A preparation mold and preparation method of metal hollow sphere

By using a mold design that evenly distributed concave hemispherical pits and convex hemispherical columns in the preparation of metal hollow spheres, combined with mixed coating and segmented sintering technology of fused paraffin and metal powder, the pollution of metal hollow sphere preparation in the existing technology is solved. The density and cost issues have achieved efficient and uniform preparation of metal hollow spheres, meeting the high-performance needs in aviation and other fields.

CN115846660BActive Publication Date: 2024-11-05NORTHWEST INSTITUTE FOR NONFERROUS METAL RESEARCH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211553897.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-06
Publication Date
2024-11-05
Estimated Expiration
2042-12-06

AI Technical Summary

Technical Problem

The existing preparation methods for metal hollow spheres have problems such as template contamination, uneven spherical shells, high thickness, high cost and limited applicable materials. In particular, it is difficult to prepare metal hollow spheres less than 5mm and have low efficient production efficiency.

Method used

The lower die punch with the concave hemispherical pit uniformly distributed on the upper surface and the upper die punch with the convex hemispherical column uniformly distributed on the lower surface were combined. Through uniform mixing and coating of fused paraffin and metal powder and segmented sintering, the hole diameter and wall are prepared. Metal hollow balls with uniform thickness.

Benefits of technology

Achieve efficient preparation of multiple metal hollow spheres, ensuring uniformity of spherical shape, wall thickness and density, reducing production costs, and is suitable for high-performance porous materials in the fields of aviation, aerospace, etc., and supports porous metal materials of different structures. preparation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115846660B_ABST
    Figure CN115846660B_ABST
Patent Text Reader

Abstract

This invention discloses a mold for preparing a hollow metal sphere, comprising a lower die punch with multiple hemispherical pits evenly distributed on its upper surface, and female dies at both ends of the lower die punch with a height higher than the lower die punch. An upper die punch, which mates with the lower die punch and the female dies, is located on the upper part of the lower die punch. Several convex hemispherical pillars, each with a hemispherical end, are evenly distributed on the lower surface of the upper die punch and mate with the hemispherical pits. The invention also discloses a method for preparing a hollow metal sphere, in which a metal powder slurry is evenly coated onto the lower die punch and the mold is closed to obtain a hollow hemisphere. The hollow hemispheres are then assembled in pairs and sintered to obtain the hollow metal sphere. The hollow metal spheres prepared by this invention have a smooth surface, high sphericity, uniform size, and adjustable wall thickness, meeting the application requirements of materials and components for heat insulation and energy absorption in aerospace, petrochemical, and transportation fields. The preparation process is short, low-cost, and allows for mass production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of porous metal material preparation, and in particular relates to a preparation mold and a preparation method for metal hollow spheres. Background Art

[0002] Honeycomb and porous materials are often used in nature to create load-bearing and weight-optimized structures. Porous metal materials are composites composed of pores and metal skeletons. They have excellent filtering, sound absorption, heat transfer, catalysis and other properties. They have the intrinsic characteristics of metal materials and have been applied on a large scale in many fields of the national economy.

[0003] Metal hollow spheres are a new type of porous metal material with regular and easily reproducible geometric shapes, thus possessing stable mechanical and physical properties.

[0004] At present, the preparation methods of metal hollow spheres mainly include template method, replacement reaction method and 3D printing method. The template method is to coat metal powder on the surface of template (such as inorganic particles, metal particles, polymer particles, etc.), and then obtain hollow spheres by heat treatment or dissolution of the template, among which polymer particles are the most commonly used templates. Domestic and foreign scholars have published patents and papers on the preparation of metal hollow spheres by template method, and the material system includes titanium alloy (such as Ti6Al4V, Ti-7Ni-0.5B), stainless steel, etc. However, the template is very easy to contaminate the metal powder during the removal process, and the spherical shell is not dense and the thickness is uneven, resulting in low mechanical properties of the hollow sphere and anisotropy. The replacement reaction method is to immerse spherical iron particles in copper sulfate solution, and iron and copper undergo replacement reaction, copper is deposited on the surface of iron particles, and iron particles gradually dissolve to finally form copper hollow spheres, but the material system applicable to this method is limited. The 3D printing method is difficult to prepare metal hollow spheres below 5mm, the cost is high, and small holes need to be reserved in the spherical shell, otherwise the internal powder cannot be cleaned.

