A method for preparing embedded specimens

Through the lyophilization and embedding process, combined with specific treatment liquid and resin process, the problem of morphology and color of hairy mammal specimens during fixing and preservation is solved, and the effect of natural, transparent and long-term preservation is achieved.

CN115836675BActive Publication Date: 2024-11-19NANNING QIANFAN TEACHING TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211505230.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-28
Publication Date
2024-11-19
Estimated Expiration
2042-11-28

AI Technical Summary

Technical Problem

In the production of hairy mammal specimens, formaldehyde is used to fix or taxiderm the formaldehyde, fur is prone to be attached or deformed, and preservatives are highly toxic, making it difficult to ensure the natural and permanent appearance of the batch finished product. save.

Method used

Using lyophilized hairy mammals to apply fur treatment solution and fur on the abdominal and thoracic cavity, combined with epoxy resin or PMMA embedding process, ensure the natural preservation of fur color and morphology, and through lyophilization and The combination of cosolvents and curing agents used during the embedding process prevents hair from bonding and deformation.

Benefits of technology

The morphology and fur color of hairy mammal specimens are achieved, with high transparency, and do not change or fade under light, and have better storage performance and production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115836675B_ABST
    Figure CN115836675B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of specimen preparation, and specifically relates to a method for preparing an embedded specimen, which comprises the following steps: (1) killing a hairy mammal, cutting open its abdomen, removing the internal organs of its chest and abdominal cavities, and obtaining an empty-stomach hairy mammal; (2) applying a pretreatment liquid to the abdominal and chest cavities of the empty-stomach hairy mammal; (3) applying a fur treatment liquid to the fur of the empty-stomach hairy mammal; (4) filling the chest and abdominal cavities of the empty-stomach hairy mammal, suturing the abdominal incision, shaping, freeze-drying, embedding, grinding, and polishing to obtain an embedded specimen. The method of the present invention ensures that the hairy mammal after freeze-drying still maintains the original fur color and external morphology, and the hairy mammal does not change color or fade when exposed to light.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of specimen preparation, and in particular relates to a method for preparing an embedded specimen. Background Art

[0002] Embedded specimens (artificial amber) are made by embedding various biological specimen materials with high-transparency polymer resins. The main features are that the product is crystal clear, easy to observe, real and natural, and permanently preserved. Due to the teaching applicability and safety and durability of the product, it has been well received by teaching, scientific research institutions and consumers since it entered the market. There is no teaching embedded specimen made by embedding freeze-dried mammals with resin on the market.

[0003] In the prior art, formalin containing formaldehyde is usually used to fix hairy mammal specimens, or the skinning method is used to prepare hairy mammal skinned specimens, and then the specimens are embedded. Both methods have their own disadvantages. For example, soaking hairy mammals in formalin not only causes formaldehyde hazards, but also makes the fur of hairy mammals soaked in formalin easily flattened or turned up; if the skinning method is used to prepare hairy mammal skinned specimens, and then embedding the specimens, the preservatives and fixatives used in this method are highly toxic. In addition, the skinning method loses the original support of the bones, and after filling the prosthesis, the hairy mammals are greatly deformed, and the appearance of the finished products produced in batches cannot be guaranteed. Summary of the invention

[0004] The present invention aims to solve the above-mentioned technical problems and provides a method for preparing an embedded specimen. The method of the present invention allows the hairy mammal to still maintain the original fur color and external shape after freeze-drying, and the hairy mammal to still maintain the original color and fluffy and vivid shape of the fur after embedding. Moreover, during the use of the embedded specimen of the hairy mammal, the hairy mammal will not change color or fade due to exposure to light.

[0005] In order to solve the above technical problems, the technical solution of the present invention is:

[0006] A method for preparing an embedded specimen comprises the following steps:

[0007] (1) killing a hairy mammal, cutting it open along the abdomen, removing its visceral organs from the chest and abdomen, and obtaining an empty-stomach hairy mammal;

[0008] (2) applying a pretreatment solution to the abdominal cavity and chest cavity of the fasting hairy mammal, using 1-4 ml of the pretreatment solution per kilogram of the fasting hairy mammal; the pretreatment solution is a mixture of benzoic acid, paraben, potassium sorbate and cosolvent A;

[0009] (3) applying a fur treatment liquid in an amount of 1.8 to 2.2 times the weight of the fasting hairy mammal on the fur of the fasting hairy mammal; the fur treatment liquid is a mixture of anhydrous ethanol, a surfactant, ammonia water and a cosolvent B, and the surfactant is one of sodium laureth sulfate, sodium lauryl sulfate and sodium laureth-3 acetate;

[0010] (4) filling the chest and abdominal cavities of fasting hairy mammals, suturing the abdominal incision, shaping, freeze-drying, embedding, grinding, and polishing to obtain embedded specimens.

[0011] Generally speaking, any mammal with hair can be used, but in the present invention, the mammal with hair is preferably a rabbit or a mouse.

[0012] Preferably, the co-solvent A of the present invention is an ethanol solution with a volume concentration of 70%, and the co-solvent B is pure water.

[0013] Applying the pretreatment liquid inside the thoracic cavity and abdominal cavity of a mammal can inhibit bacteria and preserve corrosion, and then shaping and freeze-drying to ensure that the body shape of the hairy mammal is natural and lifelike during and after freeze-drying. Preferably, in step (2) of the present invention, the pretreatment liquid is made of the following raw materials in weight percentage: 0.5-2% benzoic acid, 2-6% paraben complex ester, 1-4% potassium sorbate, and cosolvent A is added to 100%. After the pretreatment liquid of the present invention is prepared, it can be evenly distributed in the thoracic cavity and abdominal cavity of a mammal, achieving an excellent antibacterial and antiseptic effect, and through compounding, only a small amount is needed to achieve an excellent antiseptic effect.

[0014] The use of fur treatment liquid on mammalian fur can remove the grease on the fur surface, making the color and shape of the fur of the fur mammal natural and realistic during and after freeze-drying, and also making the body hair smooth and fluffy, clean the fur, and after being immersed in resin for embedding, it can naturally spread out in the viscous resin, consistent with its fluffy and smooth state in the air under natural conditions, and will not form blocks and get tangled together. In order to obtain the above effect, preferably, in step (3) of the present invention, the fur treatment liquid is made of the following raw materials in weight percentage: 12.2-12.8% anhydrous ethanol, 8.9-9.8% surfactant, 0.78-0.92% ammonia water, and co-solvent B is added to 100%.

