Cathode plate and preparation method thereof, battery and electric device

By adjusting the content of conductive agent and binder on the cathode plate to form a zebra structure, the problem of lithium deposition caused by uneven polarization of the battery core is solved, and the cycle life and safety of the battery are improved.

CN115842102BActive Publication Date: 2024-10-18CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202211451951.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-18
Publication Date
2024-10-18
Estimated Expiration
2042-11-18

AI Technical Summary

Technical Problem

During the cycle process of the battery cell, uneven temperature and expansion force lead to uneven polarization distribution of the pole pieces, resulting in lithium precipitation, which affects battery performance and safety.

Method used

Design a cathode plate whose diaphragm or active material layer is provided with different areas. The diaphragm resistance is controlled by adjusting the content of conductive agent and binder to form a zebra structure to offset uneven polarization and avoid lithium precipitation.

Benefits of technology

The uniform distribution of pole piece polarization is achieved, extending the cycle life of the battery, reducing costs, and avoiding the catastrophic consequences of lithium precipitation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115842102B_ABST
    Figure CN115842102B_ABST
Patent Text Reader

Abstract

The present invention discloses a cathode pole piece and a preparation method thereof, a battery and an electrical device, and belongs to the field of batteries. The cathode pole piece includes a current collector and a diaphragm arranged on the surface of the current collector, and the diaphragm is provided with at least two regions, wherein the two regions are defined as a first region and a second region, and the diaphragm resistance of the first region is greater than the diaphragm resistance of the second region. The present invention adjusts the relationship between the size of the diaphragm resistance in different regions on the cathode pole piece so that the pole piece itself is polarized unevenly, thereby offsetting the influence of the uneven polarization of the pole piece caused by the uneven temperature and expansion force during the cycle of the battery cell, making the polarization of the cathode pole piece of the present invention more uniform, and avoiding the phenomenon of lithium precipitation. The battery including the cathode pole piece of the present invention can effectively solve the lithium precipitation phenomenon caused by the uneven polarization of the pole piece, and has a higher cycle life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of batteries, and in particular to a cathode electrode sheet and a preparation method thereof, a battery and an electrical device. Background Art

[0002] During the cycle of the battery cell, the polarization distribution of the pole piece is prone to unevenness. When the cations move to the cathode and a reduction reaction occurs at the cathode, lithium deposition is prone to occur on the pole piece due to the uneven polarization distribution. Lithium deposition not only reduces battery performance and significantly shortens cycle life, but also limits the fast charging capacity of the battery and may cause catastrophic consequences such as combustion and explosion. Summary of the invention

[0003] The main purpose of the present invention is to provide a cathode electrode and a preparation method thereof, a battery and an electrical device, aiming to solve the technical problem that during the cycle of the battery cell, the polarization distribution of the electrode is uneven due to the influence of temperature and expansion force, resulting in lithium deposition.

[0004] To achieve the above object, the present invention provides a cathode electrode sheet, the cathode electrode sheet comprising a current collector and a membrane sheet disposed on the surface of the current collector;

[0005] The diaphragm is provided with at least two regions, wherein the two regions are defined as a first region and a second region, and the diaphragm resistance of the first region is greater than the diaphragm resistance of the second region.

[0006] In one embodiment of the present application, the conductive agent content of the first region is less than that of the second region, and the adhesive content of the first region is greater than that of the second region, so as to control the diaphragm resistance of the first region to be greater than that of the second region.

[0007] In one embodiment of the present application, the width of the first region accounts for more than one fifth of the width of the diaphragm, which can better adjust the polarization effect of the corresponding region.

[0008] In one embodiment of the present application, the membrane is an active material layer. The present invention controls different regions in the active material layer to have unequal membrane resistance to solve the problem of lithium deposition caused by uneven polarization of the pole piece due to external stress. No additional lithium material is needed to prepare a lithium deposition inhibition layer, the energy density of the battery will not be weakened, and the cost is low and the process is simple.

[0009] In one embodiment of the present application, the first region is located in the center of the active material layer, and the second region is located in the edge regions on both sides of the center. The active material layer presents a zebra structure as a whole, because the membrane resistance of the first region is larger, its own polarization is larger, and the membrane resistance of the second region is smaller, its own polarization is smaller, which can offset the uneven polarization of the electrode caused by the high temperature and small expansion force in the center of the battery cell during the battery cell cycle, resulting in smaller polarization in the center of the electrode, and the lower temperature and large expansion force of the head and tail on both sides of the center of the battery cell, resulting in larger polarization in the edge regions on both sides of the center of the electrode, thereby making the cathode electrode of the present invention more evenly polarized and avoiding the phenomenon of lithium precipitation in the middle of the electrode.

[0010] In one embodiment of the present application, the thickness of the active material layer is less than or equal to 250 mm. The active material layer within the above thickness range has better conductivity.

[0011] In one embodiment of the present application, the membrane is a bottom coating. The present invention controls different regions in the bottom coating to have unequal membrane resistance to solve the problem of lithium deposition caused by uneven polarization of the pole piece due to external stress, without the need to add additional lithium material to prepare a lithium deposition inhibition layer, and will not weaken the energy density of the battery. It is also low in cost and simple in process.

[0012] In one embodiment of the present application, the first area is located in the central area of ​​the bottom coating, and the second area is located in the edge areas on both sides of the central area. The bottom coating presents a zebra structure as a whole, the membrane resistance of the first area is larger, and its own polarization is larger, and the membrane resistance of the second area is smaller, and its own polarization is smaller, which can offset the influence of uneven polarization of the pole piece caused by the poor heat dissipation, high temperature, and small expansion force in the central area of ​​the battery cell during the battery cell cycle, resulting in smaller polarization in the central area of ​​the pole piece, and good heat dissipation, low temperature, and large expansion force in the head and tail on both sides of the central area of ​​the battery cell, resulting in larger polarization in the edge areas on both sides of the central area of ​​the pole piece, thereby making the cathode pole piece of the present invention more evenly polarized and avoiding the phenomenon of lithium precipitation in the middle of the pole piece.

[0013] In one embodiment of the present application, the thickness of the base coating layer is less than or equal to 40 μm. The base coating layer should not be too thick. Within the above thickness range, it can exert good adhesion and offset the influence of uneven polarization of the pole piece caused by the above external factors without affecting the electronic contact between the active material and the current collector.

[0014] In one embodiment of the present application, the membrane includes a primer layer and an active material layer, the primer layer is disposed on a surface of the current collector, and the active material layer is disposed on a surface of the primer layer facing away from the current collector.

[0015] In one embodiment of the present application, the active material layer is provided with at least two regions, wherein the two regions are defined as a first region of the active material layer and a second region of the active material layer, and the diaphragm resistance of the first region of the active material layer is greater than the diaphragm resistance of the second region of the active material layer;

[0016] And / or, the base coating layer has at least two regions, the two regions are defined as a first base coating layer region and a second base coating layer region, and the film resistance of the first base coating layer region is greater than the film resistance of the second base coating layer region.