[0005] Based on the shortcomings of the above methods, it is necessary to provide a preparation mold and preparation method for metal hollow spheres. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a preparation mold for metal hollow balls in view of the above-mentioned deficiencies of the prior art. The mold is combined by a lower punch having a plurality of concave hemispherical pits evenly distributed on the upper surface and an upper punch having a plurality of convex hemispherical columns evenly distributed on the lower surface to match the concave hemispherical pits, and the concave hemispherical pits and the convex hemispherical columns are matched to prepare hollow hemispherical balls with a certain wall thickness, and multiple hollow hemispherical balls can be prepared at one time, with high production efficiency.

[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is: a preparation mold for metal hollow balls, characterized in that it includes a lower die punch with a plurality of concave hemispherical pits evenly distributed on the upper surface, both ends of the lower die punch are provided with a female die with a height higher than the lower die punch, an upper die punch is provided on the upper part of the lower die punch to cooperate with the lower die punch and the female die, and a plurality of convex hemispherical columns cooperating with the concave hemispherical pits are evenly distributed on the lower surface of the upper die punch, and the convex hemispherical columns are cylinders with convex hemispherical ends.

[0008] The above-mentioned metal hollow ball preparation mold is characterized in that a partition is provided on the lower die punch, and a through hole corresponding to the concave hemispherical pit is opened on the partition; the thickness of the partition is 0.15mm to 0.3mm.

[0009] The above-mentioned mold for preparing a metal hollow ball is characterized in that the diameter of the concave hemispherical pit is not greater than 5 mm, and the diameter of the convex hemispherical column is 0.6 to 0.8 times the diameter of the concave hemispherical pit.

[0010] The above-mentioned preparation mold for a metal hollow ball is characterized in that the length of the convex hemispherical column is 1.6 to 2.0 times the radius of the convex hemispherical column.

[0011] In addition, the present invention also provides a method for preparing a hollow metal sphere, characterized in that the method comprises the following steps:

[0012] Step 1, heating the paraffin to obtain molten paraffin;

[0013] Step 2: adding metal powder to the molten paraffin obtained in step 1, and then stirring to obtain a uniform metal powder slurry;

[0014] Step 3, evenly coating the metal powder slurry obtained in step 2 on the upper surface of the lower die punch, and then placing the partition plate on the upper surface of the lower die punch to obtain the lower die punch coated with the slurry;

[0015] Step 4: close the lower die punch and the upper die punch coated with the slurry obtained in step 3 to obtain a plurality of hollow hemispheres;

[0016] Step 5: Assemble the several hollow hemispheres obtained in step 4 in pairs to obtain hollow sphere green bodies, and then sinter them to obtain several metal hollow spheres.

[0017] The present invention mixes and stirs molten paraffin and metal powder to obtain uniform metal powder slurry, uniformly coats the metal powder slurry on the upper surface of a lower die punch and then closes the die with an upper die punch to prepare a plurality of hollow hemispheres at one time, and directly obtains a hollow hemisphere by arranging a partition after the lower die punch and the upper die punch are closed, and then the plurality of hollow hemispheres are assembled and sintered to obtain a metal hollow ball.

[0018] The above method is characterized in that the metal powder in step 2 is titanium alloy powder, aluminum alloy powder, magnesium alloy powder, stainless steel powder or nickel-based alloy powder; the mass ratio of molten paraffin and metal powder in the metal powder slurry is 7 to 36:100. The present invention prepares metal powders of different components by controlling the composition of the metal powder. These metal powders have excellent comprehensive properties such as low density, high specific strength, high specific stiffness, excellent corrosion resistance, high temperature resistance, low temperature resistance, non-magnetic, and weldability, which can meet the application requirements of aviation, aerospace, nuclear industry, weapons, ocean, petroleum, chemical industry, etc. The present invention uses two metal powders to prepare hollow hemispheres respectively, and then assembles them two by two to obtain composite metal hollow spheres, giving full play to the excellent mechanical properties and corrosion resistance of the two heterogeneous metals, while achieving the purpose of weight reduction, and meeting the needs of high-performance thermal insulation materials in the fields of aerospace, petrochemical industry, etc.; the present invention controls the mass ratio of molten paraffin and metal powder to ensure the uniformity of the metal powder slurry and the molding effect of the hollow hemisphere.

[0019] The above method is characterized in that the stirring in step 2 is performed under heating conditions. The present invention prevents the molten paraffin from solidifying by stirring under heating conditions, thereby ensuring that the metal powder slurry is in a fluid state, thereby ensuring that the metal powder slurry is evenly coated on the upper surface of the lower die punch.

[0020] The above method is characterized in that the concave hemispherical pit in the lower die punch coated with slurry in step 3 is filled with metal powder slurry. The present invention ensures that a hollow hemisphere can be formed in each concave hemispherical pit when the die is closed, thereby ensuring the quality of the hollow hemisphere.

