A nine-layer co-extruded barrier film with self-sealing and easy-to-open function and its preparation process
By using a specific resin ratio and processing technology for a nine-layer co-extruded barrier film, the problem of unstable peelability after heat sealing of the co-extruded film was solved, achieving stable peelability and improved barrier performance.
Patent Information
- Application Number
- CN202211405064.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-10
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-11-10
AI Technical Summary
Existing co-extruded films are prone to peeling after heat sealing, have unstable performance, and are susceptible to stringing and delamination, affecting their performance.
The film employs a nine-layer co-extruded barrier film structure, including outer layer A, second outer layer B, second outer layer C, adhesive layer D, core layer E, adhesive layer F, second inner layer G, second inner layer H, and inner layer I. Through specific resin ratios and processing techniques, it is ensured that the film is easy to peel off after heat sealing, and the peeling interface is smooth and free of fuzz.
It achieves stable and easy-to-peel properties of the film after heat sealing, with a clean peeling interface, no stringing or delamination, which broadens the application range and improves the barrier performance.
Smart Images

Figure CN115847972B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of packaging materials, in particular to a nine-layer co-extruded barrier film which is self-sealing and easy to peel off and a preparation process thereof. Background Art
[0002] In the food field, a wide variety of packaging materials and forms attract many consumers. It is precisely because of the rapid development of packaging materials that the packaging industry has more opportunities, but it also faces challenges, such as competition from peers, the monopoly of foreign special materials, etc. Nowadays, with the development of the market, composite sheet packaging has become a special direction, especially in the cheese market boom in the past two years, it plays an important role.
[0003] According to Euromonitor data, the scale of China's cheese market (in terms of retail sales) reached 5.833 billion yuan in 2018, a year-on-year increase of 16.8%, with a compound growth rate of 22.5% from 2004 to 2018, and the market scale is expected to increase to 10.53 billion yuan in 2023. It is precisely because of the optimism about the cheese market that major manufacturers have also carried out in-depth cooperation in the cheese field, and the growth momentum of cheese sales revenue is strong.
[0004] Among the cheese stick composite materials, there is a functional film that needs to be easy to peel off. The film needs to have stable heat-sealing strength and needs to be easy to peel off after heat sealing. However, many existing co-extruded films in China have unstable peeling strength after sealing, and large areas of wire drawing will occur when peeling horizontally, affecting the use effect. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a nine-layer co-extruded barrier film which is self-sealing and easy to peel off and a preparation process thereof. The film of the invention not only has stable peeling strength, but also has a clean peeling interface without undesirable phenomena such as fuzzing, wire drawing, and delamination.
[0006] In order to achieve one of the purposes of the present invention, the present invention adopts the following technical solutions:
[0007] A nine-layer co-extruded barrier film which is self-sealing and easy to peel off, the film consists of an outer layer A, a sub-outer layer B2, a sub-outer layer C, an adhesive layer D, a core layer E, an adhesive layer F, a sub-inner layer G, a sub-inner layer H and an inner layer I, the outer layer A comprises 45-55 parts by weight of metallocene polyethylene and 45-55 parts by weight of linear low-density polyethylene; the sub-outer layer B and the sub-inner layer H each comprise 45-55 parts by weight of high-density polyethylene and 45-55 parts by weight of low-density polyethylene; the sub-outer layer C and the sub-inner layer G each comprise 70-80 parts by weight of high-density polyethylene and 20-30 parts by weight of polyolefin thermoplastic resin; the adhesive layer D and the adhesive layer F each comprise 100 parts by weight of polyolefin adhesive resin; the core layer E comprises 100 parts of vinyl alcohol-ethylene polymer resin; the inner layer I comprises 10-20 parts by weight of easy-to-peel resin and 80-90 parts by weight of low-density polyethylene.
[0008] Preferably, the outer layer A comprises 55 parts by mass of metallocene polyethylene and 45 parts by mass of linear low-density polyethylene; the sub-outer layer B and the sub-inner layer H each comprise 55 parts by mass of high-density polyethylene and 45 parts by mass of low-density polyethylene; the sub-outer layer C and the sub-inner layer G each comprise 70 parts by mass of high-density polyethylene and 30 parts by mass of polyolefin thermoplastic resin; the inner layer I comprises 15 parts by mass of easy-release resin and 85 parts by mass of low-density polyethylene.
