A modified iron-based catalyst for synthesizing alpha-olefins by hydrogenation of carbon dioxide and a preparation method thereof
By modifying the iron-based catalyst and using a combination of transition metal and alkali metal promoters on the carrier, the α-olefin selectivity and conversion rate of the carbon dioxide hydrogenation reaction are improved, and the problems of low conversion rate and selectivity in the existing technology are solved. problem, achieving efficient and low-cost α-olefin generation.
Patent Information
- Application Number
- CN202211492721.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-25
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-11-25
AI Technical Summary
In the prior art, the conversion rate and selectivity of hydrogenating carbon dioxide to produce α-olefins are low, and the catalyst stability is insufficient, resulting in high production costs and low α-olefin selectivity.
Modified iron-based catalysts are used to form iron oxides and transition metal oxides on the carrier, combined with alkali metals for modification. The preparation methods include co-precipitation and impregnation methods, and transition metals such as Zn, Cu, Mn and alkali metals are added. For example, K and Na form a catalyst with an equal molar ratio of Fe-Zn-Na-Al.
The conversion rate of CO2 and the selectivity of α-olefins are significantly improved, and the selectivity of CO and CH4 is reduced, achieving efficient α-olefin generation and reducing production costs.
Smart Images

Figure BDA0003964128350000111 
Figure BDA0003964128350000121
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of catalysts, and in particular to a modified iron-based catalyst for synthesizing alpha-olefins by hydrogenating carbon dioxide and a preparation method thereof. Background Art
[0002] Due to the chemical inertness of CO2, it is relatively easy to convert CO2 into C1 molecules such as methane, methanol, and CO by hydrogenation, but it is difficult to convert it into compounds containing more than two carbon atoms. α-olefins (R-CHCH2, olefins with terminal C=C bonds and C≥4) are very attractive as important industrial raw materials and are indispensable chemicals for the production of polymers, synthetic plasticizers, lubricants, and surfactants. With the continuous development of petrochemicals, its demand is increasing day by day around the world, so the process of synthesizing α-olefins by hydrogenation of CO2 has received widespread attention, and the research and development of catalysts is the key to realizing the synthesis of α-olefins by hydrogenation of carbon dioxide.
[0003] Existing α-olefins are mainly produced by ethylene polymerization in petrochemicals, and a few are obtained from the Fischer-Tropsch synthesis (FTS). Carbon dioxide is considered to be a potential source for the production of α-olefins, which can not only reduce carbon emissions but also provide a sustainable alternative to fossil fuels. Viable routes for hydrogenating carbon dioxide to olefins: (1) Methanol intermediate (CO2-MeOH) route: CO2 is hydrogenated on metal oxides to synthesize methanol, and methanol is converted into olefins on zeolites, realizing the direct conversion of CO2 into low-carbon olefins (ethylene, propylene and butene, C2-C4 olefins); (2) CO2 modified FTS (CO2-FTS) route: CO2 is reduced to CO through the reverse water gas shift (RWGS) reaction, and then CO is hydrogenated to olefins through the FTS reaction. Although the CO2-MeOH route has made significant progress, the main olefin products are still limited to C2-C4 olefins, and due to the inherent mechanism of the methanol to olefins (MTO) process, C 4+ The maximum selectivity for olefins does not exceed 40%. Since iron is active in both RWGS and FTS processes, Fe-based catalysts are more suitable for CO2 hydrogenation to α-olefins than other metal catalysts such as Co and Ru-based FTS catalysts. Fe3O4 is the active phase of the RWGS reaction, which converts CO2 into CO. Subsequently, in the FTS reaction, the adsorbed CO can be dissociated (hydrogen-assisted dissociation or direct dissociation) into surface carbon and surface oxygen, and these surface carbon species diffuse into the α-Fe lattice under different reaction conditions. It is generally believed that Fe carbides, especially χ-Fe5C2, are the active phases in the FTS reaction and play a key role in carbon chain growth and α-olefin selection.