[0021] The above method is characterized in that the pressure of the mold closing in step 4 is 0.4MPa to 0.6MPa, and the holding time is 2min to 5min. The present invention ensures the smooth molding of the hollow hemisphere by controlling the parameters of the mold closing.

[0022] The above method is characterized in that the sintering in step 5 is staged sintering, and the process of the staged sintering is: heating to 200°C-250°C at a heating rate of no more than 3°C / min and then keeping it warm for more than 30 minutes, then heating to 450°C-500°C at a heating rate of no more than 3°C / min and then keeping it warm for more than 30 minutes, and then heating to the final sintering temperature at a heating rate of 10°C / min and keeping it warm for 1h-2h, and the final sintering temperature is 0.7T m ~0.85T m , the T mThe present invention adopts segmented sintering to ensure that the paraffin is completely removed without destroying the overall structure of the hollow sphere, thereby ensuring that the two hollow hemispheres are metallurgically bonded and have a certain strength and rigidity.

[0023] Compared with the prior art, the present invention has the following advantages:

[0024] 1. The present invention combines a lower die punch having a plurality of concave hemispherical pits evenly distributed on the upper surface and an upper die punch having a plurality of convex hemispherical columns evenly distributed on the lower surface to cooperate with the concave hemispherical pits, and prepares a hollow hemisphere with a certain wall thickness through the cooperation of the concave hemispherical pits and the convex hemispherical columns. Multiple hollow hemispheres can be prepared at one time, and the production efficiency is high.

[0025] 2. The present invention provides female dies with a height higher than that of the lower die punch at both ends of the lower die punch to support the upper die punch when the lower die punch and the upper die punch are closed, thereby ensuring that the lower end of the convex hemispherical column does not contact the concave hemispherical pit and a certain space is formed to maintain the wall thickness of the hollow hemisphere. By adopting the convex hemispherical column as a cylinder with a convex hemispherical end, it is ensured that the convex hemispherical column can smoothly extend into the concave hemispherical pit.

[0026] 3. The present invention obtains a hollow hemisphere by uniformly applying a metal powder slurry to a lower die and then sintering the hollow hemispheres in pairs to obtain a metal hollow sphere. The prepared metal hollow spheres have uniform pore sizes, uniform and smooth pore walls, and pore structures that can be precisely controlled as needed. They have the characteristics of low density, high specific strength, and high specific stiffness. They can meet the great demands for metal hollow spheres and porous materials for energy absorption, sound insulation, and heat insulation in the fields of aviation, aerospace, transportation, machinery manufacturing, weapons and equipment, and construction. At the same time, the preparation process of the present invention is short, the cost is low, and mass production can be easily achieved, and they are suitable for preparing isotropic porous metal materials and components.

[0027] 4. The metal hollow spheres prepared by the present invention are easy to prepare structural units of porous metal materials and components with different spatial arrangements such as simple cubic structure, body-centered cubic structure, face-centered cubic structure, close-packed hexagonal structure and gradient structure, so as to meet the application requirements in different fields.

[0028] 5. The pore structure of the metal hollow spheres prepared by the present invention can be precisely controlled according to application requirements, thereby achieving synergistic control among density, compressive strength, stiffness and service performance.

[0029] 6. The preparation process of the present invention is short, the cost is low, and it is easy to achieve mass production.

[0030] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1It is a structural schematic diagram of the lower die punch and female die of the metal hollow ball preparation mold of the present invention.

[0032] Figure 2 The present invention is a schematic structural diagram of a die punch on a metal hollow ball preparation die.

[0033] Figure 3 The utility model is a schematic diagram of the connection relationship between the lower die punch, the female die and the partition plate of the metal hollow ball preparation mold of the present invention.

[0034] Figure 4 It is a schematic structural diagram of the hollow metal ball preparation mold during mold closing of the present invention.

[0035] Figure 5 This is a physical picture of the hollow sphere green body prepared in Example 2 of the present invention.

[0036] Figure 6 This is a physical picture of the titanium alloy hollow sphere prepared in Example 2 of the present invention.

[0037] Description of reference numerals:

[0038] 1—lower die punch; 1-1—concave hemispherical pit; 2—female die;

[0039] 3—upper die punch; 3-1—convex hemispherical column; 4—partition plate;

[0040] 4-1—Through hole. DETAILED DESCRIPTION

[0041] A preparation mold for a metal hollow sphere of the present invention is described in detail through Example 1.

