Fire-resistant polyphenylene ether molded body and method for producing fire-resistant polyphenylene ether molded body

By forming a specific chemical structure in the polyphenylene ether molded body and performing a two-stage heat treatment, the deficiencies in fire resistance and flame retardancy of polyphenylene ether fibers and non-woven fabrics are solved, and efficient fire resistance and heat resistance improvements are achieved. , suitable for demanding refractory sheet applications.

CN115843303BActive Publication Date: 2024-10-01TOYOBO MC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180049157.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-03-23
Publication Date
2024-10-01
Estimated Expiration
2041-03-23

AI Technical Summary

Technical Problem

Existing polyphenylene ether fibers and non-woven fabrics have deficiencies in fire resistance, flame retardancy and heat resistance, making it difficult to meet the high requirements of fire-resistant sheet applications.

Method used

By forming a refractory polyphenylene ether molded body with a specific chemical structure, infrared spectroscopy was used to detect the absorbance ratio of the wave number of C=O stretching vibration of 1732 cm-1 and the wavelength of the stretching skeleton vibration between benzene ring carbon and carbon of 1600 cm-1. is above 0.42, and undergoes two-stage heat treatment to improve its specific gravity and fire resistance.

Benefits of technology

It achieves a high degree of flame retardancy, fire resistance and heat resistance of the polyphenylene ether molded body, which is suitable for applications such as high-demand refractory sheets, and its durability and processing at high temperatures are significantly improved through a two-stage heat treatment method. sex.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115843303B_ABST
    Figure CN115843303B_ABST
Patent Text Reader

Abstract

The object of the present invention is to provide: a refractory polyphenylene ether molded body endowed with fire resistance, heat resistance, and higher flame retardancy, and a method for producing the refractory polyphenylene ether molded body. The present invention relates to a refractory polyphenylene ether molded body, characterized in that, in a measurement based on infrared spectroscopy, a wave number of 1732 cm-1 derived from C=O stretching vibration ‑1 The absorbance height A is related to the wavelength of 1600 cm-1, which is derived from the skeleton vibration caused by the stretching between carbon atoms in the benzene ring. ‑1 The absorbance height ratio (A / B) of the absorbance height B is 0.42 or more, and the specific gravity of the flame-resistant polyphenylene ether molded body is 1.25 or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a fire-resistant polyphenylene ether molded body having a specific chemical structure detectable by infrared spectroscopy and a method for producing the same. Background Art

[0002] Polyphenylene ether (hereinafter, sometimes referred to as PPE) has excellent heat resistance, flame retardancy, strength, chemical resistance, etc. Therefore, molded products formed of polyphenylene ether are used in a wide range of fields. For example, various fibers containing polyphenylene ether are known (for example, see Patent Documents 1 to 3). However, although polyphenylene ether fibers and nonwoven fabrics formed of polyphenylene ether fibers have excellent flame retardancy, they are not sufficient for use in, for example, fire-resistant sheets for protecting covers from flames.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2004-190156

[0006] Patent Document 2: Japanese Patent Application No. 2017-502179

[0007] Patent Document 3: Japanese Patent Application Publication No. 2008-138294 Summary of the invention

[0008] Problem that the invention aims to solve

[0009] Patent Documents 1 to 3 do not provide any research on the fire resistance of polyphenylene ether fibers. Therefore, polyphenylene ether fibers and polyphenylene ether molded products such as nonwoven fabrics formed from polyphenylene ether fibers have not been given sufficient fire resistance, heat resistance, and higher flame retardancy to the extent that they can be used in fire-resistant sheets, etc. This is the current situation.

[0010] Therefore, an object of the present invention is to provide a flame-resistant polyphenylene ether molded body imparted with flame resistance, heat resistance, and higher flame retardancy, and a method for producing the flame-resistant polyphenylene ether molded body.

[0011] Solutions for solving problems

[0012] The present inventors have conducted intensive studies and have found that the above-mentioned problems can be solved by forming a flame-resistant polyphenylene ether molded body having a specific chemical structure detectable by infrared spectroscopy, thereby completing the present invention.

[0013] That is, the present invention relates to a flame-resistant polyphenylene ether molded body, characterized in that the wave number derived from C=O stretching vibration is 1732 cm-1 in the measurement based on infrared spectroscopy. -1The absorbance height A is related to the wavelength of 1600 cm-1, which is derived from the skeleton vibration caused by the stretching between carbon atoms in the benzene ring. -1 The absorbance height ratio (A / B) of the absorbance height B is 0.42 or more, and the specific gravity of the flame-resistant polyphenylene ether molded body is 1.25 or more.

[0014] The flame-resistant polyphenylene ether molded article preferably has a difference between a weight loss rate (%) at 150°C and a weight loss rate (%) at 400°C relative to an initial weight at 20°C of 5.0% or less.

[0015] The LOI value of the flame-resistant polyphenylene ether molded article is preferably 35 or more.

[0016] The flame-resistant polyphenylene ether molded article preferably has a strength retention rate of 40% or more at 400°C.

[0017] The flame resistant polyphenylene ether molded article is preferably a flame resistant polyphenylene ether fiber.

[0018] The flame-resistant polyphenylene ether fiber preferably has a fineness of 100 dtex or less.

[0019] The flame resistant polyphenylene ether fibers are preferably flame resistant polyphenylene ether short fibers.

[0020] The flame resistant polyphenylene ether molded article is preferably a flame resistant polyphenylene ether nonwoven fabric.

[0021] The polyphenylene ether fibers constituting the flame-resistant polyphenylene ether nonwoven fabric preferably have a fineness of 100 dtex or less.

[0022] The flame resistant polyphenylene ether molded product is preferably a flame resistant polyphenylene ether cloth.

[0023] The flame resistant polyphenylene ether molded article is preferably a flame resistant polyphenylene ether film.

[0024] The present invention also relates to a method for producing a flame-resistant polyphenylene ether molded body, characterized in that the polyphenylene ether molded body is heat-treated in air at 120 to 240° C. for 1 to 30 hours to be infusible, and further heat-treated in air at 260 to 400° C. for 0.1 to 10 hours to be flame-resistant.

[0025] Preferably, the free radical amount of the polyphenylene ether molded article is 100 g -1 above.

[0026] The polyphenylene ether molded article is preferably a polyphenylene ether fiber.

[0027] The polyphenylene ether molded article is preferably a polyphenylene ether nonwoven fabric.

[0028] The polyphenylene ether molded article is preferably a polyphenylene ether cloth.

[0029] The polyphenylene ether molded article is preferably a polyphenylene ether film.

[0030] Effects of the Invention

[0031] In the measurement of the flame-resistant polyphenylene ether molded product of the present invention by infrared spectroscopy, the wave number derived from the stretching vibration of C=O is 1732 cm -1 The absorbance height A is related to the wavelength of 1600 cm-1, which is derived from the skeleton vibration caused by the stretching between carbon atoms in the benzene ring. -1 The absorbance height ratio (A / B) of the absorbance height B is 0.42 or more, and it has a specific amount of C=O structure, and the specific gravity of the refractory polyphenylene ether molded body is 1.25 or more. The refractory polyphenylene ether molded body of the present invention has a high specific gravity, and embodies high flame retardancy, fire resistance, heat resistance, etc., and can be suitable for refractory sheets requiring high flame retardancy. In addition, according to the manufacturing method of the present invention, two stages of heat treatment (infusibility treatment, refractory treatment) are carried out, so that a refractory polyphenylene ether molded body with high flame retardancy, fire resistance, heat resistance, etc. can be manufactured. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 This is a cross-sectional view schematically showing one embodiment of a method for producing a polyphenylene ether melt-spun fiber used in the present invention. DETAILED DESCRIPTION

[0033] 1. Fire-resistant polyphenylene ether molding

[0034] The flame-resistant polyphenylene ether molded article of the present invention is characterized in that, in the measurement by infrared spectroscopy, the wave number derived from the stretching vibration of C=O is 1732 cm -1 The absorbance height A is related to the wavelength of 1600 cm-1, which is derived from the skeleton vibration caused by the stretching between carbon atoms in the benzene ring. -1 The absorbance height ratio (A / B) of the absorbance height B is 0.42 or more, and the specific gravity of the flame-resistant polyphenylene ether molded body is 1.25 or more.