[0015] Preferably, the pretreatment liquid is applied within 0-10 minutes after removing the internal organs from the chest and abdomen of the hairy mammal, and the fur treatment liquid is used on the fur 10-15 minutes after the application of the pretreatment liquid. This will achieve the best preservation effect and facilitate the subsequent plastic surgery. If the above time is exceeded, it will be detrimental to the subsequent plastic surgery, and the obtained hairy mammal will have a stiff morphology, making it difficult to obtain a specimen with a natural morphology.

[0016] Preferably, in step (4) of the present invention, the specific steps of embedding are: mixing the main glue and the curing agent in a weight ratio of 3:1 to obtain a mixed solution; adding the mixed solution to a mold, and when the mixed solution begins to solidify, putting the freeze-dried and shaped hairy mammal into it, and after the mixed solution is completely solidified, adding the mixed solution again until the entire body of the hairy mammal is covered and solidified.

[0017] Preferably, the main adhesive of the present invention is made of the following raw materials in weight percentage: 80-95% epoxy resin, 1-12% active diluent, 0.1-8% accelerator, 0.1-1% ultraviolet absorber, and 0.1-1% antioxidant; the curing agent is at least one of polyetheramine, isophorone diamine, fatty amine, and acid anhydride. Using the main adhesive and curing agent components of the present invention can shorten the production cycle and improve production efficiency.

[0018] Preferably, the active diluent is at least one of 1,4-butanediol diglycidyl ether, C12-C14 aliphatic glycidyl ether, butyl glycidyl ether, and o-cresol glycidyl ether; and the accelerator is at least one of nonylphenol or dimethylimidazole.

[0019] In order to obtain a specimen with higher transparency and gloss and no discoloration, preferably, in step (4) of the present invention, the embedding can also adopt an MMA embedding process, comprising the following steps:

[0020] (1) Synthesis of PMMA prepolymer: 85-95 wt.% of methyl methacrylate, 0.5-5 wt.% of methacrylic acid, 4-10 wt.% of methacrylic acid functional monomer and 0.05-1 wt.% of initiator are mixed, reacted at a reaction temperature of 50-100° C. for 1-8 hours, and cooled to room temperature to obtain a PMMA prepolymer having a viscosity of 50-5000 cps at 25° C.;

[0021] (2) adding 0.3-0.6% of the weight of the PMMA prepolymer initiator to the PMMA prepolymer, mixing to obtain a mixture, pouring the mixture into a mold, maintaining it at 45-55° C. for 11.5-12.5 hours, then putting the freeze-dried and shaped hairy mammal into it, adding the mixture again until the entire body of the hairy mammal is covered, and finally maintaining it at 45-55° C. for 11.5-12.5 hours.

[0022] The invention allows the hairy mammal to be encapsulated in a transparent resin in an embedding manner, so as to be permanently preserved, and can be connected with accessories to form an embedded specimen.

[0023] Due to the adoption of the above technical solution, the beneficial effects of the present invention are:

[0024] 1. The method of the present invention can obtain a hairy mammal embedded specimen with natural fur color and realistic morphology. The specimen has high transparency and can better present the morphology and fur color of the hairy mammal.

[0025] 2. The method of the present invention allows the fur and external appearance of hairy mammals to maintain their original color and shape after freeze-drying, especially making the fur of hairy mammals fluffy, and allowing them to naturally spread out after being embedded and injected with resin in the later stage, without clumping and tangling together, and making the hair of hairy mammals consistent with the fluffy and smooth state in the air under natural conditions.

[0026] 3. During the later storage process of the embedded specimen of the hairy mammal prepared by the method of the present invention, the fur of the hairy mammal will not turn yellow under light irradiation, and has better storage performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is the rabbit embedded specimen obtained in Example 1 of the present invention.

[0028] Figure 2 This is the rabbit embedded specimen obtained in Example 5 of the present invention.

[0029] Figure 3 This is the embedded specimen of mice obtained in Example 8 of the present invention. DETAILED DESCRIPTION

[0030] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] Example 1

[0032] (1) The rabbit was killed, and a 5 cm incision was made along the abdomen to remove the internal organs of the chest and abdomen. At the same time, the rabbit was bled by cutting the aorta and rinsed with clean water to obtain an empty-stomach rabbit;

[0033] (2) 10 minutes after the organ is removed, a pretreatment solution is dipped into an absorbent cotton ball and evenly applied to the chest and abdominal surfaces of the fasting rabbit. 3 ml of the pretreatment solution is used per kilogram of the fasting rabbit. The pretreatment solution is made of the following raw materials in weight percentage: 0.8% benzoic acid, 2% paraben complex ester, 3.4% potassium sorbate, and 93.8% ethanol solution with a volume concentration of 70%;

[0034] (3) applying a fur treatment liquid twice the weight of the fasting rabbit on the fur of the fasting rabbit, rubbing the fur, and then washing it with a large amount of clean water, and draining the water; the fur treatment liquid is made of the following raw materials in weight percentage: 12.8% anhydrous ethanol, 9.4% sodium laureth sulfate, 0.85% ammonia water, and 76.95% purified water;

[0035] (4) Fill the rabbit's chest and abdominal cavities with PP cotton, suture the abdominal incision, and replace the rabbit's eyeball with an artificial eye;

[0036] (5) Plastic surgery: Use EVA board and bamboo sticks to fix the rabbit's appearance and posture;

[0037] (6) Freeze-drying: The rabbits were freeze-dried using a ZD-A3 freeze dryer. The rabbits were placed on a stainless steel tray and placed on the plate layer in the freeze dryer. They were pre-frozen at -45°C for 3 hours. The freeze dryer evaporation program was then adjusted to: -45 to -30°C, 24 hours; -30 to -25°C, 24 hours; -25 to -20°C, 24 hours; -20 to -15°C, 24 hours; -15 to -10°C, 24 hours; -10 to -5°C, 10 hours; -5 to 0°C, 10 hours ; 0-5°C, 5 hours; 5-10°C, 5 hours; 10-15°C, 5 hours; 15-20°C, 5 hours; 20-25°C, 5 hours; 25-30°C, 5 hours; 30-35°C, 5 hours; 35-40°C, 5 hours; 40-45°C, 5 hours; 45-50°C, 5 hours. During the whole process, the water trap temperature was maintained at about -60°C, and the vacuum degree was maintained at 8pa until the whole program was automatically shut down after the operation. The moisture content of the freeze-dried rabbit was 3%;