[0042] Example 1

[0043] like Figure 1 and Figure 2 As shown, the preparation mold of the metal hollow ball in this embodiment includes a lower die punch 1 with a plurality of concave hemispherical pits 1-1 uniformly distributed on the upper surface, and female dies 2 with a height higher than the lower die punch 1 are arranged at both ends of the lower die punch 1, and an upper die punch 3 cooperating with the lower die punch 1 and the female die 2 is arranged on the upper part of the lower die punch 1, and a plurality of convex hemispherical columns 3-1 cooperating with the concave hemispherical pits 1-1 are uniformly distributed on the lower surface of the upper die punch 3, and the convex hemispherical columns 3-1 are cylinders with convex hemispherical ends.

[0044] It should be noted that, by closing the mold with a lower punch 1 having multiple concave hemispherical pits 1-1 evenly distributed on the upper surface and an upper punch 3 having multiple convex hemispherical columns 3-1 evenly distributed on the lower surface and cooperating with the concave hemispherical pits 1-1, hollow hemispheres with a certain wall thickness are prepared by the cooperation between the concave hemispherical pits 1-1 and the convex hemispherical columns 3-1. Multiple hollow hemispheres can be prepared at one time, and the production efficiency is high. By arranging female molds 2 with a height higher than the lower punch 1 at both ends of the lower punch 1, the upper punch 3 is supported when the lower punch 1 and the upper punch 3 are closed, ensuring that the lower ends of the convex hemispherical columns 3-1 do not contact the concave hemispherical pits 1-1 and form a certain space to maintain the wall thickness of the hollow hemisphere. By adopting the convex hemispherical column 3-1 as a cylinder with a convex hemispherical end, it is ensured that the convex hemispherical column 3-1 can smoothly extend into the concave hemispherical pit 1-1, and the hollow hemisphere is formed by the cooperation between the convex hemispherical end and the concave hemispherical pit 1-1.

[0045] like Figure 1 , Figure 2 , Figure 3 and Figure 4 As shown, in this embodiment, a partition plate 4 is provided on the lower die punch 1, and a through hole 4-1 corresponding to the concave hemispherical pit 1-1 is opened on the partition plate 4. By providing the partition plate 4 on the lower die punch 1, after the lower die punch 1 and the upper die punch 3 are molded and separated, a hollow hemisphere is directly obtained in the concave hemispherical pit 1-1.

[0046] It should be noted that the thickness of the partition 4 is 0.15 mm to 0.3 mm, preferably 0.15 mm, 0.2 mm, 0.25 mm, 0.3 mm, and the aperture of the through hole 4-1 is equal to the diameter of the concave hemispherical pit 1-1. By controlling the thickness of the partition 4 to be smaller than the height difference between the upper surface of the female mold 2 and the upper surface of the lower die punch 1, the smooth closing of the mold is ensured.

[0047] In this embodiment, the diameter of the concave hemispherical pit 1-1 is not greater than 5 mm, and the diameter of the convex hemispherical column 3-1 is smaller than the diameter of the concave hemispherical pit 1-1. A metal hollow sphere with a diameter less than 5 mm is prepared by controlling the diameter of the concave hemispherical pit 1-1, and the prepared hollow hemisphere has a certain wall thickness by making the diameter of the convex hemispherical column 3-1 smaller than the diameter of the concave hemispherical pit 1-1. The diameter of the convex hemispherical column 3-1 is determined according to specific requirements, thereby preparing the diameters of the convex hemispherical column 3-1 with different wall thicknesses.

[0048] In this embodiment, the length of the convex hemispherical column 3-1 is greater than the height difference between the upper surface of the female mold 2 and the upper surface of the lower die punch 1. By controlling the length of the convex hemispherical column 3-1 and the height difference between the upper surface of the female mold 2 and the upper surface of the lower die punch 1, it is ensured that the convex hemispherical structure at the front end of the convex hemispherical column 3-1 extends into the concave hemispherical pit 1-1.

[0049] It should be noted that the length of the convex hemispherical column 3-1 is 1.6 to 2.0 times the radius of the convex hemispherical sphere, preferably 1.6 times, 1.7 times, 1.8 times, 1.9 times and 2.0 times, and the height difference between the upper surface of the female mold 2 and the upper surface of the lower die punch 1 is 0.5 to 0.9 times the radius of the convex hemispherical sphere, preferably 0.5 times, 0.6 times, 0.7 times, 0.8 times, 0.9 times. By controlling the quantitative relationship between the length of the convex hemispherical column 3-1 and the radius of the convex hemispherical sphere, and controlling the height difference between the upper surface of the female mold 2 and the upper surface of the lower die punch 1, it is ensured that the convex hemispherical column 3-1 is smoothly extended into the concave hemispherical pit 1-1, and it is ensured that the lower end of the convex hemispherical column 3-1 does not contact the concave hemispherical pit 1-1 and forms a certain space, thereby maintaining the wall thickness of the hollow hemisphere, and forming a hollow hemisphere through the cooperation of the convex hemispherical end and the concave hemispherical pit 1-1.