[0017] The present invention can improve the problem of uneven polarization of the electrode by adjusting the bottom coating layer or the active material layer or even jointly adjusting the relationship between the membrane resistance of different areas in the bottom coating layer and the active material layer to avoid lithium precipitation. The schemes are diverse and more conducive to production and preparation.

[0018] In one embodiment of the present application, the conductive agent content of the first region of the active material layer is less than the conductive agent content of the second region of the active material layer, and the binder content of the first region of the active material layer is greater than the binder content of the second region of the active material layer;

[0019] And / or, the conductive agent content of the first region of the primer layer is less than that of the second region of the primer layer, and the binder content of the first region of the primer layer is greater than that of the second region of the primer layer.

[0020] The present invention controls the membrane resistance in different areas by adjusting the relationship between the binder and the conductive agent content in the active material layer and / or the base coating layer. The polarization size of the electrode itself can be adjusted without adding other functional materials to overcome the influence of lithium plating caused by uneven polarization of the electrode caused by external force.

[0021] In one embodiment of the present application, the conductive agent includes at least one of conductive carbon black, conductive graphite, conductive ink, Ketjen black, carbon nanotubes, and conductive carbon fibers. The use of the above types of conductive agents is more conducive to improving the rate and cycle rate of the battery, reducing internal resistance, and increasing capacity.

[0022] In one embodiment of the present application, the binder includes at least one of polyvinylidene fluoride, polyvinyl alcohol, polytetrafluoroethylene and sodium carboxymethyl cellulose. The above types of binders have uniform substitution degree and stable viscosity, can provide stable viscosity and adhesion, enhance the electronic contact between the active material and the conductive agent and between the active material and the current collector, and better stabilize the structure of the pole piece.

[0023] To achieve the above object, the present invention also provides a method for preparing a cathode electrode sheet, comprising the following steps:

[0024] The first coating is applied on a portion of the surface of the current collector to form a first region of the diaphragm, and the second coating is applied on another portion of the surface of the current collector to form a second region of the diaphragm, to prepare the cathode electrode sheet, wherein the diaphragm resistance of the first region is greater than the diaphragm resistance of the second region.

[0025] In one embodiment of the present application, a conductive agent and a binder are uniformly mixed to obtain a first coating, and a conductive agent and a binder are uniformly mixed to obtain a second coating; the content of the conductive agent in the first coating is less than the content of the conductive agent in the second coating, and the content of the binder in the first coating is greater than the content of the binder in the second coating. By controlling the content relationship between the conductive agent and the binder to control the size of the resistance in the diaphragm, there is no need to add other functional materials, which can reduce production costs.

[0026] In one embodiment of the present application, the conductive agent and the binder are dissolved in an organic solvent and mixed evenly to obtain the first coating and / or the second coating. The organic solvent can dissolve and disperse the conductive agent and the binder to obtain a uniform coating, which is conducive to obtaining a uniform film.

[0027] In one embodiment of the present application, the first coating and / or the second coating further contain active materials. When the coating contains active materials, it can be used to prepare an active material layer, and combined with adjusting the content of the binder and the conductive agent, the active material layer can play a role in offsetting the influence of uneven polarization of the pole piece caused by external stress, thereby achieving the purpose of avoiding lithium precipitation.

[0028] In one embodiment of the present application, when the cathode electrode is used in a lithium-ion battery, the active material includes at least one of a lithium cobalt oxide compound, a nickel cobalt manganese oxide compound, a nickel cobalt aluminum oxide compound, a lithium iron phosphate compound, a lithium manganese oxide compound, a lithium iron phosphate manganese oxide compound, and a nickel manganese oxide compound. There are many types of active materials to choose from in the present invention, and various aspects such as stability, conductivity, specific capacity, and charge and discharge efficiency can be comprehensively considered to enable the battery of the present invention to have a wider range of applications. For example, using a lithium iron phosphate compound as an active material, the resulting battery has a relatively high charge and discharge efficiency and can be applied to power batteries.

[0029] In one embodiment of the present application, when the cathode electrode is applied to a sodium ion battery, the active material includes at least one of a Prussian blue material, a transition metal oxide, and a polyanion. The technical solution of the present invention can also solve the problem of uneven polarization of the cathode electrode in the sodium ion battery due to external stress.

[0030] In one embodiment of the present application, the preparation method further comprises the following steps: after coating the film on the surface of the current collector to form the film, drying and cold pressing to obtain the cathode electrode sheet. The cathode electrode sheet obtained by drying and cold pressing has a more stable structure, better electrochemical performance and longer life.

[0031] To achieve the above object, the present invention further provides a battery, the battery comprising the cathode electrode sheet as described above. The battery is any one of a battery cell, a battery module, and a battery pack. The battery using the cathode electrode sheet of the present invention also has the beneficial effects of improving the uneven polarization distribution of the electrode sheet and avoiding lithium precipitation, and has a higher cycle life.

[0032] In addition, the present invention also provides an electric device, the electric device comprising the battery as described above. The electric device of the present invention also has the beneficial effects of improving the uneven polarization distribution of the battery pole piece and avoiding lithium deposition, and has a longer service life.

[0033] The beneficial effects that can be achieved by the present invention are:

[0034] During the cycle of the battery cell, the overall temperature is uneven and the expansion forces vary. Affected by the above external factors, some areas of the electrode are prone to smaller polarization, some areas are larger polarization, and the overall polarization is uneven, which in turn causes lithium deposition on the electrode.

[0035] The present invention adjusts the relationship between the membrane resistances of different areas on the cathode electrode piece, so that the membrane resistance of the area on the cathode electrode piece with smaller polarization due to external factors is larger, and the polarization degree of the electrode piece is controlled to be larger; the membrane resistance of the area on the cathode electrode piece with larger polarization due to external factors is smaller, and the polarization degree of the electrode piece is controlled to be smaller; thereby, the polarization change caused by external stress can be offset, the polarization of the electrode piece can be made more uniform, and the phenomenon of lithium deposition on the electrode piece due to uneven polarization can be solved, especially the phenomenon of lithium deposition in the middle part of the electrode piece.

[0036] The technology of the present invention is simple, convenient and low-cost. It only needs to adjust the unequal membrane resistance of different areas in the cathode electrode to control the lithium precipitation phenomenon caused by the uneven polarization distribution of the electrode. There is no need to add additional lithium materials and prepare a lithium inhibition layer, which will not affect the battery energy density and increase the overall cost of the battery.

[0037] The battery using the cathode electrode of the present invention can also solve the above technical problems and have the same technical effects and a higher cycle life. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.