[0004] In general, the selectivity of α-olefins in the current research reports on the hydrogenation of CO2 to α-olefins is still low. The stability of catalysts and processes is another technical challenge for future industrialization. Therefore, the research and development of catalysts for the preparation of α-olefins with high selectivity by direct hydrogenation of CO2 is the key to the industrialization of α-olefins synthesized by CO2 hydrogenation.
[0005] In the prior art, the application number is 201611098885.9, which is a preparation method for a modified iron-based catalyst that can be used for the selective hydrogenation of carbon dioxide to produce α-olefins. The main active ingredient of the catalyst is designed to be Fe, and multiple additives are added for modification. The additives are directly mixed with the common Fe catalyst by a simple physical mixing method. In addition, the additives come from waste biomass powder rich in minerals after high-temperature roasting. The catalyst provided by this application has an olefin selectivity of more than 30% for the carbon dioxide hydrogenation reaction with α-olefins as the main product. In addition, the application number is 202210613800.5, a composite catalyst for direct production of light aromatics from carbon dioxide hydrogenation, and its preparation and application. The iron-based catalyst composite modified molecular sieve is used to catalyze the hydrogenation of carbon dioxide to produce light aromatics, and the conversion rate can reach 42%, and the selectivity of aromatics in total hydrocarbons can reach 63%. In the total hydrocarbons, α-olefins are not obtained as the main product.
[0006] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention
[0007] One of the technical problems to be solved by the present invention is to provide a modified iron-based catalyst for the hydrogenation of carbon dioxide to synthesize α-olefins, which can effectively reduce the production cost while improving the conversion rate of CO2 and the selectivity of α-olefins.
[0008] The second technical problem to be solved by the present invention is to provide a method for preparing a modified iron-based catalyst, the content of each component of the catalyst is controllable, and the preparation method is simple.
[0009] To achieve the above object, the present invention adopts the following technical scheme: a modified iron-based catalyst is used to catalyze the hydrogenation of carbon dioxide to synthesize α-olefins, wherein the modified iron-based catalyst is obtained by modifying an iron-based catalyst formed by iron oxide and transition metal oxide supported on a carrier with an alkali metal.
[0010] In one or more embodiments of the present invention, the present invention comprises a carrier and a main active component, a first auxiliary active component and a second auxiliary active component loaded on the carrier, wherein the main active component comprises iron, the first auxiliary active component comprises a transition metal element other than iron, the second auxiliary active component comprises an alkali metal element, and the main component of the carrier is a metal oxide: the molar ratio of the iron element of the main active component, the transition metal element of the first auxiliary active component, the alkali metal element of the second auxiliary active component and the metal element of the carrier is 100:(3-8):(1-8):(8-40).
[0011] In one or more embodiments of the present invention, the transition metal is selected from oxides formed by one or more transition metals selected from Zn, Cu, Mn or Ni.
[0012] In one or more embodiments of the present invention, the alkali metal element is selected from one or more of K and Na.
[0013] In one or more embodiments of the present invention, the support is selected from a mixture of one or more of alumina, titania or zirconia.
[0014] In order to solve the second technical problem to be solved by the present invention, the following technical solution is adopted:
[0015] The preparation method of the modified iron-based catalyst comprises the following steps:
[0016] (1) After the metal salt, iron salt and transition metal salt of the carrier are mixed and dissolved, the metal ions are precipitated by a coprecipitation method to obtain a precipitate;
[0017] (2) washing, drying and calcining the precipitate to obtain an iron-based catalyst of a metal oxide;
[0018] (3) After the iron-based catalyst is impregnated with an alkali metal salt solution, it is dried and calcined to obtain a modified iron-based catalyst.
[0019] In one or more embodiments of the present invention, the co-precipitation method in step (1) is to obtain a mixed solution A by mixed dissolution, and fully react with a carbonate solution to obtain a precipitate.
[0020] In one or more embodiments of the present invention, the coprecipitation is performed by dropping the mixed solution A into the carbonate solution, with the end point of the dropping being a pH of 7 to 10; and / or, the coprecipitation is performed at a water bath temperature ≥ 80°C.
[0021] In one or more embodiments of the present invention, the drying temperature in step (2) is 60-80°C, the roasting temperature is 400-600°C, and the roasting time is 4-8h; and / or, the drying temperature in step (3) is 50-110°C, the roasting temperature is 400-600°C, and the roasting time is 4-8h.
