] Example 2
[0050] The high molecular polymer is polybenzimidazole OPBI, the porogen is polyethylene glycol, and the organic phosphonic acid is hydroxyethylidene diphosphonic acid (HEDP). The specific preparation process is as follows:
[0051] The chemically resistant and thermally stable polybenzimidazole OPBI is dissolved in N,N-dimethylacetamide (DMAc) to form a polymer membrane solution with a concentration of 8wt%; polyethylene glycol is added thereto after being stirred evenly, and the preferred addition amount is 8-10wt%. The mixed system is fully stirred at 40°C for 6 hours, and the final mixed polymer solution is subjected to film-forming treatment on a clean substrate, and dried at 110°C for 12 hours. After the solvent is completely evaporated, the composite membrane is thoroughly washed with deionized water to remove the polyethylene glycol in the membrane. After the polyethylene glycol in the membrane is completely removed, the polymer membrane is taken out for ultrasonic cleaning, and after drying, a porous OPBI membrane is obtained.
[0052] The obtained porous OPBI membrane is immersed in a hydroxyethylidene diphosphonic acid (HEDP) aqueous solution with a concentration of 50% and an immersion temperature of 100°C. When OPBI and HEDP are fully cross-linked, the membrane is taken out and the water is dried to obtain a cross-linked porous OPBI proton exchange membrane with a dense double skin layer.
[0053] Then, a protonation treatment is performed, and the obtained cross-linked porous OPBI proton exchange membrane is immersed in a phosphoric acid solution (85wt%) at 60°C for 48 hours. After the membrane is taken out, the acid remaining on the surface is wiped off to obtain a cross-linked porous high-temperature proton exchange membrane with high stability.
[0054] Example 3
[0055] The high molecular polymer is polybenzimidazole ABPBI, the porogen is polyacrylic acid, and the organic phosphonic acid is ethylenediaminetetramethylenephosphonic acid (EDTMPA). The specific preparation process is as follows:
[0056] The polybenzimidazole ABPBI with chemical corrosion resistance and thermal stability is dissolved in N-methylpyrrolidone (NMP) to form a polymer membrane solution with a concentration of 6wt%; after stirring evenly, polyacrylic acid is added thereto, and the preferred addition amount is 80wt%. The mixed system is fully stirred at 30°C for 2 hours, and the final mixed polymer solution is subjected to film-forming treatment on a clean substrate, and dried at 80°C for 12 hours. After the solvent is completely volatilized, the above composite membrane is immersed in deionized water for 72 hours to completely remove the residual solvent in the membrane, and then the polymer membrane is taken out for ultrasonic cleaning. After drying, a porous ABPBI membrane is obtained.
[0057] The obtained porous ABPBI membrane is immersed in an aqueous solution of ethylenediaminetetramethylenephosphonic acid (EDTMPA), the concentration of the aqueous solution of ethylenediaminetetramethylenephosphonic acid (EDTMPA) is 40%, and the immersion temperature is 100°C. When ABPBI and ethylenediaminetetramethylenephosphonic acid (EDTMPA) are fully cross-linked, they are taken out and the water is dried to obtain a cross-linked porous ABPBI proton exchange membrane with a dense double skin layer.
[0058] Subsequently, a protonation treatment is performed, and the obtained cross-linked porous ABPBI proton exchange membrane is immersed in a phosphoric acid solution (85wt%) at 60°C for 48 hours. After the membrane is taken out, the acid remaining on the surface is wiped off to obtain a cross-linked porous high-temperature proton exchange membrane with high stability.
[0059] Comparative Example 1
[0060] The high molecular polymer is polybenzimidazole OPBI, and the porogen is dibutyl phthalate. The specific preparation process is as follows:
[0061] Polybenzimidazole OPBI with chemical corrosion resistance and thermal stability is dissolved in N,N-dimethylacetamide (DMAc) to form a polymer membrane solution with a concentration of 4.67wt%; after stirring evenly, dibutyl phthalate is added thereto, with a mass proportion of 50wt%. The mixed system is fully stirred at 40°C for 5 hours, and the final mixed polymer solution is subjected to film-forming treatment on a clean substrate, and dried at 80°C for 24 hours. After the solvent is completely evaporated, the composite membrane is immersed in anhydrous ethanol to dissolve the dibutyl phthalate in the membrane. The immersion temperature is 60°C and the immersion time is 72 hours. After the dibutyl phthalate is completely dissolved, the polymer membrane is taken out for ultrasonic cleaning. After drying, a porous OPBI membrane is obtained.