[0038] (7) Embedding: Evenly mix epoxy resin main glue and acid anhydride in a weight ratio of 3:1, vacuum evacuate to obtain a mixed solution, add the mixed solution to a depth of 2 mm in a square transparent acrylic mold, and when the mixed solution begins to solidify, gently place the freeze-dried rabbit on the surface of the colloid, and the rabbit will sink lightly into the colloid. After curing for 6 hours, the colloid becomes a transparent solid, and the position of the rabbit is also fixed. Continue to add the mixed solution until the whole body of the rabbit is covered, put it into a vacuum machine to remove the bubbles attached to the rabbit, and cure it at room temperature for 12 hours to obtain a completely transparent square rabbit embedded specimen crystal; the main glue is made of the following raw materials in weight percentage: epoxy resin NPEL128 86.5%, butyl glycidyl ether 7.5%, nonylphenol 5%, ultraviolet absorber UV-1960.5%, antioxidant V73-P 0.5%;

[0039] (8) Grinding off burrs and polishing to obtain a rabbit embedded specimen, which retains the original color and morphology of the rabbit (fluffy and natural fur). The morphology of the rabbit after drying is the same as that of a fresh rabbit. The embedded rabbit specimen is placed outdoors for aging for 2 months. The color of the rabbit hair does not fade significantly, and the specimen crystal does not turn yellow significantly. It is placed indoors for 6 months, and the color of the rabbit hair does not fade, and the specimen crystal does not turn yellow significantly.

[0040] Example 2

[0041] (1) The rabbit was killed, and a 5 cm incision was made along the abdomen to remove the internal organs of the chest and abdomen. At the same time, the rabbit was bled by cutting the aorta and rinsed with clean water to obtain an empty-stomach rabbit;

[0042] (2) 10 minutes after the organ is removed, a pretreatment solution is dipped into an absorbent cotton ball and evenly applied to the chest and abdominal surfaces of the fasting rabbit. 1 ml of the pretreatment solution is used per kilogram of the fasting rabbit. The pretreatment solution is made of the following raw materials in weight percentage: 0.8% benzoic acid, 2% paraben complex ester, 3.4% potassium sorbate, and 93.8% ethanol solution with a volume concentration of 70%;

[0043] (3) applying a fur treatment liquid in an amount of 1.8 times the weight of the fasting rabbit on the fur of the fasting rabbit, rubbing the fur, and then washing it with a large amount of clean water, and draining the water; the fur treatment liquid is made of the following raw materials in weight percentage: 12.8% anhydrous ethanol, 9.4% sodium lauryl sulfate, 0.85% ammonia water, and 76.95% purified water;

[0044] (4) Fill the rabbit's chest and abdominal cavities with PP cotton, suture the abdominal incision, and replace the rabbit's eyeball with an artificial eye;

[0045] (5) Plastic surgery: Use EVA board and bamboo sticks to fix the rabbit's appearance and posture;

[0046] (6) Freeze-drying: The rabbits were freeze-dried using a ZD-A3 freeze dryer. The rabbits were placed on a stainless steel tray and placed on the plate layer in the freeze dryer. They were pre-frozen at -45°C for 3 hours. The freeze dryer evaporation program was then adjusted to: -45 to -30°C, 24 hours; -30 to -25°C, 24 hours; -25 to -20°C, 24 hours; -20 to -15°C, 24 hours; -15 to -10°C, 24 hours; -10 to -5°C, 10 hours; -5 to 0°C, 10 hours ; 0-5°C, 5 hours; 5-10°C, 5 hours; 10-15°C, 5 hours; 15-20°C, 5 hours; 20-25°C, 5 hours; 25-30°C, 5 hours; 30-35°C, 5 hours; 35-40°C, 5 hours; 40-45°C, 5 hours; 45-50°C, 5 hours. During the whole process, the water trap temperature was maintained at about -60°C, and the vacuum degree was maintained at 8pa until the whole program was automatically shut down after the operation. The moisture content of the freeze-dried rabbit was 3%;

[0047] (7) Embedding: Evenly mix epoxy resin main glue and fatty amine in a weight ratio of 3:1, vacuum evacuate to obtain a mixed solution, add the mixed solution to a depth of 2 mm in a square transparent acrylic mold, and when the mixed solution begins to solidify, gently place the freeze-dried rabbit on the surface of the colloid, and the rabbit will sink lightly into the colloid. After curing for 6 hours, the colloid becomes a transparent solid, and the position of the rabbit is also fixed. Continue to add the mixed solution until the whole body of the rabbit is covered, put it into a vacuum machine to remove the bubbles attached to the rabbit, and cure it at room temperature for 12 hours to obtain a completely transparent square rabbit embedded specimen crystal; the main glue is made of the following raw materials in weight percentage: epoxy resin NPEL128 86.5%, 1,4-butanediol diglycidyl ether 12%, dimethylimidazole 0.1%, ultraviolet absorber UV-1961%, antioxidant V73-P 0.4%;

[0048] (8) Grinding off burrs and polishing to obtain a rabbit embedded specimen, which retains the original color and morphology of the rabbit (fluffy and natural hair). The morphology of the rabbit after drying is the same as that of a fresh rabbit. The embedded rabbit specimen is placed outdoors for aging for 2 months. The color of the rabbit hair does not fade significantly, and the specimen crystal does not turn yellow significantly. It is placed indoors for 6 months. The color of the rabbit hair does not fade significantly, and the specimen crystal does not turn yellow significantly, and the transparency is high.