[0035] The wavelength of the C=O stretching vibration is 1732 cm -1 The peak is formed by subjecting the polyphenylene ether molded body to a flame retardant treatment. By forming a polyphenylene ether molded body having a specific amount of such a C=O structure, a high degree of flame retardancy, fire resistance, heat resistance, etc. can be imparted. It should be noted that in the present invention, the peak derived from the stretching vibration of C=O and the peak derived from the skeleton vibration based on the stretching between carbon and carbon of the benzene ring are set to wavelengths of 1732±10cm, respectively, taking into account the measurement error based on infrared spectroscopy. -1 、1600±10cm -1 The peak of the range.

[0036] The wave number from the C=O stretching vibration is 1732 cm -1 The absorbance height A is related to the wavelength of 1600 cm-1, which is derived from the skeleton vibration caused by the stretching between carbon atoms in the benzene ring. -1 The absorbance height ratio (A / B) of the absorbance height B is 0.42 or more, preferably 0.45 or more, and more preferably 0.50 or more. By being in the aforementioned range, the absorbance height ratio can impart very high flame retardancy, and specifically, the LOI value (limiting oxygen index) can exceed 30. In addition, fire resistance, heat resistance, etc. can also be imparted. Therefore, the flame-resistant polyphenylene ether molded body of the present invention can be suitable for use as a fire-resistant sheet or the like requiring very high flame retardancy, fire resistance, heat resistance, etc. In addition, the upper limit of the aforementioned absorbance height ratio is not particularly limited, and is preferably 1.5 or less, and more preferably 1.0 or less.

[0037] For the flame-resistant polyphenylene ether molded body of the present invention, the difference between the weight loss rate (%) at 150°C and the weight loss rate (%) at 400°C is preferably 5.0% or less, more preferably 4.0% or less, and further preferably 3.5% or less relative to the initial weight at 20°C. By making the difference in weight loss rate within the aforementioned range, the degradation of the polymer is suppressed and the durability can be improved, so it is preferred. In addition, the difference in weight loss rate is expected to be 0%, but usually there is a weight reduction of about 0.1% or more, and sometimes it is about 0.15% or more.

[0038] The specific gravity of the flame-resistant polyphenylene ether molded body of the present invention is 1.25 or more, preferably 1.28 or more, more preferably 1.3 or more, further preferably 1.35 or more, further preferably 1.38 or more, and particularly preferably 1.40 or more. By making the specific gravity within the aforementioned range, the flame resistant of the polyphenylene ether molded body is fully carried out, and the fire resistance is improved. In addition, the upper limit of the specific gravity is not particularly limited, but is preferably 2.0 or less, and more preferably 1.8 or less.

[0039] The LOI value of the flame retardant polyphenylene ether molded product of the present invention is preferably 30 or more, more preferably more than 30, further preferably 32 or more, and particularly preferably 35 or more. By making the LOI value within the above range, the flame retardant polyphenylene ether molded product obtained is excellent in flame retardancy, which is preferred. Here, the LOI value refers to the limiting oxygen index, and the larger the LOI value, the better the flame retardancy. Therefore, the larger the LOI value, the more preferred, and its upper limit is not particularly limited.

[0040] The tensile elongation of the flame-resistant polyphenylene ether molded body of the present invention is preferably 5% or more, more preferably 7% or more, and further preferably 10% or more. The tensile elongation is preferably within the aforementioned range, so that processability can be improved. In addition, the upper limit of the tensile elongation is not particularly limited, but is preferably 100% or less, and more preferably 80% or less.

[0041] The fire-resistant polyphenylene ether molded body of the present invention preferably has a strength retention rate of 40% or more at 400°C, more preferably 50% or more, and further preferably 60% or more. By making the strength retention rate at 400°C in the aforementioned range, the durability when used at high temperatures is high, so it is preferred. In addition, the upper limit of the strength retention rate at 400°C is not particularly limited, but is preferably 100% or less, and more preferably 99% or less. Here, the strength retention rate at 400°C refers to: the retention rate of strength after heat treatment at 400°C for 10 minutes.

[0042] The elongation retention of the flame-resistant polyphenylene ether molded article of the present invention at 400°C is preferably 40% or more, more preferably 50% or more, and further preferably 55% or more. By making the elongation retention at 400°C in the aforementioned range, the durability when used at high temperature is high, so it is preferred. In addition, the upper limit of the elongation retention at 400°C is not particularly limited, but is preferably 100% or less, and more preferably 99% or less. Here, the elongation retention at 400°C refers to the retention of the elongation after heat treatment at 400°C for 10 minutes.

[0043] Representative examples of the refractory polyphenylene ether molded article include refractory polyphenylene ether fibers, refractory polyphenylene ether nonwoven fabrics, refractory polyphenylene ether fabrics, and refractory polyphenylene ether films. The refractory polyphenylene ether fibers may be long fibers or short fibers.

[0044] When the refractory polyphenylene ether molded body is a refractory polyphenylene ether fiber, the fineness thereof is not particularly limited and can be appropriately determined according to the purpose of using the fiber, for example, preferably 100 dtex or less, more preferably 95 dtex or less, and further preferably 90 dtex or less. By making the fineness within the aforementioned range, it can be processed into various shapes such as woven fabrics, knitted fabrics, short fiber nonwoven fabrics, and cloth, so it is preferred. In addition, the lower limit of the fineness is not particularly limited, preferably 0.1 dtex or more, more preferably 0.2 dtex or more.

[0045] The tensile strength of the flame-resistant polyphenylene ether fiber is preferably 0.8 cN / dtex or more, more preferably 0.85 cN / dtex or more, and further preferably 0.90 cN / dtex or more. By making the tensile strength within the aforementioned range, the handleability of the fiber becomes good, so it is preferred. In addition, the upper limit of the tensile strength is not particularly limited, preferably 50 cN / dtex or less, more preferably 40 cN / dtex or less.

[0046] When the flame resistant polyphenylene ether molded product is a flame resistant polyphenylene ether short fiber, the length thereof is not particularly limited and can be appropriately adjusted according to the intended use, but is usually 1 to 200 mm, preferably 2 to 180 mm, and more preferably 5 to 150 mm.

[0047] When the flame-resistant polyphenylene ether molded article is a flame-resistant polyphenylene ether nonwoven fabric, its unit area weight is not particularly limited and can be appropriately determined according to the purpose of using the nonwoven fabric. For example, 3 g / m 2 More preferably 5g / m 2 In addition, preferably 1000g / m 2 Below, more preferably 800g / m 2 the following.

[0048] The thickness of the flame-resistant polyphenylene ether nonwoven fabric is not particularly limited and can be appropriately determined depending on the purpose of using the nonwoven fabric. For example, it is preferably about 0.01 to 100 mm, and more preferably about 0.05 to 80 mm.