[0039] Figure 1 It is a schematic cross-sectional view of a cathode electrode piece of the present invention.

[0040] Figure 2 It is a schematic plan view of a diaphragm of a cathode electrode plate of the present invention.

[0041] Figure 3 A schematic cross-sectional view of an embodiment of a cathode electrode sheet having a primer layer and an active material layer according to the present invention;

[0042] Figure 4 A schematic cross-sectional view of another embodiment of a cathode electrode sheet having a primer layer and an active material layer according to the present invention;

[0043] Figure 5 The cross-sectional view of another embodiment of a cathode electrode sheet having a primer layer and an active material layer according to the present invention.

[0044] Among them, 1. current collector; 2. membrane; 21. first region; 22. second region; 3. base coating; 31. first region of base coating; 32. second region of base coating; 4. active material layer; 41. first region of active material layer; 42. second region of active material layer.

[0045] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0046] It should be understood that the specific embodiments described herein are only used to explain the present invention, and are not used to limit the present invention.

[0047] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0048] In the present invention, descriptions such as "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in the field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0049] During the cycle of the battery cell, the overall temperature is uneven and the expansion force varies. Affected by the above external factors, some areas of the electrode are prone to small polarization, some areas are large polarization, and the overall polarization is uneven, which in turn causes the problem of lithium deposition in the electrode, especially the problem of lithium deposition in the middle. For example, affected by heat dissipation, the area with poor heat dissipation in the battery cell has a high temperature, small expansion force, and small polarization of the electrode, while the area with good heat dissipation in the battery cell has a low temperature, large expansion force, and large polarization of the electrode. Affected by the above uneven polarization distribution, lithium ions will diffuse and embed lithium into the area with small polarization in the electrode, resulting in the amount of lithium embedded in the area with large polarization of the electrode being lower than the amount of lithium embedded in the area with small polarization.

[0050] In view of this, the present invention provides a cathode electrode sheet, which includes a current collector 1 and a membrane 2 arranged on the surface of the current collector 1.

[0051] Reference Figure 1 and Figure 2 , Figure 1 is a schematic diagram of the cross section of the cathode electrode. Figure 2 It is a schematic plan view of the diaphragm 2.

[0052] The diaphragm 2 is provided with at least two regions, which are defined as a first region 21 and a second region 22 . The diaphragm resistance of the first region 21 is greater than the diaphragm resistance of the second region 22 .

[0053] It is understandable that at least two regions include two, three, four or more regions. The first region 21 and the second region 22 are only two regions exemplified. Figure 1 and Figure 2 That is, there are three areas, at least two of which are set as described above.

[0054] During the cycle, the battery cell is affected by heat dissipation, and the overall temperature is uneven, and the expansion force varies. The polarization is small in the area with high temperature and small expansion force, and the polarization is large in the area with low temperature and large expansion force. Due to the uneven temperature and expansion force of the battery cell, the polarization distribution of the pole piece is uneven, resulting in lithium precipitation.

[0055] For example, during the cycle of the battery cell, the temperature in the middle of the height direction of the battery cell is high, the expansion force is small, and the corresponding polarization in the middle of the electrode is small. The head and bottom of the battery cell have good heat dissipation, low temperature, and large expansion force, and the corresponding polarization at the head and bottom of the electrode is large. Lithium ions tend to diffuse and embed lithium in the middle of the electrode, resulting in the amount of lithium embedded in the head and bottom of the electrode being lower than the amount in the middle.

[0056] Therefore, the present invention sets a diaphragm 2 on the current collector 1 of the cathode electrode, and adjusts the relationship between the size of the diaphragm resistance in different areas on the diaphragm 2, so that the resistance of the area on the cathode electrode with smaller polarization due to external factors is larger, and the polarization degree of itself is controlled to be larger; the resistance of the area with larger polarization due to external factors is smaller, and the polarization degree of itself is controlled to be smaller; thereby offsetting the polarization change caused by external stress, making the polarization of the electrode more uniform, and then solving the problem of lithium deposition on the electrode due to uneven polarization.

[0057] The present invention does not limit the method for making different regions of the diaphragm 2 have different resistances. In some embodiments, the conductive agent content of the first region 21 can be adjusted to be less than the conductive agent content of the second region 22, and the binder content of the first region 21 can be adjusted to be greater than the binder content of the second region 22, so that the diaphragm resistance of the first region 21 is greater than the diaphragm resistance of the second region 22. This method is simple and easy to operate, does not require the addition of additional functional materials, and has low cost. Of course, in other embodiments, the resistance can also be adjusted by adjusting other components of the diaphragm.

[0058] It can be understood that the content of the conductive agent and the content of the binder in the present invention refer to the weight of the conductive agent and the weight of the binder, respectively.

[0059] Specifically, the distribution of the conductive agent and the binder in the diaphragm satisfies the following relationship:

[0060] 0<eg<max(e,g);

[0061] 0<hf<max(h,f);

[0062] in;

[0063] e represents the content of the conductive agent in the second region 22 of the membrane 2;

[0064] g represents the content of the conductive agent in the first region 21 of the membrane 2;

[0065] h represents the content of the binder in the first region 21 of the membrane 2;

[0066] f represents the content of the binder in the second region 22 of the membrane 2 .

[0067] In addition, the width of the first region 21 of the diaphragm 2 accounts for more than one fifth of the width of the diaphragm 2, so as to better adjust the polarization effect of the corresponding region.

[0068] In some embodiments, the width of the first region 21 of the diaphragm 2 accounts for 1 / 5, 1 / 4, 1 / 3, 1 / 2 or 2 / 3 of the width of the diaphragm 2 .

[0069] The present invention does not limit the type of conductive agent, and can be selected from at least one of conductive carbon black, conductive graphite, conductive ink, Ketjen black, carbon nanotubes, and conductive carbon fibers. The present invention uses the above types of conductive agents, which is more conducive to improving the rate and cycle rate of the battery, reducing the internal resistance, and increasing the capacity.

[0070] The present invention does not limit the type of binder, and can be selected from at least one of polyvinylidene fluoride (PVDF), polyvinyl alcohol, polytetrafluoroethylene and sodium carboxymethyl cellulose. The above types of binders have uniform substitution degree and stable viscosity, can provide stable viscosity and adhesion, enhance the electronic contact between the active material and the conductive agent and between the active material and the current collector, and better stabilize the structure of the pole piece.

[0071] In some embodiments, membrane 2 is an active material layer.

[0072] Reference Figure 1 and Figure 2 The active material layer has a first region 21 located in the central region and a second region 22 located in the edge regions on both sides of the central region.

[0073] In this embodiment, the sheet resistance of the first region 21 of the active material layer is greater than the sheet resistance of the second region 22 .