[0049] Example 3

[0050] (1) The rabbit was killed, and a 5 cm incision was made along the abdomen to remove the internal organs of the chest and abdomen. At the same time, the rabbit was bled by cutting the aorta and rinsed with clean water to obtain an empty-stomach rabbit;

[0051] (2) 10 minutes after the organ is removed, a pretreatment solution is dipped into an absorbent cotton ball and evenly applied to the chest and abdominal surfaces of the fasting rabbit. 1 ml of the pretreatment solution is used per kilogram of the fasting rabbit. The pretreatment solution is made of the following raw materials in weight percentage: 0.8% benzoic acid, 2% paraben complex ester, 3.4% potassium sorbate, and 93.8% ethanol solution with a volume concentration of 70%;

[0052] (3) applying a fur treatment liquid in an amount of 1.8 times the weight of the fasting rabbit on the fur of the fasting rabbit, rubbing the fur, and then washing it with a large amount of clean water, and draining the water; the fur treatment liquid is made of the following raw materials in weight percentage: 12.8% anhydrous ethanol, 9.4% sodium laureth-3 acetate, 0.85% ammonia water, and 76.95% purified water;

[0053] (4) Fill the rabbit's chest and abdominal cavities with PP cotton, suture the abdominal incision, and replace the rabbit's eyeball with an artificial eye;

[0054] (5) Plastic surgery: Use EVA board and bamboo sticks to fix the rabbit's appearance and posture;

[0055] (6) Freeze-drying: The rabbits were freeze-dried using a ZD-A3 freeze dryer. The rabbits were placed on a stainless steel tray and placed on the plate layer in the freeze dryer. They were pre-frozen at -45°C for 3 hours. The freeze dryer evaporation program was then adjusted to: -45 to -30°C, 24 hours; -30 to -25°C, 24 hours; -25 to -20°C, 24 hours; -20 to -15°C, 24 hours; -15 to -10°C, 24 hours; -10 to -5°C, 10 hours; -5 to 0°C, 10 hours ; 0-5°C, 5 hours; 5-10°C, 5 hours; 10-15°C, 5 hours; 15-20°C, 5 hours; 20-25°C, 5 hours; 25-30°C, 5 hours; 30-35°C, 5 hours; 35-40°C, 5 hours; 40-45°C, 5 hours; 45-50°C, 5 hours. During the whole process, the water trap temperature was maintained at about -60°C, and the vacuum degree was maintained at 8pa until the whole program was automatically shut down after the operation. The moisture content of the freeze-dried rabbit was 3%;

[0056] (7) Embedding: Evenly mix epoxy resin main glue and polyetheramine in a weight ratio of 3:1, vacuum evacuate to obtain a mixed solution, add the mixed solution to a depth of 2 mm in a square transparent acrylic mold, and when the mixed solution begins to solidify, gently place the freeze-dried rabbit on the surface of the colloid. The rabbit will sink lightly into the colloid. After curing for 6 hours, the colloid becomes a transparent solid and the rabbit is fixed in position. Continue to add the mixed solution until the whole body of the rabbit is covered, put it into a vacuum machine to remove the bubbles attached to the rabbit, and cure it at room temperature for 12 hours to obtain a completely transparent square rabbit embedded specimen crystal; the main glue is made of the following raw materials in weight percentage: epoxy resin NPEL128 95%, C12-14 alcohol aliphatic glycidyl ether (AGE) 1%, nonylphenol 2%, dimethylimidazole 1.4%, ultraviolet absorber UV-196 0.5%, antioxidant V73-P 0.1%; the curing agent is polyetheramine D230 A mixture of 75wt.% of 1,2-diaminobenzene and 25wt.% of isophorone diamine IPDA;

[0057] (8) Grinding off burrs and polishing to obtain a rabbit embedded specimen, which retains the original color and morphology of the rabbit (fluffy and natural fur). The morphology of the rabbit after drying is the same as that of a fresh rabbit. The embedded rabbit specimen is placed outdoors for aging for 2 months. The color of the rabbit hair does not fade significantly, and the specimen crystal does not turn yellow significantly. It is placed indoors for 6 months, and the color of the rabbit hair does not fade, and the specimen crystal does not turn yellow significantly.

[0058] Example 4

[0059] (1) The rabbit was killed, and a 5 cm incision was made along the abdomen to remove the internal organs of the chest and abdomen. At the same time, the rabbit was bled by cutting the aorta and rinsed with clean water to obtain an empty-stomach rabbit;

[0060] (2) 10 minutes after the organ is removed, a pretreatment solution is dipped into an absorbent cotton ball and evenly applied to the chest and abdominal surfaces of the fasting rabbit. 1 ml of the pretreatment solution is used per kilogram of the fasting rabbit. The pretreatment solution is made of the following raw materials in weight percentage: 0.8% benzoic acid, 2% paraben complex ester, 3.4% potassium sorbate, and 93.8% ethanol solution with a volume concentration of 70%;

[0061] (3) applying a fur treatment liquid in an amount of 1.8 times the weight of the fasting rabbit on the fur of the fasting rabbit, rubbing the fur, and then washing it with a large amount of clean water, and draining the water; the fur treatment liquid is made of the following raw materials in weight percentage: 12.8% anhydrous ethanol, 9.4% sodium laureth sulfate, 0.85% ammonia water, and 76.95% purified water;

[0062] (4) Fill the rabbit's chest and abdominal cavities with PP cotton, suture the abdominal incision, and replace the rabbit's eyeball with an artificial eye;

[0063] (5) Plastic surgery: Use EVA board and bamboo sticks to fix the rabbit's appearance and posture;

[0064] (6) Freeze-drying: The rabbits were freeze-dried using a ZD-A3 freeze dryer. The rabbits were placed on a stainless steel tray and placed on the plate layer in the freeze dryer. They were pre-frozen at -45°C for 3 hours. The freeze dryer evaporation program was then adjusted to: -45 to -30°C, 24 hours; -30 to -25°C, 24 hours; -25 to -20°C, 24 hours; -20 to -15°C, 24 hours; -15 to -10°C, 24 hours; -10 to -5°C, 10 hours; -5 to 0°C, 10 hours ; 0-5°C, 5 hours; 5-10°C, 5 hours; 10-15°C, 5 hours; 15-20°C, 5 hours; 20-25°C, 5 hours; 25-30°C, 5 hours; 30-35°C, 5 hours; 35-40°C, 5 hours; 40-45°C, 5 hours; 45-50°C, 5 hours. During the whole process, the water trap temperature was maintained at about -60°C, and the vacuum degree was maintained at 8pa until the whole program was automatically shut down after the operation. The moisture content of the freeze-dried rabbit was 3%;