[0009] Preferably, the grade of metallocene polyethylene is 2010MA produced by Exxon; the grade of linear low-density polyethylene is 1002AY produced by Exxon; the grade of high-density polyethylene is FB5600 produced by Borouge Chemical Company; the grade of low-density polyethylene is 100AC produced by Exxon; the grade of polyolefin thermoplastic resin is PL1880G produced by Dow Chemical Company; the grade of polyolefin adhesive resin is PX3747 produced by Basel Company; the grade of vinyl alcohol-ethylene polymer resin is DC3203FB produced by Japan Gode Chemical Company; the grade of easy-release resin is Sealution 210 produced by Dow Chemical Company.
[0010] Preferably, the thickness ratio of the outer layer A, the sub-outer layer B, the sub-outer layer C, the adhesive layer D, the core layer E, the adhesive layer F, the sub-inner layer G, the sub-inner layer H and the inner layer I is 2:1:2:2:3:2:2:1:2.
[0011] Preferably, the thickness of the adhesive layer D and the adhesive layer F are both 4 um; the thickness of the core layer E is 6 um.
[0012] In order to achieve the second object of the present invention, a preparation process of a nine-layer co-extruded barrier film having self-sealing and easy-to-open properties is provided, comprising the following steps:
[0013] S1. According to the formula composition of each layer in the film, weigh the components of each mass and put them into nine extruders respectively. The resin is melted at high temperature in the extruder to form a fluid melt;
[0014] S2, the melt is filtered through a filter screen, and then passes through a die distributor and an annular die in sequence to form a bubble tube film, and is cooled and shaped under an internal air cooling device and an external air cooling device;
[0015] S3. The shaped film is stretched forward by a rotating device and a traction device, and then passes through a thickness measuring system, a deflection system, a corona treatment system, and a trimming device in sequence, and finally is rolled into a roll film by a winding device, thereby obtaining a nine-layer co-extruded barrier film that is self-sealing and easy to peel off.
[0016] Preferably, the processing temperatures of the nine extruders in step S1 are as follows:
[0017] The extrusion temperatures of the outer layer A extruder are 50°C, 185°C, 190°C, 195°C, 200°C, 200, 200°C;
[0018] The extrusion temperatures of the secondary outer layer B extruder are: 60°C, 190°C, 195°C, 200°C, 205°C, 205°C, 205°C;
[0019] The extrusion temperatures of the C3 extruder of the secondary outer layer were 60°C, 190°C, 195°C, 200°C, 205°C, 205°C, and 205°C respectively;
[0020] The extrusion temperatures of the adhesive layer D extruder are: 80°C, 210°C, 215°C, 220°C, 220°C, 220°C, 220°C;
[0021] The extrusion temperatures of the core layer E extruder are 100°C, 215°C, 220°C, 220°C, 220°C, 220°C, 220°C;
[0022] The extrusion temperatures of the adhesive layer F extruder are: 80°C, 210°C, 215°C, 220°C, 220°C, 220°C, 220°C;
[0023] The extrusion temperatures of the sub-inner layer G extruder were 60°C, 190°C, 195°C, 200°C, 205°C, 205°C, and 205°C respectively;
[0024] The extrusion temperatures of the secondary inner layer H extruder were 60°C, 190°C, 195°C, 200°C, 205°C, 205°C, and 205°C respectively;
[0025] The extrusion temperatures of the inner layer I extruder are 50°C, 185°C, 190°C, 195°C, 200°C, 200°C, and 200°C respectively;
[0026] The temperatures in the die zone are: 220℃, 220℃, 220℃, 220℃, 220℃, 220℃, 220℃, 220℃, 220℃, 220℃, 220℃, 220℃ respectively.
[0027] The temperatures of the die zones are: 220℃, 220℃, 220℃, 220℃, 220℃, 220℃, 220℃, 220℃, 220℃, 220℃, 220℃, 220℃, and 220℃ respectively. There are 12 heating zones in the die.