[0074] In this embodiment, the diaphragm resistance of the first region 21 can be made greater than that of the second region 22 by adjusting the conductive agent content of the first region 21 to be less than that of the second region 22 and the binder content of the first region 21 to be greater than that of the second region 22 .

[0075] The diaphragm 2 presents a zebra structure as a whole, with the first region 21 having a larger polarization and the second region 22 having a smaller polarization. This can offset the uneven polarization of the electrode caused by the higher temperature and smaller expansion force in the center of the battery cell during the battery cell cycle, resulting in smaller polarization in the center of the electrode, and lower temperature and larger expansion force in the head and tail parts on both sides of the center of the battery cell, resulting in larger polarization in the edge areas on both sides of the center of the electrode. This makes the cathode electrode of the present invention more evenly polarized, avoiding the phenomenon of lithium deposition in the middle of the electrode.

[0076] In this embodiment, the active material layer includes but is not limited to a conductive agent and a binder, and also includes other materials well known to those skilled in the art such as active materials.

[0077] Furthermore, when the cathode electrode is used in a lithium-ion battery, the active material includes at least one of a lithium cobalt oxide compound, a nickel cobalt manganese oxide compound, a nickel cobalt aluminum oxide compound, a lithium iron phosphate compound, a lithium manganese oxide compound, a lithium iron phosphate manganese oxide compound, and a nickel manganese oxide compound.

[0078] The present invention does not limit the thickness of the active material layer. Optionally, the thickness of the active material layer is less than or equal to 250 mm. The active material layer within the above thickness range has better conductivity.

[0079] In other embodiments, the membrane 2 is a primer layer, which can enhance the bonding force between the current collector 1 and the active material layer 4 .

[0080] Reference Figure 3 and Figure 5 The primer layer 3 has a primer layer first region 31 located in the central area, and a primer layer second region 32 located in the edge areas on both sides of the central area.

[0081] In this embodiment, the sheet resistance of the first area 31 of the primer layer 3 is greater than the sheet resistance of the second area 32 of the primer layer.

[0082] In this embodiment, the diaphragm resistance of the first area 31 of the base coating can be made greater than the diaphragm resistance of the second area 32 of the base coating by adjusting the conductive agent content of the first area 31 of the base coating to be less than the conductive agent content of the second area 32 of the base coating and the binder content of the first area 31 of the base coating to be greater than the binder content of the second area 32 of the base coating.

[0083] The bottom coating 3 presents a zebra structure as a whole. The polarization of the first area 31 of the bottom coating itself is larger, and the polarization of the second area 32 of the bottom coating itself is smaller. This can offset the uneven polarization of the pole piece caused by the poor heat dissipation, high temperature and small expansion force in the center area of ​​the battery cell during the battery cell cycle, which leads to smaller polarization in the center area of ​​the pole piece, and good heat dissipation, low temperature and large expansion force in the head and tail on both sides of the center area of ​​the battery cell, which leads to larger polarization in the edge areas on both sides of the center area of ​​the pole piece. This makes the cathode pole piece of the present invention more evenly polarized and avoids the phenomenon of lithium precipitation in the middle of the pole piece.

[0084] In this embodiment, the base coating 3 includes but is not limited to a conductive agent and a binder, and may also include other additives known to those skilled in the art such as calcium hydroxide, which can enhance the deposition of the conductive agent and the binder on the current collector.

[0085] The present invention does not limit the thickness of the primer layer. Optionally, the thickness of the primer layer is less than or equal to 40 μm. The primer layer should not be too thick. Within the above thickness range, it can exert good adhesion and offset the influence of uneven polarization of the pole piece caused by the above external factors, while not affecting the electronic contact between the active material and the current collector.

[0086] The present invention does not limit the coating method of the base coating layer. In some embodiments, the base coating layer can be coated by gravure roller coating. The gravure roller coating method can obtain a smooth, stable and uniform base coating layer.

[0087] In some other embodiments, in combination with reference Figures 3 to 5 The membrane 2 includes a primer layer 3 and an active material layer 4. The primer layer 3 is disposed on the surface of the current collector 1, and the active material layer 4 is disposed on the surface of the primer layer 3 away from the current collector 1.

[0088] The active material layer 4 has at least two regions, which are defined as a first active material layer region 41 and a second active material layer region 42 . The sheet resistance of the first active material layer region 41 is greater than that of the second active material layer region 42 .

[0089] And / or, the base coating 3 has at least two regions, the two regions are defined as a base coating first region 31 and a base coating second region 32 , and the film resistance of the base coating first region 31 is greater than the film resistance of the base coating second region 32 .

[0090] In this embodiment, the diaphragm resistance of the first region 41 of the active material layer can be made greater than the diaphragm resistance of the second region 42 of the active material layer by adjusting the conductive agent content of the first region 41 of the active material layer to be less than the conductive agent content of the second region 42 of the active material layer and the binder content of the first region 41 of the active material layer to be greater than the binder content of the second region 42 of the active material layer.

[0091] Similarly, the diaphragm resistance of the first area 31 of the base coating can be made greater than the diaphragm resistance of the second area 32 of the base coating by adjusting the conductive agent content of the first area 31 of the base coating to be less than the conductive agent content of the second area 32 of the base coating and the binder content of the first area 31 of the base coating to be greater than the binder content of the second area 32 of the base coating.

[0092] The present invention has various ways to adjust the resistances of different regions in the cathode electrode sheet with unequal sizes. It can adjust the membrane resistance relationship in the active material layer or the bottom coating layer, and it can also adjust the membrane resistance relationship in the active material layer and the bottom coating layer at the same time. The above methods can solve the problem of lithium deposition due to uneven polarization of the electrode sheet of the present invention.

[0093] In one embodiment, referring to Figure 3 The base coating 3 has two regions, namely a base coating first region 31 and a base coating second region 32 . The sheet resistance of the base coating first region 31 of the base coating 3 is greater than the sheet resistance of the base coating second region 32 .

[0094] In this embodiment, the polarization of the first area 31 of the bottom coating itself is larger, which can offset the effect of the reduced polarization of a part of the electrode due to poor heat dissipation, high temperature and small expansion force of the battery cell during the cycle, making the polarization of the electrode more uniform and avoiding the occurrence of lithium deposition; the polarization of the second area 32 of the bottom coating itself is smaller, which can offset the effect of the increased polarization of a part of the electrode due to good heat dissipation, low temperature and large expansion force of the battery cell during the cycle, making the polarization of the electrode more uniform and avoiding the occurrence of lithium deposition.

[0095] In this embodiment, the undercoat layer 3 also plays a role in enhancing the bonding force between the active material layer 4 and the current collector 1 .

[0096] In this embodiment, the active material layer 4 itself is evenly polarized and does not have the function of offsetting the influence of uneven polarization of the pole pieces caused during the battery cell cycle process.