[0065] (7) Embedding: Evenly mix epoxy resin main glue and acid anhydride in a weight ratio of 3:1, vacuum evacuate to obtain a mixed solution, add the mixed solution to a depth of 2 mm in a square transparent acrylic mold, and when the mixed solution begins to solidify, gently place the freeze-dried rabbit on the surface of the colloid, and the rabbit will sink lightly into the colloid. After curing for 6 hours, the colloid becomes a transparent solid, and the position of the rabbit is also fixed. Continue to add the mixed solution until the whole body of the rabbit is covered, put it into a vacuum machine to remove the bubbles attached to the rabbit, and cure it at room temperature for 12 hours to obtain a completely transparent square rabbit embedded specimen crystal; the main glue is made of the following raw materials in weight percentage: epoxy resin NPEL128 80%, o-cresol glycidyl ether 10.9%, nonylphenol 8%, ultraviolet absorber UV-196 0.1%, antioxidant V73-P 1%;

[0066] (8) Grinding off burrs and polishing to obtain a rabbit embedded specimen, which retains the original color and morphology of the rabbit (fluffy and natural fur). The morphology of the rabbit after drying is the same as that of a fresh rabbit. The embedded rabbit specimen is placed outdoors for aging for 2 months. The color of the rabbit hair does not fade significantly, and the specimen crystal does not turn yellow significantly. It is placed indoors for 6 months, and the color of the rabbit hair does not fade, and the specimen crystal does not turn yellow significantly.

[0067] Example 5

[0068] (1) The rabbit was killed, and a 5 cm incision was made along the abdomen to remove the internal organs of the chest and abdomen. At the same time, the rabbit was bled by cutting the aorta and rinsed with clean water to obtain an empty-stomach rabbit;

[0069] (2) 10 minutes after the organ is removed, dip a cotton ball in the pretreatment solution and evenly apply it to the chest and abdominal surfaces of the fasting rabbit. Use 4 ml of the pretreatment solution per kilogram of the fasting rabbit. The pretreatment solution is made of the following raw materials in weight percentage: 0.5% benzoic acid, 4% paraben complex ester, 4% potassium sorbate, and 91.5% ethanol solution with a volume concentration of 70%;

[0070] (3) applying a fur treatment liquid in an amount of 2.2 times the weight of the fasting rabbit on the fur of the fasting rabbit, rubbing the fur, and then washing it with a large amount of clean water, and draining the water; the fur treatment liquid is made of the following raw materials in weight percentage: 12.5% ​​anhydrous ethanol, 8.9% sodium laureth sulfate, 0.92% ammonia water, and 77.68% purified water;

[0071] (4) Filling the rabbit's chest and abdominal cavities with PP cotton, suturing the abdominal incision, and replacing the rabbit's eyeball with an artificial eye;

[0072] (5) Plastic surgery: Use EVA board and bamboo sticks to fix the rabbit's appearance and posture;

[0073] (6) Freeze-drying: The rabbits were freeze-dried using a ZD-A3 freeze dryer. The rabbits were placed on a stainless steel tray and placed on the plate layer in the freeze dryer. They were pre-frozen at -45°C for 3 hours. The freeze dryer evaporation program was then adjusted to: -45 to -30°C, 24 hours; -30 to -25°C, 24 hours; -25 to -20°C, 24 hours; -20 to -15°C, 24 hours; -15 to -10°C, 24 hours; -10 to -5°C, 10 hours; -5 to 0°C, 10 hours ; 0-5°C, 5 hours; 5-10°C, 5 hours; 10-15°C, 5 hours; 15-20°C, 5 hours; 20-25°C, 5 hours; 25-30°C, 5 hours; 30-35°C, 5 hours; 35-40°C, 5 hours; 40-45°C, 5 hours; 45-50°C, 5 hours. During the whole process, the water trap temperature was maintained at about -60°C, and the vacuum degree was maintained at 8pa until the whole program was automatically shut down after the operation. The moisture content of the freeze-dried rabbit was 3%;

[0074] (7) The embedding process adopts MMA embedding process, which includes the following steps:

[0075] (a) Synthesis of PMMA prepolymer: 85 wt.% of methyl methacrylate, 4.95 wt.% of methacrylic acid, 10 wt.% of methacrylic acid functional monomer and 0.05 wt.% of azobisisobutyronitrile were mixed, reacted at a reaction temperature of 50° C. for 8 hours, and cooled to room temperature to obtain a PMMA prepolymer with a viscosity of 50 cps at 25° C.;

[0076] (b) adding 0.3% of azobisisobutyronitrile by weight of the PMMA prepolymer to the PMMA prepolymer, mixing to obtain a mixture, pouring the mixture into a mold, maintaining it at 55° C. for 11.5 hours, then putting the freeze-dried rabbit into it, adding the mixture again until the whole body of the rabbit is covered, and finally maintaining it at 55° C. for 11.5 hours;

[0077] (8) Grinding off burrs and polishing to obtain a rabbit embedded specimen, which retains the original color and morphology of the rabbit (fluffy and natural fur). The morphology of the rabbit after drying is the same as that of a fresh rabbit. The embedded rabbit specimen is placed outdoors for aging for 2 months. The color of the rabbit hair does not fade significantly, and the specimen crystal does not turn yellow significantly. It is placed indoors for 6 months, and the color of the rabbit hair does not fade, and the specimen crystal does not turn yellow significantly.

[0078] Example 6

[0079] (1) The rabbit was killed, and a 5 cm incision was made along the abdomen to remove the internal organs of the chest and abdomen. At the same time, the rabbit was bled by cutting the aorta and rinsed with clean water to obtain an empty-stomach rabbit;

[0080] (2) After removing the organs, immediately dip a cotton ball in the pretreatment solution and evenly apply it to the chest and abdominal surfaces of the fasting rabbit. Use 3 ml of the pretreatment solution per kilogram of the fasting rabbit. The pretreatment solution is made of the following raw materials in weight percentage: 2% benzoic acid, 6% paraben complex ester, 1% potassium sorbate, and 91% ethanol solution with a volume concentration of 70%;

[0081] (3) applying a fur treatment liquid in an amount 2.2 times the weight of the fasting rabbit on the fur of the fasting rabbit, rubbing the fur, and then washing it with a large amount of clean water, and draining the water; the fur treatment liquid is made of the following raw materials in weight percentage: 12.2% anhydrous ethanol, 9.8% sodium laureth sulfate, 0.78% ammonia water, and 77.22% purified water;

[0082] (4) Filling the rabbit's chest and abdominal cavities with PP cotton, suturing the abdominal incision, and replacing the rabbit's eyeball with an artificial eye;