[0022] In one or more embodiments of the present invention, the calcination temperature in step (2) is 450-550° C., and the calcination time is 5-7 hours.
[0023] In one or more embodiments of the present invention, the molar amount of the alkali metal impregnated on the iron-based catalyst in step (3) is 1.0-8.0% of iron.
[0024] The invention provides an application of an iron-based catalyst in catalyzing the hydrogenation of carbon dioxide to generate alpha-olefins and a preparation method thereof, in order to solve the problems of low conversion rate of carbon dioxide hydrogenation to CO2 and low selectivity for alpha-olefins, high selectivity for by-products, etc. According to the formation principle of alpha-olefins, firstly, CO2 is reduced to CO by RWGS at the Fe3O4 position, and then hydrogenated at the χ-Fe5C2 position to generate alpha-olefins. The modified iron-based catalyst prepared by the invention has good performance, and is characterized in that the appropriate addition of an auxiliary agent can not only improve the activity of CO2, but also be beneficial to the selective synthesis of alpha-olefins. In addition, the addition of transition metal aluminum is beneficial to the dispersion of active components of the iron-based catalyst, and promotes the CO2 conversion reaction.
[0025] Therefore, compared with the prior art, the specific implementation of the present invention has the following advantages:
[0026] (1) The modified iron-based catalyst prepared by the present invention does not contain precious metals such as platinum, palladium, and rhenium, which can effectively reduce production costs;
[0027] (2) When the catalyst of the present invention is used for hydrogenation of carbon dioxide to produce α-olefins, the CO2 conversion rate can reach 45%, the CO and CH4 selectivities are less than 15%, and the α-olefin selectivity can reach more than 60%. DETAILED DESCRIPTION
[0028] The specific embodiments of the present invention are described in detail below, but it should be understood that the protection scope of the present invention is not limited by the specific embodiments.
[0029] Unless explicitly stated otherwise, throughout the specification and claims, the term “comprise” or variations such as “include” or “comprising”, etc., will be understood to include the stated elements or components but not to exclude other elements or components.
[0030] Example 1
[0031] (1) Preparation of modified iron-based catalyst
[0032] 20.2g Fe(NO3)3·9H2O, 0.45g Zn(NO3)2·6H2O and 7.5g Al(NO3)3·9H2O were weighed and dissolved in 400mL deionized water. The solution obtained after stirring was recorded as A. In addition, 10.3g anhydrous Na2CO3 solid was weighed and added to 100mL deionized water to prepare a solution with a concentration of 1.0mol / L Na2CO3. Under 80℃ water bath conditions, A was added dropwise to the prepared Na2CO3 solution, and titrated while stirring. The titration end point was pH = 7. After aging, washing, drying at 110℃, and calcining at 400℃ for 4h, the molar ratio of Fe-Zn-Al in the obtained iron-based catalyst was 100:3:40.
[0033] 0.21 g Na2CO3 was added to deionized water to prepare a 0.25 mol / L Na2CO3 solution, which was impregnated on the iron-based catalyst Fe-Zn-Al, dried at 110°C, and calcined at 400°C for 4 hours to obtain a molar ratio of Fe-Zn-Na-Al in the modified iron-based catalyst of 100:3:8:40.
[0034] (2) Evaluation of the reaction of carbon dioxide hydrogenation to α-olefins over modified iron-based catalysts
[0035] The prepared modified iron-based catalyst was loaded into the constant temperature zone in the middle of the reaction tube, and 50g of 20-40 mesh quartz sand was loaded in the upper and lower parts of the reaction tube respectively. The modified iron-based catalyst was reduced under the following reduction conditions: temperature 350°C, flow rate 80mL / min, reduction time 5h; after the reduction, the raw material was heated to 4000mL / (g / min) at a H2 / CO2 molar ratio of 1. cat h) Feed the materials, slowly increase the pressure of the reaction system to 3.0 MPa, and heat to 320°C to start the reaction.
[0036] The results of the catalytic reaction of the modified iron-based catalyst Fe-Zn-Na-Al prepared in Example 1 on the hydrogenation of carbon dioxide to produce α-olefins are shown in Table 1.
