A method for preparing a skin contact thermotherapy electrode

By using aramid nanofiber-gold composite electrode, the skin discomfort caused by airtightness of existing thermal therapy equipment and the large size of traditional devices is solved, and a light, breathable, efficient heating of the touch-free skin contact thermal therapy electrode is achieved. It is suitable for Wearing app.

CN115844623BActive Publication Date: 2024-12-06CHONGQING UNIV OF ARTS & SCI
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202211323574.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-27
Publication Date
2024-12-06
Estimated Expiration
2042-10-27

AI Technical Summary

Technical Problem

Existing thermal therapy equipment causes discomfort in the skin due to the impermeable materials, which increases the risk of skin allergies and inflammation. In addition, traditional thermal therapy devices are large in size and non-flexible, making them difficult to fit closely with the skin, have low heat transfer efficiency, and the temperature of painful areas is difficult to control.

Method used

Polyterephthalyl terephthalyl phenylenediamine, potassium hydroxide, dimethyl sulfoxide, and deionized water were used as raw materials, and the preparation of dark red aramid nanofiber dispersion, aqueous dispersion and gold composite electrode was prepared. Lightweight and breathable aramid nanofiber-gold composite electrode with good conductivity and breathability.

Benefits of technology

The preparation of a non-touch skin contact thermotherapy electrode is achieved. The electrode thickness is less than 3μm, the air permeability is high, the surface resistance is low, and it can be heated evenly. It is suitable for wearable applications and reduces the risk of skin discomfort and inflammation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115844623B_ABST
    Figure CN115844623B_ABST
Patent Text Reader

Abstract

A method for preparing a touchless skin contact thermotherapy electrode is to use poly(p-phenylene terephthalamide), potassium hydroxide, dimethyl sulfoxide, and deionized water as raw materials, and to prepare a dark red aramid nanofiber dispersion, an aramid nanofiber aqueous dispersion, and an aramid nanofiber gold composite electrode; the electrode thickness is as low as 3 μm, and the multi-point thickness uniformity is good, with an RSD of 2.07%. The electrode can be cut into any shape. The surface morphology of the electrode, as shown by the scanning electron microscopy results, has a certain number of holes on the surface, its air permeability is 1.7 L / h, and the electrode surface resistance is as low as 0.5 Ωsq ‑1 By applying voltage on both sides of the electrodes, heat can be generated to achieve thermal therapy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of bioelectric technology, and in particular relates to a method for preparing a touchless skin contact thermotherapy electrode. Background Art

[0002] Flexible electronics can be summarized as an emerging electronic technology that makes electronic devices made of organic / inorganic materials on flexible / ductile plastic or thin metal substrates. With its unique flexibility / ductility and efficient and low-cost manufacturing process, it has broad application prospects in the fields of information, energy, medical care, and national defense, such as flexible electronic displays, organic light-emitting diodes OLED, printed RFID, thin-film solar panels, electronic surface patches (Skin Patches), etc. Like traditional IC technology, manufacturing processes and equipment are also the main driving forces for the development of flexible electronic technology. The technical level indicators of flexible electronic manufacturing include chip feature size and substrate area size. The key is how to manufacture flexible electronic devices with smaller feature sizes on larger substrates at a lower cost. Flexible electronics covers organic electronics, plastic electronics, bioelectronics, nanoelectronics, printed electronics, etc., including RFID, flexible display, organic electroluminescent (OLED) display and lighting, chemical and biological sensors, flexible photovoltaics, flexible logic and storage, flexible batteries, wearable devices and other applications. With its rapid development, the fields involved have also been further expanded, and it has now become one of the research hotspots in interdisciplinary disciplines.