[0097] In one embodiment, referring to Figure 4 The active material layer 4 has two regions, namely, a first active material layer region 41 and a second active material layer region 42 . The sheet resistance of the first active material layer region 41 is greater than that of the second active material layer region 42 .

[0098] In this embodiment, the polarization of the first region 41 of the active material layer itself is larger, which can offset the effect of the reduced polarization of a part of the electrode due to poor heat dissipation, high temperature and small expansion force of the battery cell during the cycle, making the polarization of the electrode more uniform and avoiding the occurrence of lithium deposition; the polarization of the second region 42 of the active material layer itself is smaller, which can offset the effect of the increased polarization of a part of the electrode due to good heat dissipation, low temperature and large expansion force of the battery cell during the cycle, making the polarization of the electrode more uniform and avoiding the occurrence of lithium deposition.

[0099] In this embodiment, the undercoat layer 3 itself is uniformly polarized and does not have the function of offsetting the effect of uneven polarization of the pole piece caused by the above-mentioned battery cell cycle process. The undercoat layer 3 mainly plays the role of strengthening the bonding force between the active material layer 4 and the current collector 1.

[0100] In one embodiment, referring to Figure 5 The base coating 3 has two regions, namely a base coating first region 31 and a base coating second region 32 . The sheet resistance of the base coating first region 31 of the base coating 3 is greater than the sheet resistance of the base coating second region 32 .

[0101] Meanwhile, the active material layer 4 has two regions, namely, a first active material layer region 41 and a second active material layer region 42 . The sheet resistance of the first active material layer region 41 is greater than that of the second active material layer region 42 .

[0102] The orthographic projection of the first area 31 of the undercoat layer coincides with the first area 41 of the active material layer, and the orthographic projection of the second area 32 of the undercoat layer coincides with the second area 42 of the active material layer.

[0103] Furthermore, the sum of the sheet resistances in the undercoat layer first region 31 and the active material layer first region 41 is greater than the sum of the sheet resistances in the undercoat layer second region 32 and the active material layer second region 42 .

[0104] In this embodiment, the polarization of the first region 31 of the bottom coating layer and the first region 41 of the active material layer is larger, and the polarization of the second region 32 of the bottom coating layer and the second region 42 of the active material layer is smaller, which work together to offset the uneven polarization of the electrode caused by uneven temperature and expansion force during the battery cell cycle, thereby making the polarization of the cathode electrode of the present invention more uniform and avoiding the phenomenon of lithium deposition.

[0105] The present invention also provides a method for preparing a cathode electrode sheet, comprising the following steps:

[0106] A first coating is applied on a portion of the surface of the current collector to form a first region of the membrane, and a second coating is applied on another portion of the surface of the current collector to form a second region of the membrane, to prepare a cathode electrode, wherein the membrane resistance of the first region is greater than the membrane resistance of the second region.

[0107] The above membrane of the present invention includes an active material layer and / or a bottom coating layer. The resistance relationship between different regions in the active material layer and / or the bottom coating layer is adjusted to solve the problem of lithium deposition caused by uneven polarization of the pole piece.

[0108] The membrane formed by coating the first coating in the present invention has a large polarization itself and can be coated on the area of ​​the electrode that is easily affected by external factors and has a reduced polarization, thereby offsetting each other and making the polarization of the electrode more uniform, thereby avoiding lithium deposition on the electrode.

[0109] The membrane formed by coating the second coating in the present invention has a relatively small polarization itself and can be coated on the area of ​​the electrode that is easily polarized due to external factors, thereby offsetting each other and making the polarization of the electrode more uniform, thereby avoiding lithium deposition on the electrode.

[0110] In some implementations, the conductive agent and the binder are evenly mixed to obtain a first coating, and the conductive agent and the binder are evenly mixed to obtain a second coating; at the same time, the content of the conductive agent in the first coating is adjusted to be less than the content of the conductive agent in the second coating, and the content of the binder in the first coating is adjusted to be greater than the content of the binder in the second coating, so that the resistance of the first area of ​​the diaphragm is greater than the resistance of the second area of ​​the diaphragm.

[0111] In some embodiments, the conductive agent and the binder are dissolved in an organic solvent and stirred to obtain the first coating and / or the second coating. The organic solvent may be N-methylpyrrolidone.

[0112] In some embodiments, the first coating and / or the second coating include but are not limited to the above-mentioned conductive agent and binder, and additives known to those skilled in the art, such as active materials, may be added as required. The active material includes at least one of lithium cobalt oxide compounds, lithium nickel cobalt manganese oxide compounds, lithium nickel cobalt aluminum oxide compounds, lithium iron phosphate compounds, lithium manganese oxide compounds, lithium iron phosphate manganese oxide compounds, and lithium nickel manganese oxide compounds.

[0113] In some embodiments, a lithium iron phosphate compound is selected as the active material, and further, the gram capacity of the lithium iron phosphate compound is 139 mAh / g.

[0114] In some embodiments, the coating weight of the first coating and / or the second coating is 0.305 g / 1540.25 mm2, calculated based on the weight excluding the solvent. 2 .

[0115] In some embodiments, after the film is coated on the surface of the current collector, it is dried and cold pressed to obtain the cathode electrode.

[0116] The present invention further provides a battery, which includes the above-mentioned cathode electrode sheet. The battery of the present invention can be a battery cell, a battery module or a battery pack.

[0117] The battery cell, battery module or battery pack of the present invention has the same beneficial effects as the above-mentioned cathode electrode sheet, and has a higher cycle life, which will not be described in detail here.

[0118] In some embodiments, when the battery is a battery cell, the battery further includes an anode plate, a separator and an electrolyte.

[0119] The anode plate, the separator and the electrolyte can be prepared according to methods well known to those skilled in the art.

[0120] In some embodiments, the anode electrode sheet includes an active material, a conductive agent, a binder, and a current collector.

[0121] In some embodiments, the active material in the anode plate includes at least one of artificial graphite, natural graphite, and mesophase carbon microbeads.

[0122] In some embodiments, the conductive agent in the anode plate includes at least one of conductive carbon black, conductive graphite, conductive ink, Ketjen black, carbon nanotubes, and conductive carbon fibers.

[0123] In some embodiments, the binder in the anode plate includes at least one of polystyrene butadiene copolymer (SBR) and sodium carboxymethyl cellulose (CMC).

[0124] In some embodiments, the binder in the anode plate includes polystyrene butadiene copolymer (SBR) and sodium carboxymethyl cellulose (CMC).

[0125] The anode electrode sheet of the present invention can be prepared according to a preparation method well known to those skilled in the art.

[0126] In some embodiments, the active material, conductive agent and binder in the anode plate are dissolved in deionized water and mixed evenly to obtain an anode slurry, and then the anode slurry is coated on the surface of the current collector, and the anode plate is obtained after drying and cold pressing.