[0028] Preferably, the screw diameters of the nine extruders are 70 mm, 60 mm, 60 mm, 50 mm, 50 mm, 50 mm, 60 mm, 60 mm and 70 mm respectively; the die head diameter of the extruder is 500 mm; and the extrusion capacity of the extruder is 580±20 kg / h.
[0029] Preferably, the filter screen is 70 mesh / 90 mesh / 100 mesh / 90 mesh.
[0030] Preferably, the traction speed of the traction device is 55±5 m / min; the traction tension is 90±10 N; the contact roller tension of the winding device is 30±10 N; and the winding tension is 40±10 N.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] 1) The present invention improves the easy-to-peel performance and peeling state of the easy-to-peel material through special resin selection, easy-to-process layer thickness ratio structure design, and optimization of the production process, especially the easy-to-peel material in various directions after heat sealing, and the peeling strength is stable, which broadens the application range of easy-to-peel products; the present invention adopts a nine-layer co-extrusion blown film method for film preparation, and can develop and manufacture multi-layer barrier performance materials; at the same time, by adding barrier resin, the barrier performance of the packaging material can be effectively improved, thereby enriching the application range of the product, and can be applicable to various fields such as food packaging.
[0033] 2) The present invention improves the formula composition of each layer, which is beneficial to the equipment screw matching processing. The outer layer A uses reinforced polyethylene and linear low-density polyethylene, which is beneficial to improving the bonding strength with other materials during film application and composite processes, thereby improving the composite strength between different materials.
[0034] 3) In the present invention, the sub-outer layer B and the sub-outer layer C, the sub-inner layer G and the sub-inner layer H use high-density polyethylene (brand name FB5600 produced by Borouge Chemical Company), aiming to increase the rigidity and longitudinal tearability of the film, which is beneficial to alleviate the problem of die-cutting wiredrawing, and at the same time can make up for the insufficient moisture barrier performance of vinyl alcohol-ethylene polymer resin (brand name DC3203FB produced by Japan Gode Chemical Company); adding a certain proportion of low-density polyethylene to the sub-outer layer B and the sub-inner layer H can effectively improve the smoothness of film processing and the stability of the bubble; adding a certain proportion of polyolefin thermoplastic resin (brand name PL1880G produced by Dow Chemical Company) to the sub-outer layer C and the sub-inner layer G helps to improve the bonding strength between high-density polyethylene and the adhesive layer resin and prevent the material from delamination.
[0035] 4) The adhesive layer D and the adhesive layer F of the present invention use polyolefin adhesive resin (brand name: PX3747 produced by Basel Company), which can enhance the bonding force between the vinyl alcohol-ethylene polymer resin of the core layer and the polyethylene material.
[0036] 5) The core layer E of the present invention adopts vinyl alcohol-ethylene polymer resin (DC3203FB produced by Japan Gode Chemical Co., Ltd.), which can effectively improve the barrier properties of the film (especially the permeability of gases such as water vapor and oxygen), and broaden the application range of the film.
[0037] 6) The inner layer I adopts a ratio of 15% easy-to-peel resin (Sealution 210 produced by Dow Chemical Company) + 70% low-density polyethylene (100AC produced by Exxon Corporation), which can effectively improve the heat-sealing strength of the inner layer easy-to-peel resin, so that the peeling force after heat sealing is stabilized between 4N / 15mm-7N / 15mm, and the phenomenon of peeling is prevented. The film has stable heat-sealing strength and a wide heat-sealing range, and the film is easy to peel after heat sealing, suitable for easy peeling in any direction, and will not produce peeling. The added easy-to-peel resin has a main function of easy peeling performance, so that the co-extruded film can be peeled in an embedded manner, and the peeling is smooth, and there will be no surface bounce after peeling.
[0038] 7) The layer thickness ratio of the symmetrical structure is beneficial to slow down the curling of the film; the thickness of the adhesive layers D and F are 4um respectively, which can effectively improve the adhesion between the core layer E and the sub-outer layer C and the sub-inner layer G; the thickness of the core layer E is 6um, which can effectively improve the oxygen barrier performance of the film.