[0062] Then, the protonation treatment was performed, and the obtained porous OPBI polymer membrane was immersed in a phosphoric acid solution (85 wt%) at 60° C. for 48 hours. After the membrane was taken out, the acid remaining on the surface was wiped off to obtain a porous high-temperature proton exchange membrane.
[0063] The conductivity of the porous high-temperature proton exchange membrane was 0.082S cm at 160°C. -1 ( Figure 3 ), which is the conductivity perpendicular to the membrane plane measured by AC impedance spectroscopy, using an IVIUMsat electrochemical workstation. The peak power density of the hydrogen-oxygen cell assembled with this membrane is 0.92W cm at 160°C. -2 , the hydrogen permeation current density is 25.97 mA cm -2 ( Figure 5 ).
[0064] Depend on Figure 2 It can be seen that the cross-linked porous high-temperature proton exchange membrane with a dense double skin layer (Example 1) prepared by the present invention has a higher proton conductivity than the porous proton exchange membrane without a dense skin layer (Comparative Example 1); and in a humid environment, such as Figure 4 As shown in FIG. 1 , the phosphoric acid retention performance of Example 1 is much better than that of Control Example 1, indicating that a reasonable dense skin layer is beneficial to the phosphoric acid retention performance of the porous proton exchange membrane. Example 1 and Control Example 1 were assembled into fuel cells, and their battery performance was tested. Figure 5 As shown, the peak power density of Example 1 (0.98 W cm -2 ) is higher than that of control example 1 (0.92W cm -2 ), and in the constant current discharge stability test ( Figure 6 ), the internal resistance and battery voltage of Example 1 remain stable, while the internal resistance of Control Example 1 increases and the battery voltage decays rapidly due to the rapid loss of phosphoric acid.
[0065] In addition, the foregoing only describes some embodiments, which may be changed, modified, added and / or varied without departing from the scope and essence of the disclosed embodiments, which are illustrative rather than restrictive. In addition, the described embodiments relate to the embodiments currently considered to be the most practical and preferred, and it should be understood that the embodiments should not be limited to the disclosed embodiments, but rather, are intended to cover different modifications and equivalent arrangements included within the essence and scope of the embodiments. In addition, the various embodiments described above may be used in conjunction with other embodiments, such as aspects of one embodiment may be combined with aspects of another embodiment to achieve yet another embodiment. In addition, each independent feature or component of any given component may constitute another embodiment.
[0066] The foregoing description of the embodiment is provided for the purpose of illustration and description, and it is not intended to be exhaustive or limit the present disclosure. Each element or feature of a specific embodiment is generally not limited to the specific embodiment, but in the applicable case, even if not specifically shown or described, each element or feature is also interchangeable and can be used for the selected embodiment, and can also be changed in many ways. This change is not regarded as a deviation from the present disclosure, and all such changes are included in the scope of the present disclosure.
[0067] Therefore, it should be understood that the drawings and description herein are provided by way of illustration to facilitate understanding of the present invention and should not be construed as limiting the scope thereof.
Claims
1. A method for preparing a cross-linked porous high-temperature proton exchange membrane, characterized in that: The following steps are included: (1) Preparation of porous membrane substrate Dissolving a high molecular polymer containing a nitrogen heterocycle in a main chain in an organic solvent of the polymer to obtain a first polymer solution; using the first polymer solution to form a film by casting with a porogen, or casting to form a liquid film and preparing a porous base film by a water vapor induced phase inversion method; (2) Formation of a cross-linked dense double skin layer The porous polymer membrane obtained in step (1) is immersed in a polybasic organic phosphonic acid aqueous solution at a certain temperature and a certain concentration to complete the cross-linking process between the polybasic organic phosphonic acid and the polymer membrane, thereby forming a dense double skin layer with a cross-linked structure on the surface of the porous membrane; (3) Acid doping post-treatment The cross-linked porous structure membrane obtained in step (2) is saturated with acid and then the residual acid is removed to obtain the cross-linked porous structure high-temperature proton exchange membrane.