[0127] Furthermore, excluding the weight of the solvent, the coating weight of the anode slurry is 0.136 g / 1540.25 mm 2 .

[0128] In some embodiments, the isolation film includes at least one of polyethylene, polypropylene, and polyvinylidene fluoride.

[0129] The present invention does not limit the raw material composition and preparation method of the electrolyte, and the electrolyte can be prepared according to the raw material composition and preparation method known to those skilled in the art.

[0130] In some embodiments, the electrolyte includes ethylene carbonate (EC), propylene carbonate (PC), dimethyl carbonate (DMC), lithium hexafluorophosphate (LiPF6), vinylene carbonate (VC), diethylene sulfate (DTD), and 1,3-propane sultone (PS).

[0131] In the preparation method, ethylene carbonate (EC), propylene carbonate (PC) and dimethyl carbonate (DMC) are first mixed, and then lithium hexafluorophosphate (LiPF6), vinylene carbonate (VC), vinyl sulfate (DTD), and 1,3-propane sultone (PS) are dissolved in an organic solvent and stirred evenly to obtain an electrolyte.

[0132] In some embodiments, the weight ratio of ethylene carbonate (EC), propylene carbonate (PC), and dimethyl carbonate (DMC) may be 1:1:1.

[0133] In some embodiments, the mass percentages of vinylene carbonate (VC), diethyl sulfate (DTD) and 1,3-propane sultone (PS) are 3%, 1% and 1% respectively.

[0134] In some embodiments, the preparation of the electrolyte is completed in an argon atmosphere glove box with a water content of <10 ppm.

[0135] Furthermore, the present invention also provides a method for preparing a battery, comprising the following steps:

[0136] Step 1: Prepare a cathode electrode piece according to the method for preparing a cathode electrode piece of the present invention;

[0137] Step 2: stack the cathode electrode sheet, the isolation membrane and the anode electrode sheet in sequence to prepare an electrode assembly, place the electrode assembly in a shell, and inject electrolyte into the shell to obtain a battery.

[0138] It should be noted that the isolation membrane is located between the cathode electrode and the anode electrode and plays an isolation role.

[0139] The present invention does not limit the types and preparation methods of the isolation membrane, the anode electrode and the electrolyte, and the types and preparation methods known to those skilled in the art may be selected.

[0140] In some embodiments, the cathode electrode sheet, the isolation film and the anode electrode sheet are stacked in sequence and then wound to obtain a cylindrical bare battery cell.

[0141] In addition, the present invention also provides an electrical device including the above-mentioned battery. The electrical device using the above-mentioned battery has the same beneficial effects as the above-mentioned battery and has a longer service life.

[0142] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the following specific embodiments are only used to explain the present invention, and are not used to limit the present invention.

[0143] Example 1

[0144] Reference Figure 1 and Figure 2 In this embodiment, the cathode electrode sheet comprises a current collector 1 and a membrane 2 formed on the current collector. The membrane 2 is an active material layer and has two regions, a first region 21 and a second region 22 .

[0145] S10, preparation of cathode electrode:

[0146] The cathode active material lithium iron phosphate (gram capacity of 139 mAh / g), the conductive agent acetylene black, and the binder PVDF are mixed in a weight ratio of 94:4:2, and the solvent N-methylpyrrolidone is added, and the mixture is stirred and mixed to obtain a second coating; the cathode active material lithium iron phosphate (gram capacity of 139 mAh / g), the conductive agent acetylene black, and the binder PVDF are mixed in a weight ratio of 94:3:3, and the solvent N-methylpyrrolidone is added, and the mixture is stirred and mixed to obtain a first coating;

[0147] The first coating is applied to the center area of ​​the two surfaces of the cathode current collector aluminum foil to form the first area 21 of the active material layer, and the second coating is applied to the edge areas on both sides of the center area of ​​the two surfaces of the cathode current collector aluminum foil to form the second area 22 of the active material layer to obtain an active material layer with a zebra structure, and then the whole is dried and cold pressed to obtain a cathode electrode. The coating weight is 0.305g / 1540.25mm 2 (Coating weight does not include the weight of solvent).

[0148] S20, preparation of anode sheet

[0149] The anode active material artificial graphite (gram capacity of 340 mAh / g), the conductive agent acetylene black, and the binder SBR+CMC were mixed in a weight ratio of 95:1.5:3.1:0.4, and the solvent deionized water was added, and the mixture was fully stirred to obtain the anode slurry, which was then coated on both surfaces of the anode current collector copper foil, wherein the coating weight of the anode slurry was 0.136 g / 1540.25 mm 2 (The coating weight does not include the weight of the solvent), and the anode electrode sheet is obtained after drying and cold pressing.

[0150] S30, Preparation of electrolyte

[0151] In an argon atmosphere glove box with a water content of <10ppm, EC, PC, and DMC were mixed in a weight ratio of EC:PC:DMC=3:3:3, and then LiPF6, VC, DTD, and PS were added to the mixed organic solvent and stirred evenly to obtain an electrolyte, wherein the concentration of LiPF6 in the lithium-ion battery electrolyte was 1 mol / L, and the mass percentages of VC, DTD, and PS were 3%, 1%, and 1%, respectively.

[0152] S40, Preparation of isolation membrane

[0153] A polyethylene porous membrane was used as the isolation membrane.

[0154] S50, Preparation of lithium-ion secondary batteries

[0155] The cathode electrode sheet, the separator, and the anode electrode sheet are stacked in order, so that the separator is located between the cathode electrode sheet and the anode electrode sheet to play a role of isolation, and then wound to obtain a bare battery cell. The bare battery cell is placed in an outer package, injected with a prepared electrolyte, and packaged for formation to obtain a lithium-ion secondary battery.

[0156] Example 2

[0157] Reference Figure 3In this embodiment, the cathode electrode sheet has a current collector 1 and a primer layer 3 formed on the current collector, and an active material layer 4 formed on the surface of the primer layer 3 facing away from the current collector 1. The primer layer 3 has two regions: a first primer layer region 31 and a second primer layer region 32.

[0158] S10, Preparation of cathode electrode bottom coating 3

[0159] The conductive agent acetylene black, the binder, and calcium hydroxide are mixed in a weight ratio of 45:45:10, and solvent water is added, and the mixture is stirred and mixed thoroughly to obtain a second coating; the conductive agent acetylene black, the binder, and calcium hydroxide are mixed in a weight ratio of 40:50:10, and solvent water is added, and the mixture is stirred and mixed thoroughly to obtain a first coating;

[0160] The first coating is applied to the center area of ​​the two surfaces of the cathode current collector aluminum foil to form the first area 31 of the primer layer, and the second coating is applied to the edge areas on both sides of the center area of ​​the two surfaces of the cathode current collector aluminum foil to form the second area 32 of the primer layer to obtain the primer layer 3 with a zebra structure, and then the whole is dried. The coating weight is 0.305g / 1540.25mm 2 (Coating weight does not include the weight of solvent).