[0083] (5) Plastic surgery: Use EVA board and bamboo sticks to fix the rabbit's appearance and posture;

[0084] (6) Freeze-drying: The rabbits were freeze-dried using a ZD-A3 freeze dryer. The rabbits were placed on a stainless steel tray and placed on the plate layer in the freeze dryer. They were pre-frozen at -45°C for 3 hours. The freeze dryer evaporation program was then adjusted to: -45 to -30°C, 24 hours; -30 to -25°C, 24 hours; -25 to -20°C, 24 hours; -20 to -15°C, 24 hours; -15 to -10°C, 24 hours; -10 to -5°C, 10 hours; -5 to 0°C, 10 hours ; 0-5°C, 5 hours; 5-10°C, 5 hours; 10-15°C, 5 hours; 15-20°C, 5 hours; 20-25°C, 5 hours; 25-30°C, 5 hours; 30-35°C, 5 hours; 35-40°C, 5 hours; 40-45°C, 5 hours; 45-50°C, 5 hours. During the whole process, the water trap temperature was maintained at about -60°C, and the vacuum degree was maintained at 8pa until the whole program was automatically shut down after the operation. The moisture content of the freeze-dried rabbit was 3%;

[0085] (7) The embedding process adopts MMA embedding process, which includes the following steps:

[0086] (a) Synthesis of PMMA prepolymer: 95 wt.% of methyl methacrylate, 0.5 wt.% of methacrylic acid, 4 wt.% of methacrylic acid functional monomer and 0.5 wt.% of azobisisobutyronitrile were mixed, reacted at a reaction temperature of 80° C. for 5 hours, and cooled to room temperature to obtain a PMMA prepolymer with a viscosity of 2000 cps at 25° C.;

[0087] (b) adding 0.4% of azobisisobutyronitrile by weight of the PMMA prepolymer to the PMMA prepolymer, mixing to obtain a mixture, pouring the mixture into a mold, keeping it at 50° C. for 12 hours, then putting the freeze-dried rabbit into it, adding the mixture again until the whole body of the rabbit is covered, and finally keeping it at 50° C. for 12 hours;

[0088] (8) Grinding off burrs and polishing to obtain a rabbit embedded specimen, which retains the original color and morphology of the rabbit (fluffy and natural fur). The morphology of the rabbit after drying is the same as that of a fresh rabbit. The embedded rabbit specimen is placed outdoors for aging for 2 months. The color of the rabbit hair does not fade significantly, and the specimen crystal does not turn yellow significantly. It is placed indoors for 6 months, and the color of the rabbit hair does not fade, and the specimen crystal does not turn yellow significantly.

[0089] Example 7

[0090] (1) The rabbit was killed, and a 5 cm incision was made along the abdomen to remove the internal organs of the chest and abdomen. At the same time, the rabbit was bled by cutting the aorta and rinsed with clean water to obtain an empty-stomach rabbit;

[0091] (2) After removing the organs, immediately dip a cotton ball in the pretreatment solution and evenly apply it to the chest and abdominal surfaces of the fasting rabbit. Use 3 ml of the pretreatment solution per kilogram of the fasting rabbit. The pretreatment solution is made of the following raw materials in weight percentage: 1.5% benzoic acid, 3.3% paraben complex ester, 2.1% potassium sorbate, and 93.1% ethanol solution with a volume concentration of 70%;

[0092] (3) applying a fur treatment liquid of 2.2 times the weight of the fasting rabbit on the fur of the fasting rabbit, rubbing the fur, and then washing it with a large amount of clean water, and draining the water; the fur treatment liquid is made of the following raw materials in weight percentage: 12.8% anhydrous ethanol, 9.4% sodium laureth sulfate, 0.85% ammonia water, and 76.95% purified water;

[0093] (4) Filling the rabbit's chest and abdominal cavities with PP cotton, suturing the abdominal incision, and replacing the rabbit's eyeball with an artificial eye;

[0094] (5) Plastic surgery: Use EVA board and bamboo sticks to fix the rabbit's appearance and posture;

[0095] (6) Freeze-drying: The rabbits were freeze-dried using a ZD-A3 freeze dryer. The rabbits were placed on a stainless steel tray and placed on the plate layer in the freeze dryer. They were pre-frozen at -45°C for 3 hours. The freeze dryer evaporation program was then adjusted to: -45 to -30°C, 24 hours; -30 to -25°C, 24 hours; -25 to -20°C, 24 hours; -20 to -15°C, 24 hours; -15 to -10°C, 24 hours; -10 to -5°C, 10 hours; -5 to 0°C, 10 hours ; 0-5°C, 5 hours; 5-10°C, 5 hours; 10-15°C, 5 hours; 15-20°C, 5 hours; 20-25°C, 5 hours; 25-30°C, 5 hours; 30-35°C, 5 hours; 35-40°C, 5 hours; 40-45°C, 5 hours; 45-50°C, 5 hours. During the whole process, the water trap temperature was maintained at about -60°C, and the vacuum degree was maintained at 8pa until the whole program was automatically shut down after the operation. The moisture content of the freeze-dried rabbit was 3%;

[0096] (7) The embedding process adopts MMA embedding process, which includes the following steps:

[0097] (a) Synthesis of PMMA prepolymer: 87 wt.% of methyl methacrylate, 5 wt.% of methacrylic acid, 7 wt.% of methacrylic acid functional monomer and 1 wt.% of azobisisobutyronitrile were mixed, reacted at a reaction temperature of 100° C. for 1 hour, and cooled to room temperature to obtain a PMMA prepolymer with a viscosity of 5000 cps at 25° C.;

[0098] (b) adding 0.6% of azobisisobutyronitrile by weight of the PMMA prepolymer to the PMMA prepolymer, mixing to obtain a mixture, pouring the mixture into a mold, keeping it at 45° C. for 12.5 hours, then putting the freeze-dried rabbit into it, adding the mixture again until the whole body of the rabbit is covered, and finally keeping it at 45° C. for 12.5 hours;

[0099] (8) Grinding off burrs and polishing to obtain a rabbit embedded specimen, which retains the original color and morphology of the rabbit (fluffy and natural fur). The morphology of the rabbit after drying is the same as that of a fresh rabbit. The embedded rabbit specimen is placed outdoors for aging for 2 months. The color of the rabbit hair does not fade significantly, and the specimen crystal does not turn yellow significantly. It is placed indoors for 6 months, and the color of the rabbit hair does not fade, and the specimen crystal does not turn yellow significantly.