[0039] 8) The film of the present invention is a self-sealing material (i.e., the heat sealing of the inner layer and the inner layer of the film is achieved on the packaging equipment), and can achieve the easy-to-peel function after sealing, and the peeling interface is clean without undesirable phenomena such as fuzzing, wire drawing, and delamination; the film has a wide functional range, that is, within the temperature processing range of 125°C-160°C, the heat sealing strength is stable and the easy-to-peel force is stable.
[0040] 9) When preparing the film, the extrusion temperature is gradually increased to a stable level. Different resins require different processing temperatures, which depends on key factors such as the melting point and melt index of the resin. During the processing of the resin, a gradual temperature increase is required to prevent the resin from denaturing or coking due to sudden changes in temperature. In addition, impurities will be generated during the process of the resin forming a melt in the extruder, or impurities will enter the extruder during the feeding process. Therefore, a filter is needed to filter out the impurities. The size of the filter depends on the mesh size, and the efficiency of removing impurities with different mesh sizes is different.
[0041] 10) The entire film blowing equipment includes components such as a suction device, an extruder device, a die head device, a traction device, a thickness measuring device, and a winding device. The extrusion volume in the preparation process is the total weight of the resin extruded by all extruders in a certain period of time; the traction speed is the working speed of the film production process; the traction tension is the tensile tension in the film production process; the contact roller refers to the auxiliary roller used when the film is wound to better solve the problem of the appearance of the film, and the contact roller is an active guide roller; the winding tension refers to the force required for the film when it is wound. If the winding tension is too small, it will be difficult to wind, and if the tension is too large, the film will easily deform. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 It is a structural diagram of the present invention.
[0043] Figure 2 It is a schematic diagram of the process of the present invention.
[0044] Figure 3 It is a structural diagram of the present invention.
[0045] The meanings of the symbols in the accompanying drawings are as follows:
[0046] 1-outer layer A, 2-sub-outer layer B, 3-sub-outer layer C, 4-adhesive layer D, 5-core layer E, 6-adhesive layer F, 7-sub-inner layer G, 8-sub-inner layer H, 9-inner layer I. DETAILED DESCRIPTION
[0047] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the following Figure 1-3 The present invention is further described in detail with reference to the embodiments. All other embodiments obtained by ordinary technicians in the field without creative work based on the embodiments of the present invention shall fall within the scope of protection of the present invention.
[0048] A nine-layer co-extruded barrier film with self-sealing and easy-to-open properties and a preparation process thereof, wherein the film consists of an outer layer A1, a sub-outer layer B2, a sub-outer layer C3, an adhesive layer D4, a core layer E5, an adhesive layer F6, a sub-inner layer G7, a sub-inner layer H8 and an inner layer I9, the outer layer A1 comprises 45-55 parts by weight of metallocene polyethylene and 45-55 parts by weight of linear low-density polyethylene; the sub-outer layer B2 and the sub-inner layer H8 both comprise 45-55 parts by weight of high-density polyethylene and 45-55 parts by mass of low-density polyethylene; the sub-outer layer C3 and the sub-inner layer G7 each include 70-80 parts by mass of high-density polyethylene and 20-30 parts by mass of polyolefin thermoplastic resin; the adhesive layer D4 and the adhesive layer F6 each include 100 parts by mass of polyolefin adhesive resin; the core layer E5 includes 100 parts of vinyl alcohol-ethylene polymer resin; the inner layer I9 contains 10-20 parts by mass of easy-to-release resin and 80-90 parts by mass of low-density polyethylene.
[0049] Specifically, the brand of metallocene polyethylene is 2010MA produced by Exxon; the brand of linear low-density polyethylene is 1002AY produced by Exxon; the brand of high-density polyethylene is FB5600 produced by Borouge Chemical Company; the brand of low-density polyethylene is 100AC produced by Exxon; the brand of polyolefin thermoplastic resin is PL1880G produced by Dow Chemical Company; the brand of polyolefin adhesive resin is PX3747 produced by Basel Company; the brand of vinyl alcohol-ethylene polymer resin is DC3203FB produced by Japan Godsei Chemical Company; the brand of easy-release resin is Sealution produced by Dow Chemical Company 210; the layer thickness ratio of outer layer A1, sub-outer layer B2, sub-outer layer C3, adhesive layer D4, core layer E5, adhesive layer F6, sub-inner layer G7, sub-inner layer H8 and inner layer I9 is 2:1:2:2:3:2:2:1:2; the thickness of adhesive layer D4 and adhesive layer F6 are both 4um; the thickness of core layer E5 is 6um.