2. The method for preparing a cross-linked porous high-temperature proton exchange membrane according to claim 1, characterized in that: In step (1), the polymer having a nitrogen heterocycle in the main chain is polybenzimidazole (PBI), polyarylpiperidine (PAPi) or polyarylpyridine (PAPy); and the organic solvent is N, N-dimethylformamide or N, N-dimethylacetamide.
3. The method for preparing a cross-linked porous high-temperature proton exchange membrane according to claim 1 or 2, characterized in that: The specific steps of using a porogen to form a film by tape casting in step (1) are as follows: a certain amount of a porogen is added to a first polymer solution under stirring conditions to obtain a second polymer solution; the second polymer solution is tape cast on a clean substrate, and the solvent is heated to evaporate to obtain a composite membrane; and the obtained composite membrane is immersed in a solvent to dissolve the porogen in the membrane, thereby obtaining a porous base membrane.
4. The method for preparing a cross-linked porous high-temperature proton exchange membrane according to claim 1 or 2, characterized in that: The step (1) of forming a liquid film by casting and preparing a porous base membrane by a water vapor induced phase inversion method is specifically as follows: casting a first polymer solution on a clean substrate to form a liquid film, and placing the liquid film in a water vapor environment with a certain temperature and humidity, and preparing a porous base membrane by a water vapor induced phase inversion method.
5. The method for preparing a cross-linked porous high-temperature proton exchange membrane according to claim 1 or 2, characterized in that: The step (3) specifically comprises: immersing the cross-linked porous structure membrane obtained in step (2) in an 85wt% concentrated phosphoric acid solution until the membrane reaches acid absorption saturation, and removing the residual attached acid on the surface after taking it out to obtain the cross-linked porous structure high temperature proton exchange membrane.
6. The method for preparing a cross-linked porous high-temperature proton exchange membrane according to claim 1, characterized in that: The porogen described in step (1) is a combination of one or more of inorganic nanopowder or organic liquid dibutyl phthalate, low molecular weight polyethylene glycol or polyacrylic acid.
7. The preparation method according to claim 1, characterized in that: The polybasic organic phosphonic acid in step (2) is a combination of one or more of hydroxyethylidene diphosphonic acid (HEDP), aminotrimethylene phosphonic acid (ATMP), ethylenediaminetetramethylenephosphonic acid (EDTMPA), diethylenetriaminepentamethylenephosphonic acid (DTPMPA), hexamethylenediaminetetramethylenephosphonic acid (HDTMPA), and dihexylenetriaminepentamethylenephosphonic acid (BHMTPMPA); the concentration of the polybasic organic phosphonic acid is 5-60 wt%.
8. The preparation method according to claim 7, characterized in that: The concentration of the polybasic organic phosphonic acid is 20-50 wt%.
9. A cross-linked porous high temperature proton exchange membrane obtained by the method of any one of claims 1 to 8, characterized in that: The exchange membrane comprises an intermediate porous layer and a cross-linked dense double surface layer; the intermediate porous layer stores free phosphoric acid to obtain high proton conductivity, and the cross-linked dense double surface layer has a proton conduction function.
10. A cross-linked porous high-temperature proton exchange membrane according to claim 9, characterized in that: When the exchange membrane is at 160 °C, the conductivity is 0.112 S cm -1 The hydrogen permeation current density of the hydrogen-oxygen single cell assembled using the exchange membrane at 160 °C is 0.99 mA cm -2 , the output power density is 0.98 W cm -2 .
11. Use of the high temperature proton exchange membrane according to any one of claims 9 to 10 in electrolyte diaphragm materials of high temperature proton exchange membrane fuel cells or diaphragm materials of flow batteries, water electrolyzers, and electrochemical devices.