[0100] Example 8

[0101] (1) The mice were killed, a 3 cm incision was made along the abdomen, and the visceral organs of the chest and abdomen were removed. At the same time, the aorta was cut open to bleed the mice, and the mice were rinsed with clean water to obtain fasting mice;

[0102] (2) 10 minutes after the organ is removed, dip a cotton ball in the pretreatment solution and evenly apply it to the chest and abdominal surfaces of the fasting mice. Use 3 ml of the pretreatment solution per kilogram of fasting mice. The pretreatment solution is made of the following raw materials in weight percentage: 0.8% benzoic acid, 2% paraben complex ester, 3.4% potassium sorbate, and 93.8% ethanol solution with a volume concentration of 70%;

[0103] (3) applying a fur treatment liquid twice the weight of the fasting mouse on the fur of the fasting mouse, rubbing the fur, and then washing it with a large amount of clean water, and draining the water; the fur treatment liquid is made of the following raw materials in weight percentage: 12.8% anhydrous ethanol, 9.4% sodium laureth sulfate, 0.85% ammonia water, and 76.95% purified water;

[0104] (4) Fill the chest and abdominal cavities of mice with PP cotton and suture the abdominal incision;

[0105] (5) Plastic surgery: Use EVA boards and bamboo sticks to fix the appearance and posture of the mice;

[0106] (6) Freeze-drying: The mice were freeze-dried using a ZD-A3 freeze dryer. The mice were placed on a stainless steel tray and placed on the plate layer in the freeze dryer. They were pre-frozen at -45°C for 3 hours. The freeze dryer evaporation program was then adjusted to: -45 to -30°C, 24 hours; -30 to -25°C, 24 hours; -25 to -20°C, 24 hours; -20 to -15°C, 24 hours; -15 to -10°C, 24 hours; -10 to -5°C, 10 hours; -5 to 0°C, 10 hours ; 0-5°C, 5 hours; 5-10°C, 5 hours; 10-15°C, 5 hours; 15-20°C, 5 hours; 20-25°C, 5 hours; 25-30°C, 5 hours; 30-35°C, 5 hours; 35-40°C, 5 hours; 40-45°C, 5 hours; 45-50°C, 5 hours. During the whole process, the water storage chamber temperature was maintained at about -60°C, and the vacuum degree was maintained at 8pa until the whole program was automatically shut down after the operation. The moisture content of the freeze-dried mice obtained was 3%;

[0107] (7) Embedding: Evenly mix epoxy resin main glue and acid anhydride in a weight ratio of 3:1, vacuum evacuate to obtain a mixed solution, add the mixed solution to a depth of 2 mm in a square transparent acrylic mold, and when the mixed solution begins to solidify, gently place a freeze-dried mouse on the surface of the colloid, and the mouse will sink lightly into the colloid. After curing for 6 hours, the colloid becomes a transparent solid, and the mouse is also fixed in position. Continue to add the mixed solution until the whole body of the mouse is covered, put it into a vacuum machine to remove the bubbles attached to the mouse, and cure it at room temperature for 12 hours to obtain a completely transparent square mouse embedded specimen crystal; the main glue is made of the following raw materials in weight percentage: epoxy resin NPEL1288 6.5%, butyl glycidyl ether 7.5%, nonylphenol 5%, ultraviolet absorber UV-196 0.5%, antioxidant V73-P 0.5%;

[0108] (8) Grinding off burrs and polishing to obtain a mouse embedded specimen, which retains the original color and shape of the mouse (fluffy and natural hair). The shape of the mouse after drying is the same as that of a fresh mouse. The embedded mouse specimen is placed outdoors for aging for 2 months. The color of the mouse hair does not fade significantly, and the specimen crystal does not turn yellow significantly. It is placed indoors for 6 months, and the color of the mouse hair does not fade, and the specimen crystal does not turn yellow significantly.

[0109] Comparative Example 1

[0110] The difference from Example 1 is that the pretreatment solution is made of the following raw materials in weight percentage: 3% benzoic acid, 1% paraben complex ester, 5% potassium sorbate, and 91% ethanol solution with a volume concentration of 70%. (The proportion is not within the scope of the present invention) The rest is the same as Example 1.

[0111] The obtained rabbit embedded specimens retained the original color and morphology of the rabbit, but the shape of the rabbit after drying was slightly stiff and unnatural. The embedded rabbit specimens were placed outdoors for aging for 2 months, and the color did not fade significantly, and the crystals did not turn yellow significantly; but after being placed in an indoor environment for 6 months, the color of the rabbit hair darkened and turned slightly yellow, but the crystals did not turn yellow.

[0112] Comparative Example 2

[0113] The difference from Example 1 is that the pretreatment solution is made of the following raw materials in weight percentage: 2% benzoic acid, 4% potassium sorbate, and 94% ethanol solution with a volume concentration of 70%. (The paraben complex ester is missing) The rest is the same as Example 1.

[0114] The obtained rabbit embedded specimens retained the original color and morphology of the rabbit, but the shape of the rabbit was stiff after drying. The embedded rabbit specimens were placed outdoors for aging for 2 months, and the color of the rabbit hair faded significantly, but the crystals did not turn yellow significantly; but after being placed in an indoor environment for 2 months, the color of the rabbit hair darkened and turned slightly yellow, but the crystals did not turn yellow.

[0115] Comparative Example 3

[0116] The difference from Example 1 is that the paraben complex ester in the pretreatment solution is replaced with sodium lactate, and the rest is the same as Example 1. The prepared rabbit embedded specimen has a stiff and unnatural shape after drying.

[0117] Comparative Example 4

[0118] The difference from Example 1 is that the fur treatment liquid is made of the following raw materials in weight percentage: 8.8% anhydrous ethanol, 9.4% sodium lauryl polyether sulfate, 0.85% ammonia water, and 80.95% purified water. (The content of anhydrous ethanol is reduced) The rest is the same as Example 1. The rabbit hair in the obtained rabbit embedded specimen is closer to the skin and has a weak fluffy feeling.

[0119] Comparative Example 5

[0120] The difference from Example 1 is that the fur treatment solution is made of the following raw materials in weight percentage: 12.8% anhydrous ethanol, 6.4% sodium lauryl polyether sulfate, 0.85% ammonia water, and 79.95% purified water. (The surfactant content is reduced) The rest is the same as Example 1. The rabbit hair in the obtained rabbit embedded specimen has adhesion, uneven distribution, and looks stiff as a whole.