[0049] The tensile strength of the aforementioned fire-resistant polyphenylene ether nonwoven fabric is preferably 0.5 cN / 25 mm or more, more preferably 0.7 cN / 25 mm or more, and further preferably 1.0 cN / 25 mm or more. By making the tensile strength within the aforementioned range, the operability as a nonwoven fabric becomes good, so it is preferred. In addition, the upper limit of the tensile strength is not particularly limited, preferably 50 cN / 25 mm or less, more preferably 40 cN / 25 mm or less.

[0050] The fineness of the polyphenylene ether fiber forming the aforementioned flame-resistant polyphenylene ether nonwoven fabric is not particularly limited, and can be appropriately determined according to the purpose of using the nonwoven fabric, for example, preferably 100 dtex or less, more preferably 90 dtex or less, and further preferably 80 dtex or less. By making the fineness within the aforementioned range, the nonwoven fabric is flexible and easy to handle, so it is preferred. In addition, the lower limit of the fineness is not particularly limited, but is preferably 0.1 dtex or more, and more preferably 0.3 dtex or more.

[0051] When the flame-resistant polyphenylene ether molded article is a flame-resistant polyphenylene ether fabric, its weight per unit area is not particularly limited and can be appropriately determined according to the purpose of using the fabric. For example, 5 g / m 2 More preferably 10 g / m 2 In addition, preferably 2000g / m 2 Below, more preferably 1500g / m 2 the following.

[0052] The thickness of the flame-resistant polyphenylene ether fabric is not particularly limited and may be appropriately determined depending on the purpose of using the fabric. For example, the thickness is preferably 0.1 to 20 mm, and more preferably 0.2 to 18 mm.

[0053] The tensile strength of the flame-resistant polyphenylene ether fabric is preferably 1 cN / 25 mm or more, more preferably 2 cN / 25 mm or more, and further preferably 3 cN / 25 mm or more. The tensile strength is preferably within the above range, because the handling property of the fabric is good. The upper limit of the tensile strength is not particularly limited, but is preferably 5000 cN / 25 mm or less, and more preferably 4000 cN / 25 mm or less.

[0054] The fineness of the polyphenylene ether fiber forming the flame-resistant polyphenylene ether fabric is not particularly limited, and can be appropriately determined according to the purpose of using the fabric. For example, it is preferably 100 dtex or less, more preferably 90 dtex or less, and further preferably 80 dtex or less. When the fineness is within the above range, it is preferred because the fabric is flexible and easy to handle. In addition, the lower limit of the fineness is not particularly limited, but is preferably 0.1 dtex or more, and more preferably 0.3 dtex or more.

[0055] The flame-resistant polyphenylene ether molded article of the present invention is obtained by subjecting a polyphenylene ether molded article to a flame-resistant treatment. Hereinafter, the flame-resistant polyphenylene ether molded article will be described.

[0056] <Polyphenylene ether molded article>

[0057] The polyphenylene ether molded article used in the present invention contains a polyphenylene ether component.

[0058] The polyphenylene ether component is not particularly limited, and may be any of those commonly used in the art. Specifically, it may be any of the following general formula (1):

[0059]

[0060] (In formula (1), R 1 , R 2 are each independently a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms which may have a substituent, and R 3 each independently represents a hydrocarbon group having 1 to 10 carbon atoms which may have a substituent)

[0061] A homopolymer of the repeating unit shown, a copolymer containing two or more different repeating units of the general formula (1), or a copolymer having a repeating unit of the general formula (1) and a repeating unit other than the general formula (1).

[0062] As R in the above general formula (1) 1 , R 2For example, there can be mentioned a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, such as a methyl group, an ethyl group, a propyl group, an isopropyl group, a n-butyl group, an isobutyl group, a tert-butyl group, a pentyl group, a cyclopentyl group, a hexyl group, a cyclohexyl group, an octyl group, a decyl group, an aryl group having 6 to 10 carbon atoms, such as a phenyl group, a 4-methylphenyl group, a 1-naphthyl group, a 2-naphthyl group, and an aralkyl group having 7 to 10 carbon atoms, such as a benzyl group, a 2-phenylethyl group, a 1-phenylethyl group, and the like.

[0063] When the hydrocarbon group has a substituent, examples of the substituent include halogen atoms such as a fluorine atom, alkoxy groups such as a methoxy group, etc. Specific examples of the hydrocarbon group having a substituent include a trifluoromethyl group, etc.

[0064] Among them, as R 1 , R 2 , preferably a hydrogen atom or a methyl group, more preferably a hydrogen atom.

[0065] As R in the above general formula (1) 3 For example, alkyl groups having 1 to 10 carbon atoms, such as methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, tert-butyl, pentyl, cyclopentyl, hexyl, cyclohexyl, octyl and decyl, aryl groups having 6 to 10 carbon atoms, such as phenyl, 4-methylphenyl, 1-naphthyl and 2-naphthyl, and aralkyl groups having 7 to 10 carbon atoms, such as benzyl, 2-phenylethyl and 1-phenylethyl, can be mentioned.

[0066] When the hydrocarbon group has a substituent, examples of the substituent include halogen atoms such as a fluorine atom and alkoxy groups such as a methoxy group. Specific examples of the hydrocarbon group having a substituent include a trifluoromethyl group and the like.

[0067] Among them, as R 3 , preferably methyl.

[0068] Specific examples of the repeating unit of the general formula (1) include repeating units derived from 2,6-dimethyl-1,4-phenylene ether, 2,6-diethyl-1,4-phenylene ether, 2-methyl-6-ethyl-1,4-phenylene ether, and 2,6-dipropyl-1,4-phenylene ether. Among them, repeating units derived from 2,6-dimethyl-1,4-phenylene ether are preferred.

[0069] In addition, the polyphenylene ether may contain repeating units other than the general formula (1) as long as the effect of the present invention is not impaired. The content of repeating units other than the general formula (1) is not particularly limited as long as it is within the range that does not impair the effect of the present invention, and for example, it is preferably about 5 mol% or less in the copolymer, and more preferably does not contain.

[0070] The molecular weight of the polyphenylene ether is not particularly limited, but the weight average molecular weight (Mw) is preferably 40,000 to 100,000, more preferably 50,000 to 80,000. The number average molecular weight (Mn) is preferably 7,000 to 30,000, more preferably 8,000 to 20,000. The molecular weight distribution (Mw / Mn) is preferably 3.5 to 8.0, more preferably 4.0 to 6.0.

[0071] Polyphenylene ether generally has a high melt viscosity, and it is considered difficult to melt-mold in the case of high content of polyphenylene ether or in the case of single polyphenylene ether. Therefore, in the case of a process that requires melting polyphenylene ether when obtaining a polyphenylene ether molded body (such as melt spinning, etc.), it is preferred to use the following methods: a method of using a polyphenylene ether containing a polyphenylene ether component having a dislocation structure, a method of mixing a polyphenylene ether component having a high glass transition temperature with a polyphenylene ether component having a low glass transition temperature, etc. Through these methods, the melt viscosity of polyphenylene ether can be reduced, so that the melting of polyphenylene ether becomes possible, and a molded body such as melt-spun fiber, nonwoven fabric and film can be formed.

[0072] <<Polyphenylene ether having a dislocation structure>>

[0073] As the aforementioned polyphenylene ether having a dislocation structure, for example, it is preferable to form a polyphenylene ether having the following general formula (2):

[0074]

[0075] (In formula (2), R 1 , R 2 are each independently a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms which may have a substituent, and R 3 Each independently represents a hydrocarbon group having 1 to 10 carbon atoms which may have a substituent, R 3’ From the above R 3 A divalent group obtained by removing one hydrogen atom from

[0076] The polyphenylene ether of the polyphenylene ether component having the dislocation structure shown above. By having such a dislocation structure, the fluidity is improved to the extent that melt molding is possible, and melt-spun fibers, nonwoven fabrics, films, etc. can be formed.