[0037] Example 2
[0038] (1) Preparation of modified iron-based catalyst
[0039] 20.2g Fe(NO3)3·9H2O, 0.90g Zn(NO3)2·6H2O and 7.5g Al(NO3)3·9H2O were weighed and dissolved in 400mL deionized water. The solution obtained after stirring was recorded as A. In addition, 10.3g anhydrous Na2CO3 solid was weighed and added to 100mL deionized water to prepare a solution with a concentration of 1.0mol / L Na2CO3. Under 80℃ water bath conditions, A was added dropwise to the prepared Na2CO3 solution, and titrated while stirring. The titration end point was pH = 7. After aging, washing, drying at 110℃, and calcining at 400℃ for 4h, the molar ratio of Fe-Zn-Al in the obtained iron-based catalyst was 100:6:40.
[0040] 0.21 g Na2CO3 was added to deionized water to prepare a 0.25 mol / L Na2CO3 solution, which was impregnated on the iron-based catalyst Fe-Zn-Al, dried at 110°C, and calcined at 400°C for 4 hours to obtain a molar ratio of Fe-Zn-Na-Al in the modified iron-based catalyst of 100:6:8:40.
[0041] (2) Evaluation of the reaction of carbon dioxide hydrogenation to α-olefins over modified iron-based catalysts
[0042] The prepared modified iron-based catalyst was loaded into the constant temperature zone in the middle of the reaction tube, and 50g of 20-40 mesh quartz sand was loaded in the upper and lower parts of the reaction tube respectively. The modified iron-based catalyst was reduced under the following reduction conditions: temperature 350°C, flow rate 80mL / min, reduction time 5h; after the reduction, the raw material was heated to 4000mL / (g / min) at a H2 / CO2 molar ratio of 1. cat h) Feed the materials, slowly increase the pressure of the reaction system to 3.0 MPa, and heat to 320°C to start the reaction.
[0043] The results of the catalytic reaction of the modified iron-based catalyst Fe-Zn-Na-Al prepared in Example 2 on the hydrogenation of carbon dioxide to produce α-olefins are shown in Table 1.
[0044] Example 3
[0045] (1) Preparation of modified iron-based catalyst
[0046] 20.20gFe(NO3)3·9H2O, 0.72gCu(NO3)2·3H2O and 4.04gAl(NO3)3·9H2O were weighed and dissolved in 400mL deionized water, and the solution obtained after stirring was recorded as A. In addition, 13.8g of anhydrous K2CO3 solid was weighed and added to 100mL deionized water to prepare a solution with a concentration of 1.0mol / LK2CO3. Under 80℃ water bath conditions, A was added dropwise to the prepared K2CO3 solution, and titrated while stirring. The titration end point was pH=10. After aging, washing, drying at 50℃, and calcining at 600℃ for 5h, the molar ratio of Fe-Cu-Al of the iron-based catalyst was 100:6:20.
[0047] 0.14 g K2CO3 was added to deionized water to prepare a 0.25 mol / L K2CO3 solution, which was impregnated on the iron-based catalyst Fe-Cu-Al, dried at 50°C, and calcined at 600°C for 5 hours to obtain a modified iron-based catalyst Fe-Cu-K-Al with a molar ratio of 100:6:4:20.
[0048] (2) Evaluation of the reaction of carbon dioxide hydrogenation to α-olefins over modified iron-based catalysts
[0049] The modified iron-based catalyst was loaded in the constant temperature zone in the middle of the reaction tube, and 50g of 20-40 mesh quartz sand was loaded in the upper and lower parts of the reaction tube; the modified iron-based catalyst was reduced under the following conditions: temperature 350°C, flow rate 80mL / min, reduction time 5h; after the reduction, the H2 / CO2 molar ratio was 3, the raw material space velocity was 1000mL / (g cat h) Feed the materials, slowly increase the pressure of the reaction system to 3.0 MPa, and heat to 280°C to start the reaction.
[0050] The results of the catalytic reaction of carbon dioxide hydrogenation to α-olefins using the modified iron-based catalyst Fe-Cu-K-Al prepared in Example 3 are shown in Table 1.