[0050] Example 1
[0051] S1. According to the composition of each layer in the film, the outer layer A1 weighs 45 parts by mass of metallocene polyethylene and 55 parts by mass of linear low-density polyethylene; the sub-outer layer B2 and the sub-inner layer H8 weigh 45 parts by mass of high-density polyethylene and 55 parts by mass of low-density polyethylene; the sub-outer layer C3 and the sub-inner layer G7 weigh 80 parts by mass of high-density polyethylene and 20 parts by mass of polyolefin thermoplastic resin; the adhesive layer D4 and the adhesive layer F6 weigh 100 parts by mass of polyolefin adhesive resin; the core layer E5 weighs 100 parts of vinyl alcohol-ethylene polymer resin; the inner layer I9 weighs 10 parts by mass of easy-to-release resin and 90 parts by mass of low-density polyethylene, and puts them into nine extruders respectively. The resin is melted at high temperature in the extruder to form a fluid melt;
[0052] S2, the melt is filtered through a filter screen, and then passes through a die distributor and an annular die in sequence to form a bubble tube film, and is cooled and shaped under an internal air cooling device and an external air cooling device;
[0053] S3. The shaped film is stretched forward by a rotating device and a traction device, and then passes through a thickness measuring system, a deflection system, a corona treatment system, and a trimming device in sequence, and finally is rolled into a roll film by a winding device, thereby obtaining a nine-layer co-extruded barrier film 1 that is self-sealing and easy to peel off.
[0054] Example 2
[0055] S1, according to the formulation of each layer in the film, the outer layer A1 includes 55 parts by mass of metallocene polyethylene and 45 parts by mass of linear low-density polyethylene; the sub-outer layer B2 and the sub-inner layer H8 each include 55 parts by mass of high-density polyethylene and 45 parts by mass of low-density polyethylene; the sub-outer layer C3 and the sub-inner layer G7 each include 70 parts by mass of high-density polyethylene and 30 parts by mass of polyolefin thermoplastic resin; the adhesive layer D4 and the adhesive layer F6 each weigh 100 parts by mass of polyolefin adhesive resin; the core layer E5 each weighs 100 parts of vinyl alcohol-ethylene polymer resin; the inner layer I9 contains 15 parts by mass of easy-to-release resin and 85 parts by mass of low-density polyethylene, which are respectively put into nine extruders, and the resin is melted at high temperature in the extruder to form a fluid melt;
[0056] S2, the melt is filtered through a filter screen, and then passes through a die distributor and an annular die in sequence to form a bubble tube film, and is cooled and shaped under an internal air cooling device and an external air cooling device;
[0057] S3. The shaped film is stretched forward by a rotating device and a traction device, and then passes through a thickness measuring system, a deflection system, a corona treatment system, and a trimming device in sequence, and finally is rolled into a roll film by a winding device, thereby obtaining a nine-layer co-extruded barrier film 2 that is self-sealing and easy to peel off.
[0058] Example 3
[0059] S1. According to the composition of each layer in the film, the outer layer A1 weighs 50 parts by mass of metallocene polyethylene and 50 parts by mass of linear low-density polyethylene; the sub-outer layer B2 and the sub-inner layer H8 weigh 50 parts by mass of high-density polyethylene and 50 parts by mass of low-density polyethylene; the sub-outer layer C3 and the sub-inner layer G7 weigh 75 parts by mass of high-density polyethylene and 25 parts by mass of polyolefin thermoplastic resin; the adhesive layer D4 and the adhesive layer F6 weigh 100 parts by mass of polyolefin adhesive resin; the core layer E5 weighs 100 parts of vinyl alcohol-ethylene polymer resin; the inner layer I9 weighs 20 parts by mass of easy-to-release resin and 80 parts by mass of low-density polyethylene, and puts them into nine extruders respectively. The resin is melted at high temperature in the extruder to form a fluid melt;
[0060] S2, the melt is filtered through a filter screen, and then passes through a die distributor and an annular die in sequence to form a bubble tube film, and is cooled and shaped under an internal air cooling device and an external air cooling device;
[0061] S3, the shaped film is stretched forward by a rotating device and a traction device, and then passes through a thickness measuring system, a deflection system, a corona treatment system, and a trimming device in sequence, and finally is rolled into a roll film by a winding device, thereby obtaining a nine-layer co-extruded barrier film 3 that is self-sealing and easy to peel off.