[0077] As R in the above general formula (2) 1 ~R 3 , and the same substances as those of the above-mentioned general formula (1) can be exemplified. The "~" in the above-mentioned general formula (2) indicates that the structure before it is not particularly limited. The "~" part can be formed by phenyl ether units connected by para bonds, and in addition, it can have a part partially bonded by ortho bonds.

[0078] The aforementioned R 3’ Indicates that from the above R 3The divalent group obtained by removing one hydrogen atom from the group consisting of is preferably a methylene group.

[0079] The polyphenylene ether component having a dislocation structure preferably has a dislocation structure represented by the general formula (2) in a homopolymer having a repeating unit of the general formula (1), a copolymer containing two or more different repeating units of the general formula (1), or a copolymer containing a repeating unit of the general formula (1) and a repeating unit other than the general formula (1).

[0080] The amount of dislocation structure in the aforementioned polyphenylene ether component having a dislocation structure is not particularly limited, and is preferably 0.1 mol% or more, more preferably 0.12 mol% or more, further preferably 0.15 mol% or more, and particularly preferably 0.2 mol% or more relative to all polyphenylene ether structural units in the aforementioned polyphenylene ether component. In order to further stably discharge, it is preferably 0.3 mol% or more. In addition, the upper limit of the amount of dislocation structure is not particularly limited, and is preferably 10 mol% or less, more preferably 9 mol% or less. By making the amount of dislocation structure in the polyphenylene ether component having a dislocation structure within the aforementioned range, the fluidity is improved to the extent that melt molding can be performed, and a melt extrusion molded body tends to be formed, so it is preferred.

[0081] The polyphenylene ether having a dislocation structure preferably has free radicals in the polymer. In addition, the amount of free radicals in the polyphenylene ether is preferably 100 g -1 More than 120g -1 More than 150g is more preferred -1 By making the free radical amount of the above polyphenylene ether 100g -1 In addition, the upper limit of the amount of free radicals in the polyphenylene ether is not particularly limited, but from the viewpoint of oxidative degradation, it is preferably 10000 g / cm2. -1 Below, more preferably 9000g -1 Below, more preferably 8000g -1 the following.

[0082] The method for forming the polyphenylene ether component having a dislocation structure is described below.

[0083] The method of mixing a polyphenylene ether component having a high glass transition point and a polyphenylene ether component having a low glass transition point to reduce the melt viscosity will be described as a method for producing a polyphenylene ether molded article.

[0084] <Ingredients other than polyphenylene ether components>

[0085] The polyphenylene ether molded article used in the present invention may contain resin components other than the aforementioned polyphenylene ether components. Examples of resin components other than polyphenylene ether include polyamides such as styrene, polyethylene, polypropylene, polyamide 4, polyamide 6, polyamide 10, polyamide 11, polyamide 66, polyamide 6T, and polyamide 6T / 11, polyesters such as polyethylene terephthalate and polybutylene terephthalate, and polycarbonate. Among them, the content is preferably 5% by mass or less, more preferably 2% by mass or less, and even more preferably not contained (0% by mass).

[0086] Furthermore, additives such as lubricants, plasticizers, antioxidants, ultraviolet absorbers, gelling agents, and antistatic agents may be added to the polyphenylene ether molded article as long as the effects of the present invention are not impaired.

[0087] <Polyphenylene ether content>

[0088] In addition, in the polyphenylene ether molded article used in the present invention, the content of polyphenylene ether is preferably 95% by mass or more, more preferably 98% by mass or more, and further preferably substantially only polyphenylene ether (100% by mass) in the total components forming the molded article. By making the content of the polyphenylene ether in the polyphenylene ether molded article within the above range, the obtained molded article not only has excellent mechanical strength, but also has excellent heat resistance, chemical resistance, flame retardancy, etc., which is preferred.

[0089] <Method for producing polyphenylene ether molded article>

[0090] <<Polyphenylene ether fiber>>

[0091] When the polyphenylene ether molded product is a polyphenylene ether fiber, the polyphenylene ether fiber can be produced by various production methods such as melt spinning, dry spinning, wet spinning, etc. Among them, melt spinning is preferred because productivity can be improved.

[0092] use Figure 1 An example of producing polyphenylene ether melt-spun fibers is described below. Figure 1 The hopper 1 is put into an extruder 2 having a barrel and a screw, and the molten polyphenylene ether is discharged at a metering rate by a gear pump 3, and is discharged from a spinning nozzle 5 through a filter material 4 composed of fine sand, etc., to obtain a melt-spun fiber. In addition, a filter 6 composed of a metal nonwoven fabric, etc. is preferably provided on the filter material 4. By providing the filter 6, foreign matter can be removed in advance, and clogging of the filter material 4 can be prevented, etc., so it is preferred.

[0093] In addition, from the viewpoint of suppressing nozzle clogging due to oxidative crosslinking, it is preferred to provide a heat-retaining space 7 directly below the spinning nozzle 5, introduce an inert gas 8 such as nitrogen into the region and perform spinning, and it is more preferred to introduce heated inert gas using a heating torch 9. The temperature of the heated inert gas is preferably 100 to 500° C., more preferably 200 to 400° C.

[0094] The spinning speed is not particularly limited and can be appropriately set according to the desired fineness, etc., but is preferably about 100 to 400 m / min, more preferably about 100 to 200 m / min, in order to stably obtain fine-fine fibers.

[0095] The single hole discharge of the spinning nozzle is preferably 0.4 g / min or less, more preferably 0.3 g / min or less, and further preferably 0.2 g / min or less. In addition, the lower limit of the single hole discharge is not particularly limited, but is preferably 0.05 g / min or more, more preferably 0.1 g / min or more, and further preferably 0.12 g / min or more. By setting the single hole discharge to the above range, fine polyphenylene ether fibers can be obtained, which is preferred.

[0096] Examples of the polyphenylene ether as a raw material include homopolymers having repeating units of the general formula (1), copolymers containing two or more different repeating units of the general formula (1), and copolymers having repeating units of the general formula (1) and repeating units other than the general formula (1). Examples of the content of repeating units other than the general formula (1) in the copolymer include those mentioned above. Among them, homopolymers having repeating units of the general formula (1) are preferred.

[0097] Specific examples of the homopolymer having a repeating unit of the general formula (1) include poly(2,6-dimethyl-1,4-phenylene ether), poly(2,6-diethyl-1,4-phenylene ether), poly(2-methyl-6-ethyl-1,4-phenylene ether), poly(2,6-dipropyl-1,4-phenylene ether), and the like. Among them, poly(2,6-dimethyl-1,4-phenylene ether) is preferred.

[0098] As the poly(2,6-dimethyl-1,4-phenylene ether), commercially available products may be preferably used, and specific examples thereof include PPO640, PPO646, and PPOSA120 manufactured by SABIC Innovative Plastics, and ZYLON S201A and ZYLON S202A manufactured by Asahi Kasei Chemicals Corporation.

[0099] Furthermore, when the polyphenylene ether as a raw material is melted, the melt viscosity can be reduced by mixing a polyphenylene ether component having a high glass transition point and a polyphenylene ether component having a low glass transition point.