[0050] The preparation method of the hollow metal sphere of the present invention is described in detail through Examples 2 to 8.

[0051] Example 2

[0052] This embodiment includes the following steps:

[0053] Step 1: Put 12 g of paraffin wax into a beaker and heat it to obtain molten paraffin wax;

[0054] Step 2: adding 100 g of titanium alloy powder to the molten paraffin obtained in step 1, and then stirring under heating conditions to obtain a uniform titanium alloy powder slurry;

[0055] Step 3: evenly apply the titanium alloy powder slurry obtained in step 2 to the upper surface of the lower die punch 1, and then place the partition 4 on the upper surface of the lower die punch 1 to obtain the lower die punch coated with the slurry;

[0056] Step 4: The lower die punch and the upper die punch 3 coated with the slurry obtained in step 3 are molded together to obtain a plurality of titanium alloy hollow hemispheres; the mold closing pressure is 0.5 MPa, and the pressure holding time is 3 minutes;

[0057] Step 5: Assemble the hollow hemispheres obtained in step 4 in pairs to obtain hollow sphere green bodies, and then sinter to obtain a plurality of titanium alloy hollow spheres; the sintering is staged sintering, and the staged sintering process is: heating to 230°C at a heating rate of no more than 3°C / min and then keeping warm for more than 30 minutes, then heating to 460°C at a heating rate of no more than 3°C / min and then keeping warm for more than 30 minutes, and then heating to the final sintering temperature at a heating rate of 10°C / min and keeping warm for 2 hours, and the final sintering temperature is 0.8T m , the T m is the melting point of titanium alloy powder.

[0058] After testing, the sphericity of the titanium alloy hollow sphere prepared in this embodiment is above 0.95, the wall thickness is 0.2 mm, and the density is 1.4 g / cm 3 .

[0059] Figure 5 This is a physical picture of the hollow sphere green body prepared in this embodiment. Figure 6 is a physical picture of the titanium alloy hollow sphere prepared in this embodiment. Figure 5 and Figure 6 It can be seen that the hollow sphere green body prepared in this embodiment has a smooth surface and high sphericity, and still maintains a complete spherical structure after sintering.

[0060] Example 3

[0061] This embodiment includes the following steps:

[0062] Step 1: Put 20 g of paraffin wax into a beaker and heat it to obtain molten paraffin wax;

[0063] Step 2: adding 100 g of aluminum alloy powder to the molten paraffin obtained in step 1, and then stirring under heating conditions to obtain a uniform aluminum alloy powder slurry;

[0064] Step 3: evenly apply the aluminum alloy powder slurry obtained in step 2 to the upper surface of the lower die punch 1, and then place the partition 4 on the upper surface of the lower die punch 1 to obtain the lower die punch coated with the slurry;

[0065] Step 4: close the die of the lower punch and the upper punch 3 coated with the slurry obtained in step 3 to obtain a plurality of hollow aluminum alloy hemispheres; the closing pressure is 0.6 MPa, and the holding time is 2 min;

[0066] Step 5: assemble the several hollow hemispheres obtained in step 4 in pairs to obtain hollow sphere green bodies, and then sinter to obtain several aluminum alloy hollow spheres; the sintering is staged sintering, and the staged sintering process is: heating to 250°C at a heating rate of no more than 3°C / min and then keeping warm for more than 30 minutes, then heating to 490°C at a heating rate of no more than 3°C / min and then keeping warm for more than 30 minutes, and then heating to the final sintering temperature at a heating rate of 10°C / min and keeping warm for 1 hour, and the final sintering temperature is 0.8T m , the T m is the melting point of aluminum alloy powder.

[0067] After testing, the titanium alloy hollow sphere prepared in this embodiment has a sphericity of more than 0.95, a wall thickness of 0.2 mm, and a density of 0.9 g / cm 3 .