[0051] Example 4
[0052] (1) Preparation of modified iron-based catalyst
[0053] 20.20gFe(NO3)3·9H2O, 0.96gCu(NO3)2·3H2O and 4.04gAl(NO3)3·9H2O were weighed and dissolved in 400mL deionized water, and the solution obtained after stirring was recorded as A. In addition, 13.8g of anhydrous K2CO3 solid was weighed and added to 100mL deionized water to prepare a solution with a concentration of 1.0mol / LK2CO3. Under 80℃ water bath conditions, A was added dropwise to the prepared K2CO3 solution, and titrated while stirring. The titration end point was pH=10. After aging, washing, drying at 50℃, and calcining at 600℃ for 5h, the molar ratio of Fe-Cu-Al of the iron-based catalyst was 100:8:20.
[0054] 0.14 g K2CO3 was added to deionized water to prepare a 0.25 mol / L K2CO3 solution, which was impregnated on the iron-based catalyst Fe-Cu-Al, dried at 50°C, and calcined at 600°C for 5 hours to obtain a modified iron-based catalyst Fe-Cu-K-Al with a molar ratio of 100:8:4:20.
[0055] (2) Evaluation of the reaction of carbon dioxide hydrogenation to α-olefins over modified iron-based catalysts
[0056] The modified iron-based catalyst was loaded in the constant temperature zone in the middle of the reaction tube, and 50g of 20-40 mesh quartz sand was loaded in the upper and lower parts of the reaction tube; the modified iron-based catalyst was reduced under the following conditions: temperature 350°C, flow rate 80mL / min, reduction time 5h; after the reduction, the H2 / CO2 molar ratio was 3, the raw material space velocity was 1000mL / (g cat h) Feed the materials, slowly increase the pressure of the reaction system to 3.0 MPa, and heat to 280°C to start the reaction.
[0057] The results of the catalytic reaction of carbon dioxide hydrogenation to α-olefins using the modified iron-based catalyst Fe-Cu-K-Al prepared in Example 4 are shown in Table 1.
[0058] Example 5
[0059] (1) Preparation of modified iron-based catalyst
[0060] 20.2g Fe(NO3)3·9H2O, 0.44g Ni(NO3)2·6H2O and 1.5g Al(NO3)3·9H2O were weighed and dissolved in 400mL deionized water. The solution obtained after stirring was recorded as A. In addition, 10.6g anhydrous Na2CO3 solid was weighed and added to 100mL deionized water to prepare a solution with a concentration of 1.0mol / LNa2CO3. Under 80℃ water bath conditions, A was added dropwise to the prepared Na2CO3 solution, and titrated while stirring. The titration end point was pH = 7. After aging, washing, drying at 80℃, and calcination at 550℃ for 6h, the molar ratio of Fe-Ni-Al of the iron-based catalyst was 100:3:8.
[0061] 0.03 g Na2CO3 was added to deionized water to prepare a 0.25 mol / L Na2CO3 solution, which was impregnated on the iron-based catalyst Fe-Ni-Al. After drying at 80°C and calcining at 550°C for 6 hours, the molar ratio of the modified iron-based catalyst Fe-Ni-Na-Al was obtained to be 100:3:1:8.
[0062] (2) Evaluation of the reaction of carbon dioxide hydrogenation to α-olefins over modified iron-based catalysts
[0063] The modified iron-based catalyst was loaded in the constant temperature zone in the middle of the reaction tube, and 50g of 20-40 mesh quartz sand was loaded in the upper and lower parts of the reaction tube; the modified iron-based catalyst was reduced under the following conditions: temperature 400°C, flow rate 150mL / min, and reduction time 8h; after the reduction, the H2 / CO2 molar ratio was 4, and the raw material space velocity was 5000mL / (g cat h) Feed the materials, slowly increase the pressure of the reaction system to 6.0 MPa, and heat to 250°C to start the reaction.
[0064] The results of the catalytic reaction of carbon dioxide hydrogenation to α-olefins using the modified iron-based catalyst Fe-Ni-Na-Al prepared in Example 5 are shown in Table 1.