[0100] The glass transition temperature of the polyphenylene ether component having a high glass transition temperature is preferably 170° C. or higher, more preferably 200° C. or higher, and further preferably 210° C. or higher. In addition, the upper limit of the glass transition temperature is preferably 230° C. or lower. By setting the glass transition temperature of the polyphenylene ether component having a high glass transition temperature to be within the above range, a polyphenylene ether molded product having high heat resistance can be obtained, which is preferred.

[0101] The glass transition temperature of the polyphenylene ether component having a low glass transition temperature is preferably lower than 170° C. By adding a polyphenylene ether component having a glass transition temperature lower than 170° C., the melt viscosity is reduced and the fluidity is improved.

[0102] The content of the polyphenylene ether component having a glass transition temperature of 170° C. or more is preferably 70% by mass or more, more preferably 80% by mass or more, and further preferably 90% by mass or more in the polyphenylene ether as a raw material. In addition, the upper limit of the content of the polyphenylene ether component having a glass transition temperature of 170° C. or more is not particularly limited, but is preferably 100% by mass or less. In the present invention, when a polyphenylene ether component having a high glass transition temperature (i.e., a high molecular weight) is included in the aforementioned range, the obtained polyphenylene ether melt-extruded molded product has excellent mechanical strength, heat resistance, chemical resistance, flame retardancy, etc., so it is preferred.

[0103] In addition, the polyphenylene ether as a raw material, and resin components and additives other than the polyphenylene ether component may be simultaneously included. The resin components and additives other than the polyphenylene ether component are as described above. In addition, the content of the resin component other than the polyphenylene ether component in the raw material is preferably 5% by mass or less, more preferably 2% by mass or less, and further preferably does not contain (0% by mass).

[0104] As the extruder having a barrel and a screw, a single-screw extruder or a twin-screw extruder commonly used in the art can be used. In the present invention, a twin-screw extruder is preferably used.

[0105] The peripheral speed of the screw is not particularly limited and can be set to a range commonly used in the art. However, when a polyphenylene ether having a dislocation structure is used to form a molded body, the peripheral speed of the screw must be a peripheral speed that causes a dislocation reaction of the polyphenylene ether as a raw material. In addition, the amount of free radicals in the polyphenylene ether having a dislocation structure is 100 g. -1Based on the above viewpoints, the circumferential speed of the screw is preferably 3.6 m / min or more, more preferably 3.7 m / min or more, and further preferably 3.8 m / min or more. In addition, the upper limit of the circumferential speed of the screw is not particularly limited, and is preferably 94.2 m / min or less. In the present invention, by increasing the screw speed to make the circumferential speed of the screw above 3.6 m / min, a high shear force can be applied to the raw material polyphenylene ether in the barrel, thereby cutting the molecular chain of the polyphenylene ether and generating free radicals. As a result, a free radical amount of 100 g -1 The above-mentioned polyphenylene ether having a dislocation structure. By forming the above-mentioned polyphenylene ether having a dislocation structure, the polyphenylene ether can be melt-extruded.

[0106] If the temperature in the barrel is too low, the fluidity of the resin is poor, and if it is too high, the fluidity is improved, but foaming due to thermal decomposition of the resin occurs, so it is necessary to select a processing temperature that strikes a balance. The temperature in the barrel is, for example, preferably 250 to 350°C, more preferably 280 to 330°C.

[0107] <<Polyphenylene ether staple fiber>>

[0108] The polyphenylene ether staple fibers can be obtained, for example, by cutting the aforementioned polyphenylene ether fibers into short tow-like fibers.

[0109] <<Polyphenylene ether nonwoven fabric>>

[0110] The method for producing the polyphenylene ether nonwoven fabric is not particularly limited, and a method commonly used in the art can be suitably adopted. The method for producing the nonwoven fabric includes, for example, spunbonding, meltblowing, spunlacing, needlepunching, thermal bonding, chemical bonding, etc. Among them, spunbonding is preferred.

[0111] As raw materials and the like used for forming the polyphenylene ether nonwoven fabric, the same ones as those described for the polyphenylene ether fibers can be used.

[0112] <<Polyphenylene ether fabric>>

[0113] The polyphenylene ether fabric is formed of the aforementioned polyphenylene ether fiber. The aforementioned fabric may further include: one or more fibers selected from the group consisting of wholly aromatic polyester fibers, polybenzoxazole (PBO) fibers, polybenzimidazole (PBI) fibers, polybenzothiazole (PBTZ) fibers, polyimide (PI) fibers, polysulfoneamide (PSA) fibers, polyetheretherketone (PEEK) fibers, polyetherimide (PEI) fibers, polyarylate (PAr) fibers, melamine fibers, phenolic fibers, fluorine-based fibers, polyphenylene sulfide (PPS) fibers, cellulose fibers, polyolefin fibers, acrylic fibers, rayon fibers, cotton fibers, animal hair fibers, polyurethane fibers, polyvinyl chloride fibers, polyvinylidene chloride fibers, acetate fibers, and polycarbonate fibers.

[0114] The ratio of the polyphenylene ether fiber contained in the polyphenylene ether fabric is, for example, 50 to 100 mass %, preferably 55 to 98 mass %, more preferably 60 to 95 mass %, and further preferably 65 to 90 mass %, from the viewpoint of mechanical strength, flame retardancy, heat resistance, high temperature stability, chemical resistance, etc.

[0115] The polyphenylene ether fabric can be produced by a common method. For example, a method is exemplified in which short-staple yarns of the above-mentioned fibers are blended with cotton to obtain short-staple yarns, and then the short-staple yarns are woven into a twill or plain weave using a rapier loom or the like with single or double yarns.

[0116] <<Other molded products>>

[0117] As mentioned above, as the refractory polyphenylene ether molded body of the present invention, representative examples include refractory polyphenylene ether fibers, refractory polyphenylene ether nonwoven fabrics, or refractory polyphenylene ether fabrics, but for example, refractory polyphenylene ether films, etc. can also be mentioned. As their manufacturing methods, they can be manufactured by methods commonly used in the art. It should be noted that each measurement method recorded in the embodiment records the measurement method for refractory PPE fibers and refractory PPE films, but the measurement method recorded in the embodiment can also be applied to the molded bodies such as refractory PPE nonwoven fabrics and refractory PPE fabrics and measured.

[0118] 2. Method for producing fire-resistant polyphenylene ether molded body

[0119] The method for producing a flame-resistant polyphenylene ether molded body of the present invention is characterized in that the polyphenylene ether molded body is heat-treated in air at 120 to 240° C. for 1 to 30 hours to be infusible (infusibility treatment), and further heat-treated in air at 260 to 400° C. for 0.1 to 10 hours to be flame-resistant (fire-resistant treatment).

[0120] As the polyphenylene ether molded article, those described above can be preferably used.

[0121] In the aforementioned infusibility treatment, the polyphenylene ether molded body is treated in air at 120 to 220° C. for 1 to 30 hours. Here, in air refers to an environment that is not particularly adjusted. In addition, the treatment temperature is 120 to 240° C., preferably 140 to 230° C., and more preferably 160 to 220° C. In addition, the treatment time is 1 to 30 hours, preferably 1.5 to 25 hours, and more preferably 2 to 20 hours. By setting the aforementioned treatment time and treatment temperature, the polyphenylene ether molded body will not melt in the subsequent refractory treatment, and an appropriate refractory treatment can be implemented.