[0068] Example 4

[0069] This embodiment includes the following steps:

[0070] Step 1: Put 36 g of paraffin wax into a beaker and heat it to obtain molten paraffin wax;

[0071] Step 2: adding 100 g of magnesium alloy powder to the molten paraffin obtained in step 1, and then stirring under heating conditions to obtain a uniform magnesium alloy powder slurry;

[0072] Step 3: evenly apply the magnesium alloy powder slurry obtained in step 2 to the upper surface of the lower die punch 1, and then place the partition 4 on the upper surface of the lower die punch 1 to obtain the lower die punch coated with the slurry;

[0073] Step 4: The lower die punch and the upper die punch 3 coated with the slurry obtained in step 3 are molded together to obtain a plurality of magnesium alloy hollow hemispheres; the mold closing pressure is 0.4 MPa, and the pressure holding time is 5 minutes;

[0074] Step 5: assemble the hollow hemispheres obtained in step 4 in pairs to obtain hollow sphere green bodies, and then sinter to obtain a plurality of magnesium alloy hollow spheres; the sintering is staged sintering, and the staged sintering process is: heating to 200°C at a heating rate of no more than 3°C / min and then keeping warm for more than 30 minutes, then heating to 480°C at a heating rate of no more than 3°C / min and then keeping warm for more than 30 minutes, and then heating to the final sintering temperature at a heating rate of 10°C / min and keeping warm for 1.5 hours, and the final sintering temperature is 0.8T m , the T m is the melting point of magnesium alloy powder.

[0075] After testing, the sphericity of the magnesium alloy hollow sphere prepared in this embodiment is above 0.95, the wall thickness is 0.2 mm, and the density is 0.55 g / cm 3 .

[0076] Example 5

[0077] This embodiment includes the following steps:

[0078] Step 1: Put 8 g of paraffin wax into a beaker and heat it to obtain molten paraffin wax;

[0079] Step 2: adding 100 g of stainless steel powder to the molten paraffin obtained in step 1, and then stirring under heating conditions to obtain a uniform stainless steel powder slurry;

[0080] Step 3: evenly apply the stainless steel powder slurry obtained in step 2 to the upper surface of the lower die punch 1, and then place the partition 4 on the upper surface of the lower die punch 1 to obtain the lower die punch coated with the slurry;

[0081] Step 4: The lower die punch and the upper die punch 3 coated with the slurry obtained in step 3 are molded together to obtain a plurality of stainless steel hollow hemispheres; the mold closing pressure is 0.5 MPa, and the pressure holding time is 4 minutes;

[0082] Step 5: assemble the several hollow hemispheres obtained in step 4 in pairs to obtain hollow sphere green bodies, and then sinter to obtain several stainless steel hollow spheres; the sintering is staged sintering, and the staged sintering process is: heating to 210°C at a heating rate of no more than 3°C / min and then keeping warm for more than 30 minutes, then heating to 460°C at a heating rate of no more than 3°C / min and then keeping warm for more than 30 minutes, and then heating to the final sintering temperature at a heating rate of 10°C / min and keeping warm for 1 hour, and the final sintering temperature is 0.75T m , the T m is the melting point of stainless steel powder.

[0083] After testing, the stainless steel hollow sphere prepared in this embodiment has a sphericity of more than 0.95, a wall thickness of 0.3 mm, and a density of 3.8 g / cm 3 .

[0084] Example 6

[0085] This embodiment includes the following steps:

[0086] Step 1: Put 7 g of paraffin wax into a beaker and heat it to obtain molten paraffin wax;

[0087] Step 2: adding 100 g of nickel-based alloy powder to the molten paraffin obtained in step 1, and then stirring under heating conditions to obtain a uniform nickel-based alloy powder slurry;

[0088] Step 3: evenly apply the nickel-based alloy powder slurry obtained in step 2 to the upper surface of the lower die punch 1, and then place the partition 4 on the upper surface of the lower die punch 1 to obtain the lower die punch coated with the slurry;

[0089] Step 4: The lower die punch and the upper die punch 3 coated with the slurry obtained in step 3 are molded together to obtain a plurality of nickel-based alloy hollow hemispheres; the mold closing pressure is 0.5 MPa, and the pressure holding time is 3 minutes;

[0090] Step 5: assemble the hollow hemispheres obtained in step 4 in pairs to obtain hollow sphere green bodies, and then sinter to obtain a plurality of nickel-based alloy hollow spheres; the sintering is staged sintering, and the staged sintering process is: heating to 220°C at a heating rate of no more than 3°C / min and then keeping warm for more than 30 minutes, then heating to 450°C at a heating rate of no more than 3°C / min and then keeping warm for more than 30 minutes, and then heating to the final sintering temperature at a heating rate of 10°C / min and keeping warm for 2 hours, and the final sintering temperature is 0.7T m ~0.85T m , the T m Is the melting point of nickel-based alloy powder.