[0062] Specifically, in the above embodiments 1-3, the processing temperatures of the nine extruders in step S1 are as follows:
[0063] The extrusion temperatures of the outer layer A1 extruder are: 50℃, 185℃, 190℃, 195℃, 200℃, 200, 200℃; the extrusion temperatures of the sub-outer layer B2 extruder are: 60℃, 190℃, 195℃, 200℃, 205℃, 205℃, 205℃; the extrusion temperatures of the sub-outer layer C3 extruder are: 60℃, 190℃, 195℃, 200℃, 205℃, 205℃, 205℃; the extrusion temperatures of the adhesive layer D4 extruder are: 80℃, 210℃, 215℃, 220℃, 220℃, 220℃, 220℃; the extrusion temperatures of the core layer E5 extruder are: 100℃, 215℃, 220℃, 220℃, 220℃, 220℃, 220℃; the extrusion temperatures of the adhesive layer F6 extruder are: The extrusion temperatures are: 80℃, 210℃, 215℃, 220℃, 220℃, 220℃, 220℃; the extrusion temperatures of the sub-inner layer G7 extruder are: 60℃, 190℃, 195℃, 200℃, 205℃, 205℃, 205℃; the extrusion temperatures of the sub-inner layer H8 extruder are: 60℃, 190℃, 195℃, 200℃, 205℃, 205℃, 205℃; the extrusion temperatures of the inner layer I9 extruder are: 50℃, 185℃, 190℃, 195℃, 200℃, 200℃, 200℃; the die zone temperatures are: 220℃, 220℃, 220℃, 220℃, 220℃, 220℃, 220℃, 220℃, 220℃, 220℃, 220℃, 220℃.
[0064] The screw diameters of the nine extruders are 70mm, 60mm, 60mm, 50mm, 50mm, 50mm, 60mm, 60mm and 70mm respectively; the die diameter of the extruder is 500mm. The filter screens are 70 mesh / 90 / mesh / 100 mesh / 90 mesh. The extrusion capacity of the extruder is 580±20kg / h; the traction speed of the traction device is 55±5m / min; the traction tension is 90±10N; the contact roller tension of the winding device is 30±10N; and the winding tension is 40±10N. The present invention adopts a film blowing process, and the film blowing requires a ring die of a special color, and the resin in the extruder passes through the ring die to form a bubble tube film (a certain air intake device is required in the bubble tube).
[0065] Comparative Example 1
[0066] S1, according to the formulation of each layer in the film, the outer layer A1 includes 55 parts by mass of metallocene polyethylene and 45 parts by mass of linear low-density polyethylene; the sub-outer layer B2 and the sub-inner layer H8 each include 55 parts by mass of high-density polyethylene and 45 parts by mass of low-density polyethylene; the sub-outer layer C3 and the sub-inner layer G7 each include 70 parts by mass of high-density polyethylene and 30 parts by mass of polyolefin thermoplastic resin; the adhesive layer D4 and the adhesive layer F6 each weigh 100 parts by mass of polyolefin adhesive resin; the core layer E5 each weighs 100 parts of vinyl alcohol-ethylene polymer resin; the inner layer I9 contains 50 parts by mass of easy-to-release resin and 50 parts by mass of low-density polyethylene, which are respectively put into nine extruders, and the resin is melted at high temperature in the extruder to form a fluid melt;
[0067] S2, the melt is filtered through a filter screen, and then passes through a die distributor and an annular die in sequence to form a bubble tube film, and is cooled and shaped under an internal air cooling device and an external air cooling device;
[0068] S3, the shaped film is stretched forward by a rotating device and a traction device, and then passes through a thickness measuring system, a deflection system, a corona treatment system, and a trimming device in sequence, and finally is rolled into a roll film by a winding device, thereby obtaining a nine-layer co-extruded barrier film 4 that is self-sealing and easy to peel off.