[0122] After the aforementioned infusibility treatment, as a fire-resistant treatment, the polyphenylene ether is treated at 260 to 400° C. in air for 0.1 to 10 hours. In air refers to an environment that has not been specially adjusted. In addition, the treatment temperature is 260 to 400° C., preferably 270 to 380° C., and more preferably 280 to 360° C. In addition, the treatment time is 0.1 to 10 hours, preferably 0.3 to 8 hours, and more preferably 0.5 to 6 hours. By setting the aforementioned treatment time and treatment temperature, a C=O bond structure is formed in the polyphenylene ether molded body, and a fire-resistant molded body showing very high flame retardancy, fire resistance, heat resistance, etc. can be formed.

[0123] <Application>

[0124] The flame-resistant polyphenylene ether short fibers can be used, for example, for heat-resistant adhesives, C / C composites, industrial brushes, brake materials, and the like.

[0125] The aforementioned fire-resistant polyphenylene ether non-woven fabric can be used, for example, for automobile sound-absorbing materials, automobile interior materials, heat-insulating materials, household fire-extinguishing cloths, fireproof covers, pipe surface materials, plastic fireproof materials, anti-spreading materials, anti-dust dispersion surface materials, cement reinforcement materials, friction materials, gland packings, sealing materials, fire-fighting clothing, welding spark protection sheets, etc.

[0126] The flame-resistant polyphenylene ether fabric can be used, for example, for heat insulating materials, work clothes (for firefighting, competition, and pilots), heat-resistant gloves, disaster prevention headbands, interior materials for transportation equipment, heat-resistant clothing, and electromagnetic wave shielding materials.

[0127] Example

[0128] The present invention will be described in more detail below by showing examples and comparative examples, but the present invention is not limited to the following examples. It should be noted that the evaluation methods of physical properties and the like in the following examples are as follows.

[0129] (1) Dislocation structure in the molded body

[0130] With a resonant frequency of 600MHz 1H-NMR measurement was performed using an NMR device manufactured by BRUKER (device name: AVANCE-NEO600), and the measurement was performed as follows.

[0131] After dissolving 10 mg of the molded body (sample) obtained in the examples and comparative examples in deuterated chloroform, the solution was filled into an NMR tube for measurement within 1 hour. Deuterated chloroform was used as the blocking solvent, the waiting time was set to 1 second, the data collection time was set to 4 seconds, and the number of accumulations was set to 64 times.

[0132] The analysis of the dislocation structure amount was carried out as follows.

[0133] The R from the 3 and 5 positions of polyphenylene ether 1 , R 2 The peak of the proton of the base is the same as that of the R 3’ The peak integration values ​​of the proton peaks of the divalent groups (methylene and the like) shown are designated as A and B, and the dislocation structure amount is determined by the following formula.

[0134] Dislocation structure amount (mol%) = {B / (A+B)}×100

[0135] (2) Free radical amount

[0136] The amount of free radicals in the polyphenylene ether was measured under the following conditions using an electron spin resonance device (ESR, manufactured by JEOL Ltd., JES-FA100). 3 However, depending on the shape of the sample, it is not possible to fill 0.1 g of sample without falling into the range of 0.1 to 0.2 g / cm 3 In the case of the range of 0.2 g / cm 3 The free radical amount was calculated according to the following formula.

[0137] Normalized intensity of sample = signal intensity of sample / manganese intensity

[0138] Normalized intensity of blank = signal intensity of blank / manganese intensity

[0139] Free radical amount = (standardized intensity of sample - standardized intensity of blank) / sample weight

[0140] (Measurement conditions)

[0141] Sample tube: EPW-005J (made by Sigemi)

[0142] Manganese strength: Secondary integrated value in the range of 320 to 322 mT

[0143] Signal intensity of sample and blank: 2nd integrated value in the range of 322.1 to 329.3 mT

[0144] Magnetic field: 325.8±7.5mT

[0145] Microwave power: 0.1mW

[0146] Scan time: 4 minutes

[0147] Modulation width: 0.12mT

[0148] Amplitude: 1000

[0149] Time constant: 0.3 seconds

[0150] Mn mark: 800

[0151] Scans: 2

[0152] (3) Specific gravity

[0153] A dry type automatic density meter (product name: AccuPyc II1340, manufactured by Shimadzu Corporation) was used to measure the density of the sample at 10 cm 3 The cuvette is filled with the sample to about 80% of its capacity, and the measurement is performed in helium gas.

[0154] (4) Fineness

[0155] The thickness was measured by the method described in JIS L-1095 9.4.1.

[0156] (5) Tensile strength and tensile elongation

[0157] The test was performed in accordance with JIS L1013 8.5.1. In the case of fibers, single fibers were evaluated and the test was performed at a chuck spacing of 10 mm and a tensile speed of 10 mm / min. In the case of nonwoven fabrics, samples were taken with a width of 25 mm and a length of 100 mm and the test was performed at a chuck spacing of 50 mm and a tensile speed of 100 mm / min. The tensile elongation was set to the elongation at which the strength reached the maximum.

[0158] (6) Absorbance height ratio (A / B)

[0159] The fibers obtained in Examples 1 to 7 and Comparative Examples 1 to 7 were powdered in a mortar and mixed with KBr to form tablets to be used as measurement samples. The films obtained in Examples 8 to 11 were used as measurement samples as they were.

[0160] The absorbance of the obtained sample was measured by a microscopic transmission method under the following conditions using an infrared spectrophotometer (FTIR) (product name: 3100FT-IR / 600UMA, manufactured by Varian).

[0161] (Measurement conditions)

[0162] Field of view: 80mm×80mm

[0163] Measurement wavelength range: 400cm -1 Up to 4000cm -1

[0164] Cumulative times: 128 times

[0165] Resolution: 4cm -1

[0166] Plot the obtained spectrum, connecting the wavelengths 1550-1480cm -1 The minimum value and 1900~1800cm -1 The minimum value baseline is used as the evaluation method, and the peak height (peak absorbance height) from the baseline is used for evaluation.

[0167] 1742~1722cm -1 The peak height of the absorbance is set as A, 1610-1590cm -1 The peak height of is set as absorbance height B, which is defined by the value of A / B.

[0168] (7) Difference in weight loss rate

[0169] Using a thermogravimetric apparatus (product name: TGA Q50, manufactured by TA INSTRUMENTS), 10 mg of the sample was filled into an aluminum pan, the temperature was raised from 20°C to 480°C at 20°C / min, and the weight at 150°C and the weight at 400°C were measured. Then, the weight loss rate (%) at 150°C and the weight loss rate (%) at 400°C relative to the initial weight at 20°C were determined according to the following formula, and the difference between them was calculated.

[0170] Weight loss rate at 150°C (%) = {(initial weight at 20°C - weight at 150°C) / initial weight at 20°C} × 100

[0171] Weight loss rate at 400°C (%) = {(initial weight at 20°C - weight at 400°C) / initial weight at 20°C} × 100

[0172] (8) 400℃ strength retention

[0173] The strength of each sample was measured by the method described in "(3) Tensile strength and tensile elongation" above after being placed in an oven at 400°C for 10 minutes. The 400°C strength retention was calculated using the following formula.

[0174] 400℃ strength retention rate (%) = (sample strength after treatment / sample strength before treatment) × 100

[0175] (9) 400℃ elongation retention

[0176] The elongation of the sample after placing it in an oven at 400° C. for 10 minutes was measured by the method described in “(3) Tensile Strength and Tensile Elongation” above, and the 400° C. elongation retention was calculated by the following formula.

[0177] 400℃ elongation retention rate (%) = (elongation of sample after treatment / elongation of sample before treatment) × 100

[0178] (10) LOI value (flame retardancy)

[0179] The oxygen index is determined by JIS L 1091E method. When the combustion lasts for more than 50 mm, propane gas is used as the heat source of the igniter. The fiber is made into short fibers of about 5 mm, dispersed in water and made into paper, and processed by hot calender at 220°C. The size is a circle with a diameter of 25 mm and a unit area weight of 140 g / m 2 The nonwoven fabric was evaluated directly without any processing.