[0091] After testing, the nickel-based alloy hollow sphere prepared in this embodiment has a sphericity of more than 0.95, a wall thickness of 0.2 mm, and a density of 2.7 g / cm 3 .

[0092] Example 7

[0093] This embodiment includes the following steps:

[0094] Step 1: Put 10 g of paraffin wax into a beaker and heat it to obtain molten paraffin wax;

[0095] Step 2: adding 100 g of nickel-based alloy powder to the molten paraffin obtained in step 1, and then stirring under heating conditions to obtain a uniform nickel-based alloy powder slurry;

[0096] Step 3: evenly apply the nickel-based alloy powder slurry obtained in step 2 to the upper surface of the lower die punch 1, and then place the partition 4 on the upper surface of the lower die punch 1 to obtain the lower die punch coated with the slurry;

[0097] Step 4: The lower die punch and the upper die punch 3 coated with the slurry obtained in step 3 are molded together to obtain a plurality of nickel-based alloy hollow hemispheres with a radius of 2.0 mm and a wall thickness of 0.2 mm; the mold closing pressure is 0.5 MPa, and the holding time is 4 minutes;

[0098] Step 5: Put 12 g of paraffin wax into a beaker and heat it to obtain molten paraffin wax;

[0099] Step 6: Add 100 g of titanium alloy powder to the molten paraffin obtained in step 5, and then stir under heating conditions to obtain a uniform titanium alloy powder slurry;

[0100] Step 7: evenly apply the titanium alloy powder slurry obtained in step 6 to the upper surface of the lower die punch 1, and then place the partition plate 4 on the upper surface of the lower die punch 1 to obtain the lower die punch coated with the slurry;

[0101] Step 8: The lower die punch and the upper die punch 3 coated with the slurry obtained in step 7 are molded together to obtain a plurality of titanium alloy hollow hemispheres with a radius of 1.8 mm and a wall thickness of 0.2 mm; the mold closing pressure is 0.5 MPa, and the holding time is 3 minutes;

[0102] Step nine, assembling the titanium alloy hollow hemisphere prepared in step eight and the nickel-based alloy hollow hemisphere prepared in step four in pairs to obtain hollow sphere green bodies, and then sintering to obtain a plurality of nickel-based alloy-titanium alloy composite hollow spheres; the sintering is a staged sintering, and the staged sintering process is: heating to 240°C at a heating rate of no more than 3°C / min and then keeping warm for more than 30 minutes, then heating to 500°C at a heating rate of no more than 3°C / min and then keeping warm for more than 30 minutes, and then heating to the final sintering temperature at a heating rate of 10°C / min and keeping warm for 1.5 hours, and the final sintering temperature is 0.7T m , the T m Is the melting point of nickel-based alloy powder.

[0103] After testing, the nickel-based alloy-titanium alloy composite hollow sphere prepared in this embodiment has a sphericity of more than 0.95, a wall thickness of 0.3 mm, and a density of 3.1 g / cm 3 .

[0104] Example 8

[0105] This embodiment includes the following steps:

[0106] Step 1: Put 8 g of paraffin wax into a beaker and heat it to obtain molten paraffin wax;

[0107] Step 2: adding 100 g of stainless steel powder to the molten paraffin obtained in step 1, and then stirring under heating conditions to obtain a uniform stainless steel powder slurry;

[0108] Step 3: evenly apply the stainless steel powder slurry obtained in step 2 to the upper surface of the lower die punch 1, and then place the partition 4 on the upper surface of the lower die punch 1 to obtain the lower die punch coated with the slurry;

[0109] Step 4: The lower die punch and the upper die punch 3 coated with the slurry obtained in step 3 are molded together to obtain a plurality of stainless steel hollow hemispheres with a radius of 2.5 mm and a wall thickness of 0.3 mm; the mold closing pressure is 0.6 MPa, and the pressure holding time is 3 min;

[0110] Step 5: Put 12 g of paraffin wax into a beaker and heat it to obtain molten paraffin wax;

[0111] Step 6: Add 100 g of titanium alloy powder to the molten paraffin obtained in step 5, and then stir under heating conditions to obtain a uniform titanium alloy powder slurry;

[0112] Step 7: evenly apply the titanium alloy powder slurry obtained in step 6 to the upper surface of the lower die punch 1, and then place the partition plate 4 on the upper surface of the lower die punch 1 to obtain the lower die punch coated with the slurry;

[0113] Step 8: The lower die punch and the upper die punch 3 coated with the slurry obtained in step 7 are molded together to obtain a plurality of titanium alloy hollow hemispheres with a radius of 1.8 mm and a wall thickness of 0.2 mm; the mold closing pressure is 0.5 MPa, and the holding time is 3 minutes;