[0003] Flexible electronics have attracted great attention due to their wide applications in various fields such as wearable electronics, soft robotics, electronic skin, and implantable bioelectronics. Flexible conductors, which refer to types of conductive elements that can be bent, are indispensable building blocks for these devices and systems. To date, the research focus of flexible electronics has been on developing high-performance conductors with enhanced flexibility, stretchability, conductivity, and performance reliability. Conductors for wearable and skin-mounted electronic devices are mostly made of impermeable elastic films, and the long-term wearing comfort caused by the material and structural properties of these conductors and devices has been largely ignored. From the perspective of physiological comfort, healthy skin requires a thermal microenvironment that can provide sufficient permeability for visible or hidden sweat. Covering the skin with impermeable materials may cause an uncomfortable sensation and increase the risk of skin allergies and inflammation. In orthopedics, medical thermotherapy pads are commonly used to relieve pain, improve blood circulation, and reduce inflammation. They are also used to treat arthritis, joint stiffness, cervical spondylosis, and physical injuries. Existing thermotherapy devices have several key deficiencies that hinder the widespread application of thermotherapy devices in clinical practice. On the one hand, traditional thermal therapy hot compress devices are large or non-flexible, making it difficult to fit closely to human skin, with limited efficiency in heat energy transfer, making it difficult to control the local temperature of the painful area, and greatly reducing the therapeutic effect. From the perspective of physiological comfort, healthy skin requires a thermal microenvironment that can provide sufficient permeability for visible or hidden sweat. Covering the skin with impermeable materials may cause an uncomfortable feeling and increase the risk of skin allergies and inflammation. Therefore, flexible and stretchable devices with good breathability, moisture and liquid permeability are very suitable for wearable applications. Summary of the invention

[0004] The present invention aims at a method for preparing a touchless skin contact electrode.

[0005] The present invention is achieved through the following technical solutions:

[0006] A method for preparing a touchless skin contact thermotherapy electrode, characterized in that it is prepared from poly(p-phenylene terephthalamide), potassium hydroxide, dimethyl sulfoxide, and deionized water as raw materials, and is respectively prepared through the preparation of a dark red aramid nanofiber dispersion, the preparation of an aramid nanofiber water dispersion, and the preparation of an aramid nanofiber gold composite electrode; wherein in the preparation process of the dark red aramid nanofiber dispersion, the mass ratio of poly(p-phenylene terephthalamide) to potassium hydroxide is 1:1.5, the mass volume ratio of potassium hydroxide to deionized water is 1.5:20, g / ml, and the volume ratio of dimethyl sulfoxide to deionized water is 450-550:20.

[0007] Furthermore, the dark red aramid nanofiber dispersion is prepared by placing poly(p-phenylene terephthalamide), potassium hydroxide, dimethyl sulfoxide, and deionized water in a closed container, stirring at a uniform speed for 4 to 5 hours at a stirring speed of 400 to 1000 rpm. After the stirring is completed, a dark red aramid nanofiber dispersion is obtained with a concentration of 1.9 mg / ml to 2.1 mg / ml.

[0008] Furthermore, the preparation of the aramid nanofiber aqueous dispersion is to take a dark red aramid nanofiber dispersion and deionized water, mix them in a volume ratio of 1:2-3, first stir at a speed of 400-1000 rpm for 5-8 minutes, take it out, and then ultrasonically disperse it for 5-10 minutes under an ultrasonic frequency of 20-40 Hz, and then use a mixed cellulose microporous filter membrane with a pore size of 0.22 μm for vacuum filtration, collect the filter cake, wash it with deionized water and anhydrous ethanol in sequence, repeat 3 times to obtain light yellow aramid nanofibers, and redisperse the light yellow aramid nanofibers in deionized water, and ultrasonically perform it for 30-35 minutes under an ultrasonic frequency of 20-40 Hz to obtain the aramid nanofiber aqueous dispersion; the mass ratio of the filter cake, deionized water, and anhydrous ethanol is 1:30-50:30-50, and the concentration of the aramid nanofiber aqueous dispersion is 0.9 mg / ml-1.1 mg / ml.

[0009] Further, the preparation of the aramid nanofiber gold composite electrode is to take a glass plate of suitable size as a bottom plate, drip the aramid nanofiber aqueous dispersion on the bottom plate, ensure that 0.09ml to 1.1ml is dripped per 1 cm glass plate, and after the dripping is completed, place it in a constant temperature drying oven at 75 to 85°C and dry it for 4 to 6 hours. After the drying is completed, gold is plated on the surface. The material is a gold target material, and the magnetron sputtering is a vacuum degree of 10 -3 ~10 -2 Pa, introduce Ar to adjust the gas pressure to 3Pa, the current to 10-25mA, the voltage to 250-300V, the sputtering power to 20-40W, the sputtering time to 110-160s, and after the gold plating is completed, separate it from the glass sheet to obtain a thin, breathable aramid nanofiber-gold composite electrode.