[0065] Example 6
[0066] (1) Preparation of modified iron-based catalyst
[0067] 20.20gFe(NO3)3·9H2O, 1.0gMn(NO3)2·4H2O and 5.63gAl(NO3)3·9H2O were weighed and dissolved in 400mL deionized water, and the solution obtained after stirring was recorded as A. In addition, 15.68g of anhydrous K2CO3 solid was weighed and added to 100mL deionized water to prepare a solution with a concentration of 1.0mol / LK2CO3. Under 80℃ water bath conditions, A was added dropwise to the prepared K2CO3 solution, and titrated while stirring. The titration end point was pH=8. After aging, washing, drying at 110℃, and calcining at 500℃ for 5h, the molar ratio of Fe-Mn-Al of the iron-based catalyst was 100:8:30.
[0068] 0.17 g K2CO3 was added to deionized water to prepare a 0.25 mol / L K2CO3 solution, which was impregnated on the iron-based catalyst Fe-Mn-Al, dried at 110°C, and calcined at 500°C for 5 hours to obtain a modified iron-based catalyst Fe-Mn-K-Al with a molar ratio of 100:8:5:30.
[0069] (2) Evaluation of the reaction of carbon dioxide hydrogenation to α-olefins over modified iron-based catalysts
[0070] The modified iron-based catalyst Fe-Mn-K-Al was loaded in the constant temperature zone in the middle of the reaction tube, and 50g of 20-40 mesh quartz sand was loaded in the upper and lower parts of the reaction tube; the modified iron-based catalyst Fe-Mn-K-Al was reduced, and the reduction conditions were: temperature 400°C, flow rate 80mL / min, and reduction time 5h; after the reduction was completed, according to the H2 / CO2 molar ratio of 1, the raw material space velocity 5000mL / (g cat h) Feed the materials, slowly increase the pressure of the reaction system to 3.0 MPa, and heat to 320°C to start the reaction.
[0071] The results of the catalytic reaction of carbon dioxide hydrogenation to α-olefins using the modified iron-based catalyst Fe—Mn—K—Al prepared in Example 6 are shown in Table 1.
[0072] Comparative Example 1
[0073] (1) Preparation of iron-based catalysts
[0074] 20.2gFe(NO3)3·9H2O, 0.97gCu(NO3)2·3H2O and 3.75gAl(NO3)3·9H2O were weighed and dissolved in 400mL deionized water, and the solution obtained after stirring was recorded as A. In addition, 15.68g of anhydrous K2CO3 solid was weighed and added to 100mL deionized water to prepare a solution with a concentration of 1.0mol / LK2CO3. Under 80℃ water bath conditions, A was added dropwise to the prepared K2CO3 solution, and titrated while stirring. The titration end point was pH=10. After aging, washing, drying at 50℃, and calcination (600℃) for 5h, the molar ratio of Fe-Cu-Al of the iron-based catalyst was 100:8:20.
[0075] (2) Evaluation of the reaction of hydrogenation of carbon dioxide to α-olefins catalyzed by iron-based catalysts
[0076] The iron-based catalyst Fe-Cu-Al was loaded in the constant temperature zone in the middle of the reaction tube, and 50g of 20-40 mesh quartz sand was loaded in the upper and lower parts of the reaction tube; the iron-based catalyst Fe-Cu-Al was reduced under the following conditions: temperature 350°C, flow rate 80mL / min, and reduction time 5h; after the reduction, the raw material was heated to 1000mL / (g / min) at a H2 / CO2 molar ratio of 3. cat h) Feed the materials, slowly increase the pressure of the reaction system to 3.0 MPa, and heat to 320°C to start the reaction.
[0077] The results of the catalytic reaction of the iron-based catalyst Fe-Cu-Al prepared in Comparative Example 1 on the hydrogenation of carbon dioxide to produce α-olefins are shown in Table 1.