[0114] Step nine, assembling the titanium alloy hollow hemisphere prepared in step eight and the stainless steel hollow hemisphere prepared in step four in pairs to obtain a hollow sphere green body, and then sintering to obtain a plurality of stainless steel-titanium alloy composite hollow spheres; the process of the segmented sintering is: heating to 220°C at a heating rate of no more than 3°C / min and then keeping it warm for more than 30 minutes, then heating to 470°C at a heating rate of no more than 3°C / min and then keeping it warm for more than 30 minutes, and then heating to the final sintering temperature at a heating rate of 10°C / min and keeping it warm for 2 hours, and the final sintering temperature is 0.85T m , the T m is the melting point of the metal powder.

[0115] After testing, the stainless steel-titanium alloy composite hollow sphere prepared in this embodiment has a sphericity of more than 0.95, a wall thickness of 0.4 mm, and a density of 2.8 g / cm 3 .

[0116] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A preparation mold for a metal hollow ball, It is characterized in that The invention comprises a lower die punch (1) having a plurality of concave hemispherical pits (1-1) uniformly distributed on the upper surface, a female die (2) having a height higher than that of the lower die punch (1) being arranged at both ends of the lower die punch (1), an upper die punch (3) cooperating with the lower die punch (1) and the female die (2) being arranged on the upper part of the lower die punch (1), a plurality of convex hemispherical columns (3-1) cooperating with the concave hemispherical pits (1-1) being uniformly distributed on the lower surface of the upper die punch (3), the convex hemispherical columns (3-1) being cylinders with convex hemispherical ends; a partition plate (4) being arranged on the lower die punch (1), and a through hole (4-1) corresponding to the concave hemispherical pits (1-1) being opened on the partition plate (4); The method for preparing a hollow metal ball by using a mold comprises the following steps: Step 1, heating the paraffin to obtain molten paraffin; Step 2: adding metal powder to the molten paraffin obtained in step 1, and then stirring to obtain a uniform metal powder slurry; Step 3: evenly apply the metal powder slurry obtained in step 2 to the upper surface of the lower die punch (1), and then place the partition (4) on the upper surface of the lower die punch (1) to obtain the lower die punch coated with the slurry; Step 4: close the lower die and upper die (3) coated with the slurry obtained in step 3 to obtain a plurality of hollow hemispheres; Step 5: Assemble the several hollow hemispheres obtained in step 4 in pairs to obtain hollow sphere green bodies, and then sinter them to obtain several metal hollow spheres.

2. A mold for preparing a metal hollow sphere according to claim 1, It is characterized in that The diameter of the concave hemispherical pit (1-1) is no greater than 5 mm, and the diameter of the convex hemispherical column (3-1) is smaller than the diameter of the concave hemispherical pit (1-1).

3. A preparation mold for a metal hollow sphere according to claim 1, It is characterized in that The length of the convex hemispherical column (3-1) is greater than the height difference between the upper surface of the female die (2) and the upper surface of the lower die punch (1).

4. A preparation mold for a metal hollow sphere according to claim 1, It is characterized in that The metal powder in step 2 is titanium alloy powder, aluminum alloy powder, magnesium alloy powder, stainless steel powder or nickel-based alloy powder; the mass ratio of molten paraffin and metal powder in the metal powder slurry is 7 to 36:

100.

5. A preparation mold for a metal hollow sphere according to claim 1, It is characterized in that The stirring in step 2 is carried out under heating conditions.

6. A preparation mold for a metal hollow sphere according to claim 1, It is characterized in that The concave hemispherical pit (1-1) in the lower die punch coated with the slurry in step 3 is filled with metal powder slurry.

7. A preparation mold for a metal hollow sphere according to claim 1, It is characterized in that The mold closing pressure in step 4 is 0.4MPa to 0.6MPa, and the pressure holding time is 2min to 5min.

8. A preparation mold for a metal hollow sphere according to claim 1, It is characterized in that The sintering in step 5 is staged sintering, and the process of staged sintering is: heating to 200°C-250°C at a heating rate of no more than 3°C / min, and then keeping the temperature for more than 30 minutes, then heating to 450°C-500°C at a heating rate of no more than 3°C / min, and then keeping the temperature for more than 30 minutes, and then heating to the final sintering temperature at a heating rate of 10°C / min, and then keeping the temperature for 1h-2h, and the final sintering temperature is 0.7T m ~0.85T m , the T m is the melting point of the metal powder.