[0010] The aramid nanofiber membrane of the present invention is a non-woven fabric-like film formed by spreading fibers, with gaps between the fibers to ensure a certain air permeability. During the preparation of the aramid nanofiber gold composite electrode, gold is deposited on the surface of the fiber, so the gold plating thickness can be adjusted, so that the electrode of the present invention has both air permeability and good conductivity.

[0011] Beneficial effects:

[0012] A non-touch skin contact electrode, the electrode thickness is as low as 3μm, and the multi-point thickness uniformity is good, RSD is 2.07%, this electrode can be cut into any shape. The surface morphology of this electrode, as shown by the scanning electron microscopy results, has a certain number of holes on the surface, its air permeability is 1.7L / h, and the electrode surface resistance is as low as 0.5Ωsq -1 By applying voltage on both sides of the electrodes, heat can be generated to achieve thermal therapy. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 : Scanning electron microscope image of the electrode surface of Example 1 of the present invention.

[0014] Figure 2 : Temperature-time relationship diagram of the electrode under different heating voltages in Example 1 of the present invention.

[0015] Figure 3 : Infrared imaging of the electrode (2cm*1cm) of Example 1 of the present invention at a heating voltage of 0.6V. DETAILED DESCRIPTION

[0016] The present invention will be further described in detail below through embodiments and in conjunction with the accompanying drawings.

[0017] Example 1

[0018] A non-touch skin contact thermal therapy electrode is prepared according to the following steps:

[0019] 1. Preparation of dark red aramid nanofiber dispersion:

[0020] Put poly(p-phenylene terephthalamide), potassium hydroxide, dimethyl sulfoxide and deionized water in a closed container and stir them at a constant speed for 4.5 hours at a stirring speed of 800 rpm. After stirring, a dark red aramid nanofiber dispersion with a concentration of 2.0 mg / ml is obtained. The mass ratio of poly(p-phenylene terephthalamide) to potassium hydroxide is 1:1.5, the mass volume ratio of potassium hydroxide to deionized water is 1.5:20, g / ml, and the volume ratio of dimethyl sulfoxide to deionized water is 500:20;

[0021] 2. Preparation of aramid nanofiber aqueous dispersion:

[0022] Take a dark red aramid nanofiber dispersion and deionized water, mix them in a volume ratio of 1:2.5, first stir at a speed of 800 rpm for 7 minutes, take them out, and then ultrasonically disperse them for 8 minutes under an ultrasonic frequency of 30HZ, then use a mixed cellulose microporous filter membrane with a pore size of 0.22μm for vacuum filtration, collect the filter cake, wash it with deionized water and anhydrous ethanol in sequence, repeat 3 times to obtain light yellow aramid nanofibers, redisperse the light yellow aramid nanofibers in deionized water, and ultrasonically treat it at an ultrasonic frequency of 30HZ for 32 minutes to obtain an aramid nanofiber aqueous dispersion; the mass ratio of the filter cake, deionized water, and anhydrous ethanol is 1:40:40, and the concentration of the aramid nanofiber aqueous dispersion is 1.0mg / ml;

[0023] 3. Preparation of Aramid Nanofiber-Gold Composite Electrode

[0024] Take a glass plate of suitable size as the bottom plate, drip aramid nanofiber aqueous dispersion on the bottom plate, ensure that 1.0 ml is dripped for every 1 cm of glass plate, after dripping, place it in a constant temperature drying oven at 80℃, dry for 5 hours, after drying, plate gold on the surface, the material is gold target, the magnetron sputtering is vacuumed to 10 -3 Pa, Ar was introduced to adjust the gas pressure to 3Pa, the current was 20mA, the voltage was 280V, the sputtering power was 30W, the sputtering time was 150s, and the gold plating was completed. It was separated from the glass sheet to obtain a thin, breathable aramid nanofiber-gold composite electrode. The prepared electrode was placed under an electron microscope for observation. The electrode had a uniform pore size, indicating good air permeability. Figure 1 ; The obtained electrode was heated at different voltages to investigate the temperature-time relationship. The voltage, temperature, and time graphs are shown in Figure 2 ; The prepared electrode (2cm*1cm) was heated at a voltage of 0.6V and infrared images were taken at different finger positions. Figure 3 .