[0078] Comparative Example 2
[0079] (1) Preparation of modified iron-based catalyst
[0080] Weigh 20.20g Fe(NO3)3·9H2O and 1.88g Al(NO3)3·9H2O and dissolve them in 400mL deionized water. The solution obtained after stirring is recorded as A. In addition, weigh 15.68g of anhydrous K2CO3 solid and add 100mL deionized water to prepare a solution with a concentration of 1.0mol / L K2CO3. In an 80℃ water bath, add A dropwise to the prepared K2CO3 solution and titrate while stirring. The titration end point is pH = 10. After aging, washing, drying at 50℃, and calcining at 600℃ for 5h, the molar ratio of Fe-Al catalyst is 100:10.
[0081] 0.28g K2CO3 was added to deionized water to prepare a 0.25mol / L K2CO3 solution, which was impregnated on the Fe-Al catalyst. After drying at 50°C and calcining at 600°C for 5h, the molar ratio of Fe-K-Al in the modified iron-based catalyst was 100:8:10.
[0082] (2) Evaluation of the reaction of carbon dioxide hydrogenation to α-olefins over modified iron-based catalysts
[0083] The modified iron-based catalyst Fe-K-Al was loaded in the constant temperature zone in the middle of the reaction tube, and 50g of 20-40 mesh quartz sand was loaded in the upper and lower parts of the reaction tube; the modified iron-based catalyst Fe-K-Al was reduced, and the reduction conditions were: temperature 350°C, flow rate 80mL / min, and reduction time 5h; after the reduction was completed, according to the H2 / CO2 molar ratio of 3, the raw material space velocity 1000mL / (g cat h) Feed the materials, slowly increase the pressure of the reaction system to 3.0 MPa, and heat to 320°C to start the reaction.
[0084] The results of the catalytic reaction of carbon dioxide hydrogenation to α-olefins using the modified iron-based catalyst Fe-Al-K prepared in Comparative Example 2 are shown in Table 1.
[0085] Table 1 Reaction results of carbon dioxide hydrogenation to α-olefins catalyzed by modified iron-based catalyst
[0086]
[0087]
[0088] In Table 1, is the conversion rate of CO2, C2-C3 = For olefin products with carbon chains from 2 to 3, C 4+ = For α-olefin products with carbon chains greater than or equal to 4, other C 2+ Other hydrocarbon products with carbon number ≥ 2.
[0089] From the data analysis in Table 1, it can be seen that in Comparative Example 2, the catalytic performance of the iron-based catalyst without adding transition metal oxide as a promoter is poor, the conversion rate of CO2 is only 32.8%, the selectivity of CO is high, and the products are mainly methane and other hydrocarbon products with a carbon number ≥ 2, and the selectivity of α-olefin products is only 21.8%. In Comparative Example 1, the catalytic performance of the iron-based catalyst without adding alkali metal oxide as a promoter is also poor, the selectivity of CO is high, the conversion rate of CO2 is only 36.2%, and the products are mainly methane and low-carbon alkanes, and the selectivity of α-olefin products is only 15.8%. In Examples 1 to 6, in the iron-based catalyst after adding transition metal and alkali metal additives at the same time, the selectivity of CO is significantly reduced, and the conversion rate of CO2 and the selectivity of α-olefin products are significantly increased. Among them, copper and zinc oxides have a greater impact on the performance of the iron-based catalyst. When the iron-based catalyst with transition metal copper oxide or zinc oxide as an additive is used to catalyze the reaction of hydrogenating carbon dioxide to produce α-olefins, the conversion rate of CO2 is increased to more than 40%, especially under the catalytic action of the catalyst Fe-Cu-Al-K, the conversion rate of CO2 is as high as 45%. In addition, the selectivity of α-olefin products is increased to more than 65%, and the selectivity of CO is less than 10%. Therefore, by adding transition metal and alkali metal additives to the iron-based catalyst at the same time, the selectivity of CO and CH4 can be greatly reduced. Selecting appropriate transition metal and alkali metal additives to add to the iron-based catalyst can greatly improve the selectivity of α-olefins, thereby obtaining a higher yield.