[0161] S20, cathode electrode preparation

[0162] The cathode active material lithium iron phosphate (gram capacity of 139 mAh / g), the conductive agent acetylene black, and the binder PVDF are mixed in a weight ratio of 94:4:2, and the solvent N-methylpyrrolidone is added, and the mixture is fully stirred to obtain a cathode slurry; the cathode slurry is evenly coated on the surface of the above-mentioned primer layer 3 away from the current collector 1 to form an active material layer 4, and then the whole is dried and cold pressed to obtain a cathode electrode sheet.

[0163] S30, preparation of anode electrode

[0164] The anode active material artificial graphite (gram capacity of 340 mAh / g), the conductive agent acetylene black, and the binder SBR+CMC were mixed in a weight ratio of 95:1.5:3.1:0.4, and the solvent deionized water was added, and the mixture was fully stirred to obtain the anode slurry, which was then coated on both surfaces of the anode current collector copper foil, wherein the coating weight of the anode slurry was 0.136 g / 1540.25 mm 2 (The coating weight does not include the weight of the solvent), and the anode electrode sheet is obtained after drying and cold pressing.

[0165] S40, Preparation of electrolyte

[0166] In an argon atmosphere glove box with a water content of <10ppm, EC, PC, and DMC were mixed in a weight ratio of EC:PC:DMC=3:3:3, and then LiPF6, VC, DTD, and PS were added to the mixed organic solvent and stirred evenly to obtain an electrolyte, wherein the concentration of LiPF6 in the lithium-ion battery electrolyte was 1 mol / L, and the mass percentages of VC, DTD, and PS were 3%, 1%, and 1%, respectively.

[0167] S50, Preparation of isolation membrane

[0168] A polyethylene porous membrane was used as the isolation membrane.

[0169] S60, Preparation of lithium-ion secondary batteries

[0170] The cathode electrode sheet, the separator, and the anode electrode sheet are stacked in order, so that the separator is located between the cathode electrode sheet and the anode electrode sheet to play a role of isolation, and then wound to obtain a bare battery cell. The bare battery cell is placed in an outer package, injected with a prepared electrolyte, and packaged for formation to obtain a lithium-ion secondary battery.

[0171] Embodiment 3-6

[0172] The preparation methods of Examples 3-6 are basically the same as those of Example 1, except that the weight ratios of the conductive agent and the binder in the first region 21 and the second region 22 of the cathode electrode active material layer are different, as shown in Table 1.

[0173] Examples 7-10

[0174] The preparation methods of Examples 7-10 are basically the same as those of Example 2, except that the weight ratios of the conductive agent and the binder in the first area 31 of the cathode electrode bottom coating and the second area 32 of the bottom coating are different, as shown in Table 1 for details.

[0175] Comparative Example 1

[0176] The preparation method of Comparative Example 1 is substantially the same as that of Example 1, except that the weight of the conductive agent and the weight of the binder in the first region 21 of the active material layer are respectively the same as the weight of the conductive agent and the weight of the binder in the second region 22 .

[0177] Comparative Example 2

[0178] The preparation method of comparative example 2 is substantially the same as that of example 2, except that the weight of the conductive agent and the weight of the binder in the first region 31 of the primer layer are respectively the same as the weight of the conductive agent and the weight of the binder in the second region 32 of the primer layer.

[0179] Comparative Example 3

[0180] The preparation method of Comparative Example 3 is basically the same as the preparation method of Example 1, except that the conductive agent content in the first region 21 of the cathode active material layer is greater than the conductive agent content in the second region 22, and the binder content in the first region 21 of the cathode active material layer is less than the binder content in the second region 22, as shown in Table 1 for details.

[0181] Comparative Example 4

[0182] The preparation method of Comparative Example 4 is basically the same as the preparation method of Example 1, except that the conductive agent content in the first area 31 of the cathode primer coating is greater than the conductive agent content in the second area 32 of the cathode primer coating, and the binder content in the first area 31 of the cathode primer coating is less than the binder content in the second area 32 of the cathode primer coating, as shown in Table 1 for details.

[0183] Table 1 Contents of conductive agent and binder in active material layer or undercoat layer of cathode electrode sheet in Examples and Comparative Examples

[0184]

[0185]

[0186] “-” in the table means no addition.

[0187] Performance Testing

[0188] The lithium ion secondary batteries prepared in the examples and comparative examples were tested as follows. The test results are shown in Table 2.

[0189] (1) Room temperature cycle performance test of lithium-ion secondary batteries

[0190] At 25°C, the lithium-ion secondary battery is first charged at a constant current of 1C (i.e., the current value that completely discharges the theoretical capacity within 1 hour) to a voltage of 3.65V, then charged at a constant voltage of 3.65V to a current of 0.05C. After standing for 5 minutes, the lithium-ion secondary battery is discharged at a constant current of 1C to a voltage of 2.5V. This is a charge and discharge cycle process, and the discharge capacity this time is the discharge capacity of the first cycle. The lithium-ion secondary battery is subjected to multiple cycle charge and discharge tests according to the above method until the discharge capacity of the lithium-ion secondary battery decays to 80%, and the number of cycles of the lithium-ion secondary battery is recorded.

[0191] (2) High temperature cycle performance test of lithium-ion secondary batteries

[0192] At 60°C, the lithium-ion secondary battery is first charged at a constant current of 1C (i.e., the current value that completely discharges the theoretical capacity within 1 hour) to a voltage of 3.65V, then charged at a constant voltage of 3.65V to a current of 0.05C. After standing for 5 minutes, the lithium-ion secondary battery is discharged at a constant current of 1C to a voltage of 2.5V. This is a charge and discharge cycle process, and the discharge capacity this time is the discharge capacity of the first cycle. The lithium-ion secondary battery is subjected to multiple cycle charge and discharge tests according to the above method, and the discharge capacity of the 500th cycle is detected.

[0193] Capacity retention rate of the lithium ion secondary battery after 500 cycles at 60° C.=(discharge capacity at the 500th cycle / discharge capacity at the first cycle)×100%.

[0194] Table 2 Performance test results of lithium ion secondary batteries of the embodiments and comparative examples

[0195]

[0196] From Table 2, we can see that:

[0197] The lithium ion secondary batteries of Examples 1-10 have a higher cycle life function when the capacity decays to 80% than the lithium ion secondary batteries of Comparative Examples 1-4, and the capacity retention rate after 500 cycles is higher, and the electrode does not have lithium plating, indicating that the cathode electrode of the present invention can effectively improve the problem of lithium plating of the electrode, thereby increasing the cycle life of the battery.