[0025] Experiment 1: Thickness measurement of the electrode prepared in Example 1

[0026] Method: Using a KLA-Tencor probe-type step profiler such as KLA-Tencor AlphaStep D-600 StylusProfiler thickness profiler, the thickness of 6 points at different positions of the electrode in Example 1 was measured. The experimental results are shown in the following table:

[0027] sample 1# 2# 3# 4# 5# 6# RSD Example 1 (μm) 2.91 2.87 2.83 2.95 2.86 2.99 2.07%

[0028] Results: As can be seen from the above table, the thickness of the electrode of the present invention is uniform and less than 3 μm.

[0029] Experiment 2: Measuring the air permeability of the electrode prepared in Example 1

[0030] Method: The air permeability of the sample was tested using the TQD-G1 air permeability tester produced by Jinan Languang Electromechanical Technology Co., Ltd. 10 samples with a diameter of 50 mm were randomly cut from the electrode. One of the samples was clamped in the air permeability tester to make the sample flat, without deformation, and with good sealing on both sides of the sample. The pressure difference value set for this test is 100Pa. Adjust the pressure control valve to adjust the pressure difference on both sides of the sample. When the pressure difference reaches the set value, the test stops. The equipment automatically displays the gas flow rate passing through the sample at this time. Repeat the sample loading and pressure control valve adjustment operations until the test of 10 samples is completed.

[0031] Results: After testing 10 pieces, the average air permeability was 1.7 L / h, indicating that the electrode of the present invention has excellent air permeability.

[0032] Experiment 3: Surface resistance measurement of the electrode prepared in Example 1

[0033] Method: The surface resistance is measured by the four-probe method, and the test instrument is SDY-4 from Shenzhen Excellence Instrument Co., Ltd. The specific test steps are as follows:

[0034] (1) Connect the power supply and turn on the main unit. The "R" and "I" indicators will light up. Preheat for about 5 minutes.

[0035] (2) Check working conditions: working temperature is 23±2℃, relative humidity is 65%. The following operations can be performed only when the above conditions are met.

[0036] (3) Based on the diameter and thickness of the silicon wafer and the correction coefficient of the probe, calculate the current value of the measured silicon wafer and the standard sample.

[0037] (4) Remove the probe protective cover and wipe the probe and work platform with an alcohol cotton ball.

[0038] (5) Select the current range according to the instructions based on the range of resistivity values ​​required by each contract.

[0039] (6) Use a standard sample to calibrate the tester. Test at least three points at the center of the silicon wafer and compare their average value with the resistance value of the standard sample. If the difference is within 1.5%, testing can be performed.

[0040] (7) Place the ultra-thin electrode to be tested in the center of the probe holder test table for testing.

[0041] (8) The probe is pressed against the center point of the ultra-thin electrode. When the measured value stabilizes, read the resistivity value displayed on the display.

[0042] 9. If the measured value on the display screen fluctuates unstably and exceeds the deviation range during the measurement process, stop working and check whether there are any abnormalities in the room temperature, the silicon rod measuring surface, and the display.

[0043] 10. After the whole batch of measurements is completed, the probe is covered with a protective cover, and the lifting frame is lowered to 5cm-8cm above the measuring table. Turn off the power switch.

[0044] Result: Electrode surface resistance 0.5Ωsq -1 .

[0045] Example 2

[0046] A non-touch skin contact thermal therapy electrode is prepared according to the following steps:

[0047] 1. Preparation of dark red aramid nanofiber dispersion:

[0048] Put poly(p-phenylene terephthalamide), potassium hydroxide, dimethyl sulfoxide and deionized water in a closed container and stir them at a constant speed for 4 hours at a stirring speed of 1000 rpm. After the stirring is completed, a dark red aramid nanofiber dispersion is obtained with a concentration of 2.0 mg / ml. The mass ratio of poly(p-phenylene terephthalamide) to potassium hydroxide is 1:1.5, the mass volume ratio of potassium hydroxide to deionized water is 1.5:20, g / ml, and the volume ratio of dimethyl sulfoxide to deionized water is 500:20;

[0049] 2. Preparation of aramid nanofiber aqueous dispersion:

[0050] Take a dark red aramid nanofiber dispersion and deionized water, mix them in a volume ratio of 1:3, first stir at a speed of 1000 rpm for 5 minutes, take it out, and then ultrasonically disperse it for 10 minutes under an ultrasonic frequency of 20HZ, then use a mixed cellulose microporous filter membrane with a pore size of 0.22μm for vacuum filtration, collect the filter cake, wash it with deionized water and anhydrous ethanol in sequence, repeat 3 times to obtain light yellow aramid nanofibers, and redisperse the light yellow aramid nanofibers in deionized water, and ultrasonicate it for 35 minutes under an ultrasonic frequency of 20HZ to obtain an aramid nanofiber aqueous dispersion; the mass ratio of the filter cake, deionized water, and anhydrous ethanol is 1:50:30, and the concentration of the aramid nanofiber aqueous dispersion is 0.9mg / ml;

[0051] 3. Preparation of Aramid Nanofiber-Gold Composite Electrode

[0052] Take a glass plate of suitable size as the bottom plate, drip aramid nanofiber aqueous dispersion on the bottom plate, ensure that 1.1 ml is dripped for every 1 cm of glass plate, after dripping, place it in a constant temperature drying oven at 85℃, dry for 4 hours, after drying, plate gold on the surface, the material is gold target, the vacuum degree of magnetron sputtering is 10 -2Pa, Ar was introduced to adjust the gas pressure to 3 Pa, the current was 10 mA, the voltage was 300 V, the sputtering power was 20 W, and the sputtering time was 160 s. After the gold plating was completed, it was separated from the glass sheet to obtain a thin, breathable aramid nanofiber-gold composite electrode.

[0053] The electrode prepared in Example 2 was subjected to thickness measurement, air permeability measurement and surface resistance measurement according to the experimental method of Example 1. The experimental results showed that the thickness was less than 3 μm, the RSD of 6 points was 1.93%, the air permeability was 1.6 L / h, and the surface resistance was 0.5 sq -1 .

[0054] Example 3

[0055] A non-touch skin contact thermal therapy electrode is prepared according to the following steps:

[0056] 1. Preparation of dark red aramid nanofiber dispersion:

[0057] Put poly(p-phenylene terephthalamide), potassium hydroxide, dimethyl sulfoxide and deionized water in a closed container and stir them at a constant speed for 5 hours at a stirring speed of 400 rpm. After the stirring is completed, a dark red aramid nanofiber dispersion is obtained with a concentration of 2.0 mg / ml. The mass ratio of poly(p-phenylene terephthalamide) to potassium hydroxide is 1:1.5, the mass volume ratio of potassium hydroxide to deionized water is 1.5:20, g / ml, and the volume ratio of dimethyl sulfoxide to deionized water is 500:20;

[0058] 2. Preparation of aramid nanofiber aqueous dispersion:

[0059] Take a dark red aramid nanofiber dispersion and deionized water, mix them in a volume ratio of 1:2, first stir at a speed of 400 rpm for 8 minutes, take it out, and then ultrasonically disperse it for 10 minutes under an ultrasonic frequency of 20HZ, then use a mixed cellulose microporous filter membrane with a pore size of 0.22μm for vacuum filtration, collect the filter cake, wash it with deionized water and anhydrous ethanol in sequence, repeat 3 times to obtain light yellow aramid nanofibers, and redisperse the light yellow aramid nanofibers in deionized water, and ultrasonicate it for 30 minutes under an ultrasonic frequency of 20HZ to obtain an aramid nanofiber aqueous dispersion; the mass ratio of the filter cake, deionized water, and anhydrous ethanol is 1:50:30, and the concentration of the aramid nanofiber aqueous dispersion is 0.9mg / ml;

[0060] 3. Preparation of Aramid Nanofiber-Gold Composite Electrode

[0061] Take a glass plate of suitable size as the bottom plate, drip aramid nanofiber aqueous dispersion on the bottom plate, ensure that 1.1 ml is dripped for every 1 cm of glass plate, and after dripping, place it in a 75℃ constant temperature drying oven and dry it for 6 hours. After drying, gold is plated on the surface. The material is gold target material. The magnetron sputtering is vacuumed to 10 -2 Pa, Ar was introduced to adjust the gas pressure to 3 Pa, the current was 25 mA, the voltage was 250 V, the sputtering power was 20 W, the sputtering time was 110 s, the gold plating was completed, and it was separated from the glass sheet to obtain a thin, breathable aramid nanofiber-gold composite electrode.