[0180] (11) Flame contact test

[0181] (11-1) Self-extinguishing

[0182] The sample flame was exposed to the burner for 10 seconds, and after the flame was removed, the flame was evaluated to see whether it disappeared. Methane gas was used as the gas. If the flame disappeared within 10 seconds, it was evaluated as self-extinguishing (0), and if the flame did not disappear within 10 seconds, it was evaluated as non-self-extinguishing (×).

[0183] (11-2) Shrinkage / deformation

[0184] The sample was exposed to the flame of the burner for 10 seconds, and after the flame was removed, the sample was evaluated for shrinkage / deformation. Methane gas was used as the gas. The sample was evaluated as 0 if it did not shrink / deform, and as × if it did shrink / deform.

[0185] (12) Shrinkage at 350℃

[0186] Each flame-resistant polyphenylene ether fiber sample was placed in an oven at 350° C., and the dimensions of the sample after 1 hour were measured with a vernier caliper. The 350° C. shrinkage rate was determined from the following formula.

[0187] 350°C shrinkage (%) = 100 - {(size of sample after heat treatment / size of sample before heat treatment) × 100}

[0188] <Fire-resistant polyphenylene ether fiber>

[0189] Example 1

[0190] Poly(2,6-dimethyl-1,4-phenylene oxide) (PPO640, glass transition temperature (Tg): 221°C, manufactured by SABIC Innovative Plastics) was extruded using a twin-screw extruder manufactured by Technovel Corporation (product name: KZW15TW-30MG). The twin-screw extruder was as follows: the barrel had 4 zones, and the barrels were set as barrels 1, 2, 3, and 4 from the hopper side, respectively, barrels 1 to 3 were set to 280°C, barrel 4 and the barrel head were set to 300°C, the screw rotation speed was set to 700 rpm, and the peripheral speed of the screw was set to 33.0 m / min.

[0191] A gear pump is set downstream of the extruder to measure the discharge rate of the polymer, and it is extruded to a nozzle (nozzle hole diameter: 0.45 mm, nozzle hole pad length: 1.35 mm, number of nozzle holes: 48) with the help of a metal non-woven filter (product name: NF-07, manufactured by Nippon Seisen Co., Ltd.) (total discharge: 10.15 g / min, single hole discharge: 0.211 g / min). A surface heater is arranged directly under the nozzle, and the nozzle temperature is set to 316°C. A 60mm insulation space is set directly under the nozzle, and nitrogen heated to 400°C is continuously introduced into this area. The polymer discharged from the nozzle is wound at a spinning speed of 95 m / min. The obtained fiber has a dislocation structure (dislocation structure amount: 2.7 mol% relative to all PPE units), and the amount of free radicals remaining in the fiber is 410 g. -1 .

[0192] The fibers thus obtained were divided and heat-treated in air at 200°C for 2 hours (infusibility treatment) in a manner that the fibers were not fused, and then heated to 280°C at 1°C / min and heat-treated in air at 280°C for 2 hours (refractory treatment) to refractory the fibers. The refractory polyphenylene ether fibers obtained had a specific gravity of 1.42 and a fineness of 26.1 dtex.

[0193] When the obtained fire-resistant polyphenylene ether fiber was measured by infrared spectroscopy, the -1 A peak derived from C=O stretching vibration was observed. In addition, the wave number derived from C=O stretching vibration is 1732 cm -1 The absorbance height A is related to the wavelength of 1600 cm-1, which is derived from the skeleton vibration caused by the stretching between carbon atoms in the benzene ring. -1 The absorbance height ratio (A / B) of the absorbance height B was 0.65. The evaluation results are shown in Tables 1 and 2.

[0194] Examples 2 to 6, Comparative Example 1

[0195] Flame-resistant polyphenylene ether fibers were produced in the same manner as in Example 1 except that the type of raw material PPE used and the flame-resistant treatment conditions were changed as shown in Table 1. The evaluation results are shown in Tables 1 and 2.

[0196] Example 7

[0197] Using EBC300 (NMV Corporation), the fiber spun in the same manner as in Example 1 was irradiated with an electron beam 20 times under the conditions of an accelerating voltage of 200 kV and an electron beam dose of 100 kGy. The irradiation atmosphere was carried out in a nitrogen atmosphere. After that, a heat treatment (infusibility treatment) at 180°C for 16 hours was performed, and then the temperature was raised to 280°C at 1°C / min, and a heat treatment (refractory treatment) at 280°C for 2 hours was performed in air to refractory the fiber, thereby producing a refractory polyphenylene ether fiber. The evaluation results are shown in Table 1. The specific gravity of the refractory polyphenylene ether film produced was 1.53, and the refractory treatment was fully performed.

[0198] Comparative Example 2

[0199] Various evaluations were performed using the polyphenylene ether melt-spun fibers (without flame retardant treatment) obtained in Example 1. Table 1 shows the evaluation results.

[0200] Comparative Example 3

[0201] Various evaluations were performed using para-aramid fibers (product name: Kevlar, manufactured by DUPONT-TORAY) (without flame retardant treatment). The evaluation results are shown in Table 1.

[0202] Comparative Example 4

[0203] Various evaluations were performed using single fibers of acrylonitrile (PAN)-based flame-resistant nonwoven fabric (product name: NEW LASTAN TOP5150Z, manufactured by Asahi Kasei Corporation). The evaluation results are shown in Table 1.

[0204] Comparative Example 5

[0205] Various evaluations were performed using Novoloid fibers (product name: Kynol, manufactured by Gunei Chemical Industry Co., Ltd.). Table 1 shows the evaluation results.

[0206] Comparative Example 6

[0207] Polyphenylene ether fibers were produced in the same manner as in Example 1 except that only the infusibility treatment (heat treatment at 180° C. for 16 hours) was performed without the flame retardant treatment (heat treatment at 280° C. for 2 hours).

[0208] Comparative Example 7

[0209] The same treatment as in Example 1 was performed except that the infusibility treatment (heat treatment at 200°C for 2 hours) was not performed and only the refractory treatment (heat treatment at 280°C for 2 hours) was performed. However, the polyphenylene ether fiber melted during the refractory treatment and no refractory fiber was obtained.

[0210] [Table 1]

[0211]

[0212] [Table 2]

[0213]

[0214] <Fire-resistant polyphenylene ether film>

[0215] Example 8

[0216] Poly(2,6-dimethyl-1,4-phenylene oxide) (PPO640, glass transition temperature (Tg): 221° C., manufactured by SABIC Innovative Plastics) was extruded using a twin-screw extruder manufactured by Technovel Corporation (product name: KZW15TW-45MG). The twin-screw extruder was set to 320° C., the screw speed was set to 150 rpm, and the screw peripheral speed was set to 7.1 m / min.

[0217] A gear pump was set at the downstream of the extruder to measure the discharge rate of the polymer, and the polymer was extruded into a T-die (TDS / 150-SGI) manufactured by Technovel Corporation at a discharge rate of 5.0 g / min. The polymer extruded from the T-die was taken up with a roll (FPU-200-SGI) manufactured by Technovel Corporation at a pulling speed of 3.3 m / min to produce a molten polyphenylene ether film. The amount of free radicals remaining in the obtained film was 1600 g. -1 After that, the obtained film was subjected to heat treatment (infusibility treatment) at 200°C for 2 hours in air, and then the temperature was raised to 280°C at 1°C / min, and heat treated (fire-resistant treatment) at 280°C for 2 hours in air to produce a fire-resistant polyphenylene ether film. The evaluation results are shown in Table 3. The specific gravity of the manufactured fire-resistant polyphenylene ether film was 1.27, and the fire-resistant treatment was fully carried out.