[0069] Comparative Example 2
[0070] S1, according to the formulation of each layer in the film, the outer layer A1 includes 55 parts by mass of metallocene polyethylene and 45 parts by mass of linear low-density polyethylene; the sub-outer layer B2 and the sub-inner layer H8 each include 55 parts by mass of high-density polyethylene and 45 parts by mass of low-density polyethylene; the sub-outer layer C3 and the sub-inner layer G7 each include 70 parts by mass of high-density polyethylene and 30 parts by mass of polyolefin thermoplastic resin; the adhesive layer D4 and the adhesive layer F6 each weigh 100 parts by mass of polyolefin adhesive resin; the core layer E5 each weighs 100 parts of vinyl alcohol-ethylene polymer resin; the inner layer I9 contains 85 parts by mass of easy-to-release resin and 15 parts by mass of low-density polyethylene, which are respectively put into nine extruders, and the resin is melted at high temperature in the extruder to form a fluid melt;
[0071] S2, the melt is filtered through a filter screen, and then passes through a die distributor and an annular die in sequence to form a bubble tube film, and is cooled and shaped under an internal air cooling device and an external air cooling device;
[0072] S3, the shaped film is stretched forward by a rotating device and a traction device, and then passes through a thickness measuring system, a deflection system, a corona treatment system, and a trimming device in sequence, and finally is rolled into a roll film by a winding device, so as to obtain a nine-layer co-extruded barrier film 5 that is self-sealing and easy to peel off.
[0073] Comparative Example 3
[0074] According to the formula composition of ordinary easy-to-peel PE film, 55 parts by mass of linear low-density polyethylene and 45 parts by mass of polyethylene are weighed for the outer layer; 50 parts by mass of polyethylene, 40 parts by mass of linear low-density polyethylene and 10 parts by mass of polyolefin thermoplastic resin are weighed for the middle layer, and 65 parts by mass of polyethylene, 20 parts by mass of linear low-density polyethylene and 10 parts by mass of polybutene are weighed for the inner layer, which are respectively put into the extruder, and then the three-layer co-extrusion blown film process is adopted to prepare the film to obtain ordinary easy-to-peel PE film 6.
[0075] The brand of metallocene polyethylene is 2010MA produced by Exxon; the brand of linear low-density polyethylene is 1002AY produced by Exxon; the brand of high-density polyethylene is FB5600 produced by Borouge Chemical Company; the brand of low-density polyethylene is 100AC produced by Exxon; the brand of polyolefin thermoplastic resin is PL1880G produced by Dow Chemical Company; the brand of polyolefin adhesive resin is PX3747 produced by Basel Company; the brand of vinyl alcohol-ethylene polymer resin is DC3203FB produced by Japan Gode Chemical Company; the brand of easy-release resin is Sealution 210 produced by Dow Chemical Company; the brand of polyethylene is 2420H produced by China National Petroleum Corporation, and the brand of polybutene is PB8640 produced by AndeBasel Company.