[0062] The electrode prepared in Example 3 was subjected to thickness measurement, air permeability measurement and surface resistance measurement according to the experimental method of Example 1. The experimental results showed that the thickness was less than 3 μm, the RSD of 6 points was 1.83%, the air permeability was 1.7 L / h, and the surface resistance was 0.4 sq -1 .

Claims

1. A method for preparing a non-touch skin contact thermotherapy electrode, characterized in that: The invention adopts poly(p-phenylene terephthalamide), potassium hydroxide, dimethyl sulfoxide and deionized water as raw materials, and is obtained by respectively preparing dark red aramid nanofiber dispersion, preparing aramid nanofiber water dispersion and preparing aramid nanofiber gold composite electrode; wherein in the preparation process of the dark red aramid nanofiber dispersion, the mass ratio of poly(p-phenylene terephthalamide) to potassium hydroxide is 1:1.5, the mass volume ratio of potassium hydroxide to deionized water is 1.5:20, g / ml, the volume ratio of dimethyl sulfoxide to deionized water is 450-550:20, and the preparation of the aramid nanofiber water dispersion comprises the following steps: taking the dark red aramid nanofiber dispersion and the deionized water, mixing them in a volume ratio of 1:2-3, firstly stirring at a rotation speed of 40 The method comprises the steps of: stirring at 0 to 1000 rpm for 5 to 8 minutes, taking out, and then ultrasonically dispersing for 5 to 10 minutes at an ultrasonic frequency of 20 to 40 Hz, and then vacuum filtering with a mixed cellulose microporous filter membrane with a pore size of 0.22 μm, collecting the filter cake, washing with deionized water and anhydrous ethanol in sequence, and repeating the process for 3 times to obtain light yellow aramid nanofibers, and re-dispersing the light yellow aramid nanofibers in deionized water, and ultrasonically dispersing for 30 to 35 minutes at an ultrasonic frequency of 20 to 40 Hz to obtain an aramid nanofiber aqueous dispersion; the mass ratio of the filter cake, deionized water, and anhydrous ethanol is 1:30 to 50:30 to 50, and the concentration of the aramid nanofiber aqueous dispersion is 0.9 mg / ml to 1.1 mg / mL.

2. The method for preparing a touchless skin contact thermotherapy electrode according to claim 1, characterized in that: The dark red aramid nanofiber dispersion is prepared by placing poly(p-phenylene terephthalamide), potassium hydroxide, dimethyl sulfoxide and deionized water in a closed container, stirring at a constant speed for 4 to 5 hours at a stirring speed of 400 to 1000 rpm. After the stirring is completed, a dark red aramid nanofiber dispersion is obtained with a concentration of 1.9 mg / ml to 2.1 mg / ml.

3. The method for preparing a touchless skin contact thermotherapy electrode according to claim 2, characterized in that: The preparation of the aramid nanofiber gold composite electrode is to take a glass plate of suitable size as a bottom plate, drip the aramid nanofiber water dispersion on the bottom plate, ensure that 0.09ml~1.1ml is dripped per 1 cm glass plate, and after the dripping is completed, place it in a constant temperature drying oven at 75~85℃, dry for 4~6 hours, and after the drying is completed, gold is plated on the surface. The material is a gold target material, and the magnetron sputtering is a vacuum degree of 10 -3 ~10 -2 Pa, introduce Ar to adjust the gas pressure to 3Pa, the current is 10~25mA, the voltage is 250~300V, the sputtering power is 20~40W, the sputtering time is 110~160s, and the gold plating is completed and separated from the glass sheet to obtain a thin, breathable aramid nanofiber-gold composite electrode.

Citation Information

Patent Citations

  • Preparing method of water-dispersed aramid nanofiber and aramid nanopaper

    CN108285540A

  • Flexible high-strength aramid nanofiber-based composite electrothermal film and preparation method thereof

    CN109788586A

  • Conductive fabric and preparation method and application thereof

    CN110106474A

  • Copper nanowire / aramid nanofiber composite conductive film and preparation method thereof