[0121] Comparative Example 6

[0122] The difference from Example 1 is that the fur treatment solution is made of the following raw materials in weight percentage: 12.8% anhydrous ethanol, 9.4% sodium laureth sulfate, 2.85% ammonia water, and 74.95% purified water. (The ammonia water content is increased) The rest is the same as Example 1. The rabbit hair in the obtained rabbit embedded specimen looks stiff and unnatural.

[0123] Comparative Example 7

[0124] The difference from Example 1 is that the sodium laureth sulfate in the fur treatment solution is replaced with sodium dodecylbenzene sulfonate. The rest is the same as Example 1. The rabbit hair in the obtained rabbit embedded specimen looks not very glossy, slightly stiff, and relatively close to the skin.

[0125] Comparative Example 8

[0126] The difference from Example 1 is that 8 ml of pretreatment liquid is used for every kilogram of fasting hairy mammal, and the rest is the same as Example 1. During plastic surgery, the rabbit is relatively stiff as a whole and is not easy to perform plastic surgery. The final prepared rabbit embedded specimen is stiff and unnatural after drying.

[0127] Comparative Example 9

[0128] The difference from Example 1 is that in step (3), a fur treatment liquid 3 times the weight of the fasting hairy mammal is applied to the fur of the fasting hairy mammal. In the subsequent preparation, the rabbit has a serious hair breakage problem.

[0129] Comparative Example 10

[0130] The difference from Example 1 is that in step (3), a fur treatment liquid of 1 times the weight of the fasting hairy mammal is applied to the fur of the fasting hairy mammal, and when resin is subsequently added for embedding, the rabbit hair becomes tangled or even lumps.

[0131] The above description is a detailed description of the preferred feasible embodiments of the present invention, but the embodiments are not intended to limit the scope of the patent application of the present invention. All equivalent changes or modified changes completed under the technical spirit suggested by the present invention should fall within the patent scope covered by the present invention.

Claims

1. A method for preparing an embedded specimen, characterized in that: The following steps are involved: (1) killing a hairy mammal, cutting it open along the abdomen, removing its visceral organs from the chest and abdomen, and obtaining an empty-stomach hairy mammal; (2) applying a pretreatment solution to the abdominal cavity and chest cavity of the fasting hairy mammal, using 1-4 ml of the pretreatment solution per kilogram of the fasting hairy mammal; the pretreatment solution is a mixture of benzoic acid, paraben, potassium sorbate and cosolvent A; (3) applying a fur treatment liquid in an amount of 1.8 to 2.2 times the weight of the fasting hairy mammal on the fur of the fasting hairy mammal; the fur treatment liquid is a mixture of anhydrous ethanol, a surfactant, ammonia water and a cosolvent B, and the surfactant is one of sodium laureth sulfate, sodium lauryl sulfate and sodium laureth-3 acetate; (4) filling the chest and abdominal cavities of an empty-bellied hairy mammal, suturing the abdominal incision, shaping, freeze-drying, embedding, grinding, and polishing to obtain an embedded specimen; In the step (2), the pretreatment liquid is made of the following raw materials in weight percentage: 0.5-2% benzoic acid, 2-6% paraben complex ester, 1-4% potassium sorbate, and the co-solvent A is added to 100%; In the step (3), the fur treatment liquid is made of the following raw materials in weight percentage: 12.2-12.8% anhydrous ethanol, 8.9-9.8% surfactant, 0.78-0.92% ammonia water, and co-solvent B is added to 100%.

2. The method for preparing an embedded specimen according to claim 1, characterized in that: The hairy mammal is a rabbit or a mouse.

3. The method for preparing an embedded specimen according to claim 1, characterized in that: The co-solvent A is an ethanol solution with a volume concentration of 70%, and the co-solvent B is pure water.

4. The method for preparing an embedded specimen according to claim 1, characterized in that: The pretreatment liquid is applied within 0-10 minutes after the internal organs of the chest and abdomen of the furry mammal are removed, and the fur treatment liquid is then applied to the fur 10-15 minutes after the pretreatment liquid is applied.

5. The method for preparing an embedded specimen according to claim 1, characterized in that: In the step (4), the specific steps of embedding are: mixing the main glue and the curing agent in a weight ratio of 3:1 to obtain a mixed solution; adding the mixed solution to the mold, and when the mixed solution begins to solidify, putting the freeze-dried and shaped hairy mammal into it, and after the mixed solution is completely solidified, adding the mixed solution again until the entire body of the hairy mammal is covered and solidified.

6. The method for preparing an embedded specimen according to claim 5, characterized in that: The main glue is made of the following raw materials in weight percentage: 80-95% epoxy resin, 1-12% active diluent, 0.1-8% accelerator, 0.1-1% ultraviolet absorber, and 0.1-1% antioxidant; the curing agent is at least one of polyether amine, isophorone diamine, fatty amine, and acid anhydride.

7. The method for preparing an embedded specimen according to claim 6, characterized in that: The active diluent is at least one of 1,4-butanediol diglycidyl ether, C12-C14 aliphatic glycidyl ether, butyl glycidyl ether, and o-cresol glycidyl ether; the accelerator is at least one of nonylphenol or dimethylimidazole.

8. The method for preparing an embedded specimen according to claim 1, characterized in that: In the step (4), the embedding adopts the MMA embedding process, which includes the following steps: (1) Synthesis of PMMA prepolymer: 85-95 wt.% of methyl methacrylate, 0.5-5 wt.% of methacrylic acid, 4-10 wt.% of methacrylic acid functional monomer and 0.05-1 wt.% of initiator are mixed, reacted at a reaction temperature of 50-100° C. for 1-8 hours, and cooled to room temperature to obtain a PMMA prepolymer having a viscosity of 50-5000 cps at 25° C.; (2) adding 0.3-0.6% of the weight of the PMMA prepolymer initiator to the PMMA prepolymer, mixing to obtain a mixture, pouring the mixture into a mold, maintaining it at 45-55° C. for 11.5-12.5 hours, then putting the freeze-dried and shaped hairy mammal into it, adding the mixture again until the entire body of the hairy mammal is covered, and finally maintaining it at 45-55° C. for 11.5-12.5 hours.