[0218] Examples 9 and 10

[0219] The flame resistant polyphenylene ether film was produced in the same manner as in Example 8 except that the production conditions were changed to those described in Table 3. The evaluation results are shown in Table 3. The specific gravity of the flame resistant polyphenylene ether film of Example 9 was 1.25, and the specific gravity of the flame resistant polyphenylene ether film of Example 10 was 1.29, indicating that the flame resistant was fully achieved.

[0220] Embodiment 11

[0221] The film prepared in the same manner as in Example 10 was irradiated with electron beams 20 times using EBC300 (NMV Corporation) at an accelerating voltage of 200 kV and an electron beam dose of 100 kGy. The irradiation atmosphere was nitrogen. Afterwards, the film was subjected to refractory treatment in the same manner as in Example 8 to produce a refractory polyphenylene ether film. The evaluation results are shown in Table 3. The specific gravity of the refractory polyphenylene ether film was 1.35, and refractory treatment was fully performed.

[0222] [Table 3]

[0223]

[0224] In addition, "PPO640" in Tables 1 and 3 refers to poly(2,6-dimethyl-1,4-phenylene oxide) (PPO640, glass transition temperature (Tg): 221°C, manufactured by SABIC Innovative Plastics), "SA120" refers to poly(2,6-dimethyl-1,4-phenylene oxide) (PPOSA120, glass transition temperature (Tg): 159°C, manufactured by SABIC Innovative Plastics), "para-aramid" refers to para-aramid fiber (product name: Kevlar, manufactured by DUPONT-TORAY), "flame-resistant PAN" refers to single fiber of acrylonitrile-based flame-resistant nonwoven fabric (product name: NEW LASTAN TOP5150Z, manufactured by Asahi Kasei Corporation), and "Novoloid" refers to Novoloid fiber (product name: Kynol, manufactured by Gunei Chemical Industry Co., Ltd.).

[0225] As shown in Table 1, the flame-resistant polyphenylene ether fiber of the present invention has a very high LOI value and is also excellent in the flame contact test. In addition, the difference in weight loss rate between 150°C and 400°C is also small, and the strength retention rate and elongation retention rate at 400°C are also very high. In addition, the specific gravity of the flame-resistant polyphenylene ether fiber of the present invention is 1.37 or more, and the flame resistant is fully performed. On the other hand, the flame-resistant polyphenylene ether fiber of Comparative Example 1 with a specific gravity of 1.19 has excellent self-extinguishing properties in the flame contact test, but causes shrinkage / deformation, which is insufficient. The weight loss rate difference of the unfire-resistant polyphenylene ether fiber of Comparative Example 2 is small, but the strength retention rate, elongation retention rate, LOI value and flame contact test at 400°C are poor and insufficient. The untreated para-aramid fiber of Comparative Example 3 is also insufficient in various evaluations. In addition, the flame-resistant acrylonitrile (PAN) fiber of Comparative Example 4 was excellent in the flame contact test, but the weight loss rate difference was large, and the elongation retention rate at 400°C was poor and insufficient. In the cured Novoloid fiber of Comparative Example 5, it was excellent in the flame contact test, but all other evaluations were poor. In addition, in the fiber of Comparative Example 6 that made the PPE fiber infusible, the self-extinguishing property was excellent in the flame contact test, but it caused shrinkage / deformation, which was insufficient. In addition, in Comparative Example 7, the infusibility treatment was not performed before the flame-resistant treatment, so the polyphenylene ether fiber melted during the flame-resistant treatment and could not be evaluated.

[0226] As shown in Table 3, the flame-resistant polyphenylene ether film of the present invention has a specific gravity of 1.25 or more, is sufficiently flame-resistant, and is also very excellent in the flame contact test.

[0227] Description of Reference Numerals

[0228] 1 Hopper

[0229] 2 Extruder

[0230] 3 Gear pump

[0231] 4 Filters

[0232] 5 Spinning nozzle

[0233] 6 Filter Material

[0234] 7 Insulation space

[0235] 8 Introduction of inert gas

[0236] 9 Heating torch

Claims

1. A fire-resistant polyphenylene ether molded body, characterized in that: In the measurement based on infrared spectroscopy, the wave number from C=O stretching vibration is 1732 cm -1 The absorbance height A is related to the wavelength of 1600 cm-1, which is derived from the skeleton vibration caused by the stretching between carbon atoms in the benzene ring. -1 The absorbance height ratio (A / B) of the absorbance height B is 0.42 or more, and the specific gravity of the flame-resistant polyphenylene ether molded body is 1.25 or more.

2. The flame-resistant polyphenylene ether molded body according to claim 1, characterized in that: The difference between the weight loss rate (%) at 150°C and the weight loss rate (%) at 400°C relative to the initial weight at 20°C is 5.0% or less.

3. The flame-resistant polyphenylene ether molded body according to claim 1, characterized in that: LOI value is 35 or above.

4. The flame-resistant polyphenylene ether molded body according to claim 1, characterized in that: The strength retention rate at 400°C is 40% or more.

5. The flame-resistant polyphenylene ether molded body according to claim 1, characterized in that: The fire-resistant polyphenylene ether molded body is a fire-resistant polyphenylene ether fiber.

6. The flame-resistant polyphenylene ether molded body according to claim 5, characterized in that: The fineness is less than 100 dtex.

7. The flame-resistant polyphenylene ether molded body according to claim 5 or 6, characterized in that: The fire-resistant polyphenylene ether fiber is a fire-resistant polyphenylene ether short fiber.

8. The flame-resistant polyphenylene ether molded body according to any one of claims 1 to 4, characterized in that The fire-resistant polyphenylene ether molded body is a fire-resistant polyphenylene ether non-woven fabric.

9. The flame-resistant polyphenylene ether molded body according to claim 8, characterized in that: The fineness of the polyphenylene ether fibers forming the flame-resistant polyphenylene ether nonwoven fabric is 100 dtex or less.

10. The flame-resistant polyphenylene ether molded body according to any one of claims 1 to 4, characterized in that The fire-resistant polyphenylene ether molded body is a fire-resistant polyphenylene ether cloth.

11. The flame-resistant polyphenylene ether molded article according to any one of claims 1 to 4, characterized in that The fire-resistant polyphenylene ether molded body is a fire-resistant polyphenylene ether film.

12. A method for producing a flame-resistant polyphenylene ether molded body according to any one of claims 1 to 11, characterized in that: The polyphenylene ether molded body is heat treated in air at 120 to 240° C. for 1 to 30 hours to be infusible, and further heat treated in air at 260 to 400° C. for 0.1 to 10 hours to be flame-resistant.

13. The method for producing a flame-resistant polyphenylene ether molded body according to claim 12, characterized in that: The free radical amount of the polyphenylene ether molded body is 100g -1 above.

14. The method for producing a flame-resistant polyphenylene ether molded body according to claim 12 or 13, characterized in that: The polyphenylene ether molded body is polyphenylene ether fiber.

15. The method for producing a flame-resistant polyphenylene ether molded body according to claim 12 or 13, characterized in that: The polyphenylene ether molded body is a polyphenylene ether nonwoven fabric.

16. The method for producing a flame-resistant polyphenylene ether molded body according to claim 12 or 13, characterized in that: The polyphenylene ether molded body is a polyphenylene ether cloth.