[0198] The conductive agent content and binder content in each area of ​​the cathode electrode of the lithium-ion secondary battery of Comparative Example 1 and Comparative Example 2 are distributed relatively evenly, the resistance difference is not large, and the polarization of the cathode electrode itself is also relatively uniform, which cannot offset the polarization changes of the electrode caused by uneven temperature and expansion force during the battery cell cycle. Lithium deposition occurs on the electrode, and the battery's cycle life function deteriorates.

[0199] In Comparative Example 3, the conductive agent content of the first region 21 of the cathode active material layer is higher than that of the second region 22, and the binder content is lower, so the resistance of the first region 21 is lower than that of the second region 22. As a result, the polarization of the first region 21 itself is smaller, and it cannot offset the influence of the high temperature and small expansion force in the middle part during the battery cell cycle, which leads to the decrease in polarization of the pole piece; while the polarization of the second region 22 itself is larger, and it cannot offset the influence of the low temperature and large expansion force in the head and tail parts during the battery cell cycle, which leads to the increase in polarization of the pole piece. Lithium deposition occurs in the pole piece, and the cycle life function of the battery is deteriorated compared with the batteries of Examples 1 and Examples 3 to 6.

[0200] Similarly, in Comparative Example 4, the conductive agent content of the first area 31 of the cathode bottom coating is higher than that of the second area 32 of the bottom coating, and the content of the binder is lower, so the resistance of the first area 31 of the bottom coating is lower than that of the second area 32 of the bottom coating. As a result, the polarization of the first area 31 of the bottom coating itself is smaller, which cannot offset the influence of the high temperature and small expansion force in the middle part during the battery cell cycle, which leads to the decrease in polarization of the pole piece, while the polarization of the second area 32 of the bottom coating itself is larger, which cannot offset the influence of the low temperature and large expansion force in the head and tail parts during the battery cell cycle, which leads to the increase in polarization of the pole piece, and lithium deposition occurs in the pole piece. Compared with the batteries of Examples 2 and Examples 7 to 10, the battery cycle life function is deteriorated.

[0201] The above are only optional embodiments of the present invention, and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A cathode electrode sheet, comprising a current collector and a membrane sheet disposed on the surface of the current collector, characterized in that: The diaphragm is provided with at least two regions, wherein the two regions are defined as a first region and a second region, and the diaphragm resistance of the first region is greater than the diaphragm resistance of the second region; The membrane includes at least one of an active material layer and a primer layer.

2. The cathode electrode according to claim 1, characterized in that: The membrane includes a conductive agent and a binder, wherein the conductive agent content in the first region is less than that in the second region, and the binder content in the first region is greater than that in the second region.

3. The cathode electrode according to claim 1, characterized in that: The width of the first region accounts for more than one fifth of the width of the diaphragm.

4. The cathode electrode according to any one of claims 1 to 3, characterized in that: The first region is located in the center of the active material layer, and the second region is located in the edge regions on both sides of the center.

5. The cathode electrode according to any one of claims 1 to 3, characterized in that: The thickness of the active material layer is less than or equal to 250 mm.

6. The cathode electrode according to any one of claims 1 to 3, characterized in that: The first area is located in the center area of ​​the base coating layer, and the second area is located in the edge areas on both sides of the center area.

7. The cathode electrode according to any one of claims 1 to 3, characterized in that: The thickness of the primer layer is less than or equal to 40 μm.

8. The cathode electrode according to any one of claims 1 to 3, characterized in that: The membrane comprises a primer layer and an active material layer. The primer layer is disposed on a surface of the current collector, and the active material layer is disposed on a surface of the primer layer away from the current collector.

9. The cathode electrode according to any one of claims 1 to 3, characterized in that: The active material layer is provided with at least two regions, wherein the two regions are defined as a first region of the active material layer and a second region of the active material layer, and the membrane resistance of the first region of the active material layer is greater than the membrane resistance of the second region of the active material layer; And / or, the base coating layer has at least two regions, the two regions are defined as a first base coating layer region and a second base coating layer region, and the film resistance of the first base coating layer region is greater than the film resistance of the second base coating layer region.

10. The cathode electrode according to claim 9, characterized in that: The conductive agent content of the first region of the active material layer is less than the conductive agent content of the second region of the active material layer, and the binder content of the first region of the active material layer is greater than the binder content of the second region of the active material layer; And / or, the conductive agent content of the first region of the primer layer is less than that of the second region of the primer layer, and the binder content of the first region of the primer layer is greater than that of the second region of the primer layer.

11. The cathode electrode according to claim 2, characterized in that: The conductive agent includes at least one of conductive carbon black, conductive graphite, conductive ink, Ketjen black, carbon nanotubes, and conductive carbon fibers.

12. The cathode electrode according to claim 2, characterized in that: The binder includes at least one of polyvinylidene fluoride, polyvinyl alcohol, polytetrafluoroethylene and sodium carboxymethyl cellulose.

13. A method for preparing a cathode electrode sheet according to any one of claims 1 to 12, characterized in that: The following steps are involved: The cathode electrode sheet is prepared by coating a first coating on a portion of the surface of the current collector to form a first region of the diaphragm, and coating a second coating on another portion of the surface of the current collector to form a second region of the diaphragm, wherein the diaphragm resistance of the first region is greater than that of the second region.

14. The method for preparing a cathode electrode sheet according to claim 13, characterized in that: The conductive agent and the binder are mixed evenly to obtain a first coating, and the conductive agent and the binder are mixed evenly to obtain a second coating; The content of the conductive agent in the first coating is less than that in the second coating, and the content of the binder in the first coating is greater than that in the second coating.

15. The method for preparing a cathode electrode sheet according to claim 14, characterized in that: The conductive agent and the binder are dissolved in an organic solvent and mixed evenly to obtain the first coating and / or the second coating.

16. The method for preparing a cathode electrode sheet according to claim 14 or 15, characterized in that: The first coating material and / or the second coating material further contain active materials.

17. The method for preparing a cathode electrode sheet according to claim 16, characterized in that: The active material includes at least one of a lithium cobalt oxide compound, a nickel cobalt manganese oxide lithium compound, a nickel cobalt aluminum oxide compound, a lithium iron phosphate compound, a lithium manganese oxide compound, a lithium iron phosphate manganese oxide compound, and a nickel manganese oxide lithium compound.

18. The method for preparing a cathode electrode sheet according to claim 13, characterized in that: The preparation method further comprises the following steps: after the film is formed by coating the surface of the current collector, drying and cold pressing are performed to obtain the cathode electrode sheet.

19. A battery, characterized in that: The battery comprises the cathode electrode according to any one of claims 1 to 12, and the battery is any one of a battery cell, a battery module, and a battery pack.

20. An electrical device, characterized in that: The electrical device comprises the battery according to claim 19.

Citation Information

Patent Citations

  • Electrochemical device and electronic device

    CN114270560A