[0090] On the one hand, the present invention uses transition metal as an auxiliary agent to modify iron-based oxides, which significantly improves the reaction performance of iron-based oxides as catalysts. In particular, the Zn auxiliary agent in the transition metal can form a spinel-type composite oxide with the iron oxide, inhibiting the sintering of the catalyst and thus improving the stability of the catalytic reaction. In addition, the zinc oxide auxiliary agent can also regulate the distribution of the sodium oxide auxiliary agent in the catalyst, inhibiting the secondary adsorption hydrogenation process of olefins in the reaction; on the other hand, the alkaline earth metal auxiliary agent can further optimize the reaction performance of iron-based oxides as catalysts, wherein the sodium oxide auxiliary agent, as an alkaline oxide auxiliary agent, is conducive to the chemical adsorption of CO2 by the catalyst and inhibits the dissociative adsorption of H2, effectively improving the activity of the catalyst and olefin selectivity. And the sodium oxide auxiliary agent promotes the carburization of iron species, and the ratio of the active center Fe3O4 of the RWGS reaction and the active center Fe5C2 of the FTS reaction in the catalyst can be regulated by controlling the Na content, thereby improving the conversion rate of CO2 and inhibiting the generation of the intermediate species CO.
[0091] Among the various supports for iron-based catalysts, alumina has the advantages of high surface area, strong metal-support interaction and avoiding sintering of active components during the reaction, making it the optimal support for iron-based catalysts.
[0092] In summary, compared with the prior art, the present invention has the following advantages:
[0093] (1) The modified iron-based catalyst prepared by the present invention does not contain precious metals such as platinum, palladium, and rhenium, which can effectively reduce production costs;
[0094] (2) When the catalyst of the present invention is used for hydrogenation of carbon dioxide to produce α-olefins, the CO2 conversion rate can reach 45%, the CO and CH4 selectivities are less than 15%, and the α-olefin selectivity can reach more than 60%.
[0095] The foregoing description of specific exemplary embodiments of the present invention is for the purpose of illustration and demonstration. These descriptions are not intended to limit the present invention to the precise form disclosed, and it is clear that many changes and variations can be made based on the above teachings. The purpose of selecting and describing the exemplary embodiments is to explain the specific principles of the present invention and its practical application, so that those skilled in the art can realize and utilize various different exemplary embodiments of the present invention and various different selections and changes. The scope of the present invention is intended to be limited by the claims and their equivalents.
Claims
1. A modified iron-based catalyst for the hydrogenation of carbon dioxide to α-olefins, It is characterized in that Weigh 20.20 g Fe(NO 3 ) 3 9H 2 O, 0.72gCu(NO 3 ) 2 ·3H 2 O and 4.04gAl(NO 3 ) 3 9H 2 O was dissolved in 400 mL of deionized water and the solution obtained after stirring was recorded as A. In addition, 13.8 g of anhydrous K 2 CO 3 Add 100mL of deionized water to the solid to make a concentration of 1.0mol / LK 2 CO 3 In a water bath at 80°C, add A dropwise to the prepared K 2 CO 3 The solution was titrated while stirring, and the titration endpoint was pH = 10. After that, it was aged, washed, dried at 50°C, and calcined at 600°C for 5 hours to obtain an iron-based catalyst with a molar ratio of Fe-Cu-Al of 100:6:20; 0.14gK 2 CO 3 Add to deionized water to make 0.25mol / LK 2 CO 3 The solution was impregnated on an iron-based catalyst Fe-Cu-Al, dried at 50°C, and calcined at 600°C for 5 hours to obtain a modified iron-based catalyst Fe-Cu-K-Al with a molar ratio of 100:6:4:20.
Citation Information
Patent Citations
Catalyst for preparing low-carbon olefin by synthesized gas and its use
CN101024192A
Catalyst for hydrocarbon synthesis by CO2 catalytic hydrogenation and preparation method thereof
CN102309967A
Method for preparing low-carbon olefin catalyst through carbon dioxide hydrogenation
CN104624194A
Iron-based catalyst for low-carbon olefin production through CO2 hydrogenation, and preparation and applications thereof
CN106031871A
Preparation of iron-based catalyst for preparing alpha-alkene from carbon dioxide through hydrogenation, catalyst and application
CN108144617A
Cited By
A core-shell structured FeZnC@Al2O3 catalyst and its application in catalytic CO2 hydrogenation to α-olefins
CN120205193B