[0076] Comparative Example 4
[0077] S1. According to the formula composition, weigh the component resins in parts by weight respectively. The outer layer and the sub-outer layer both weigh 55 parts by weight of the first polyethylene (brand name 1002AY produced by Exxon) and 45 parts by weight of the second polyethylene (brand name 2420H produced by PetroChina); the middle layer weighs 100 parts by weight of EVOH (brand name F171B produced by Kuraray Co., Ltd. of Japan); the sub-inner layer weighs 40 parts by weight of the first polyethylene (brand name 1002AY produced by Exxon), 50 parts by weight of the second polyethylene (brand name 2420H produced by PetroChina) and 10 parts by weight of linear polyethylene (brand name PL1880 produced by Dow Chemical). G); the inner layer weighs 20 parts by weight of the first polyethylene (brand 1002AY produced by Exxon), 65 parts by weight of the second polyethylene (brand 2420H produced by PetroChina), and 15 parts by weight of polybutene (brand PB8640 produced by LyondellBasell); the adhesive layer weighs 100 parts by weight of low-density polyethylene (brand 41E762 produced by DuPont of the United States), and an adhesive layer is provided between the sub-outer layer and the middle layer and between the middle layer and the sub-inner layer, and the adhesive layer includes 100 parts by weight of low-density polyethylene (41E762 produced by DuPont of the United States), and then the resins of each layer are extruded at high temperature through 7 extruders to form a melt;
[0078] S2, the melt in step S1 passes through the filter screen and then forms a ring-shaped bubble tube film through the die distributor, and then is cooled and shaped in an air cooling device;
[0079] S3, the shaped film is sequentially passed through a traction device, a thickness measuring system, a corona treatment system, an edge trimming device and a winding device to obtain a co-extruded film 7.
[0080] Table 1 Components and ratios in co-extruded films
[0081]
[0082]
[0083] The films prepared in Example 2 and Comparative Examples 1-4 were tested for performance, and the results are shown in Table 2-3 below:
[0084] Heat seal strength test table 2
[0085]
[0086]
[0087] As shown in Table 2, the barrier easy-peel co-extruded film 2 prepared by Example 2 of Table 1 has a heat sealing strength MD value maintained between 2.58N / 15mm-3.55N / 15mm and a TD value maintained between 1.98N / 15mm-3.22N / 15mm at a heat sealing temperature of 125°C-160°C. The film has a low overall heat sealing strength and a wide heat sealing range while meeting the heat sealing strength requirements. The barrier easy-peel co-extruded films 4 / 5 prepared by Comparative Examples 1-2 have a heat sealing strength MD value between 125°C-160°C and a heat sealing strength of The heat sealing strength of the co-extruded film is maintained between 4.59N / 15mm-12.5N / 15mm, and the TD value is maintained between 3.44N / 15mm-8.02N / 15mm, both of which have high heat sealing strength. Due to the increase in the addition ratio of the easy-to-remove resin (Sealution210 produced by Dow Chemical Company) in Comparative Examples 1 and 2, when the heat sealing temperature gradually increases, the heat sealing strength of the co-extruded film is gradually enhanced. However, when the heat sealing strength of the co-extruded film is higher than 5N / 15mm, there are film stretching and extension phenomena at the peeling interface of the co-extruded film.
[0088] Barrier performance test table 3
[0089]
[0090] The data in Table 3 above illustrate that the oxygen barrier properties (0.97cc / (m2*24h), 0.95cc / (m2*24h), 0.98cc / (m2*24h)) and moisture barrier properties (2.56g / (m2*24h), 2.58g / (m2*24h), 2.55g / (m2*24h)) of the co-extruded films prepared in Example 2 and Comparative Examples 1-2 are similar, and better than the oxygen barrier properties and moisture barrier properties of Comparative Examples 3-4. The co-extruded films prepared in Example 2 and Comparative Examples 1-2 are prepared by a nine-layer co-extrusion blown film process, indicating that the barrier effect of the barrier easy-peel co-extruded films 2 / 4 / 5 is better than that of the ordinary easy-peel PE film, which is conducive to the preparation of easy-peel packaging materials with relatively high barrier requirements.
[0091] It can also be seen from Table 3 above that the heat sealing strengths of the co-extruded films prepared in Example 2 and Comparative Examples 1-2 are 3.55 N / 15 mm, 7.85 N / 15 mm and 12.5 N / 15 mm, respectively, while the raw material formulas of the barrier easy-peel co-extruded films 2 / 4 / 5 are basically the same, only the addition ratios of the easy-peel resin and the low-density polyethylene (brand 100AC produced by Exxon) of the inner layer are different during the preparation process. However, the heat sealing strength (easy-peel strength) performances of the prepared barrier easy-peel co-extruded films 2 / 4 / 5 are different, and with the increase in the addition ratio of the easy-peel resin, the heat sealing strength (easy-peel strength) also gradually increases. When the heat sealing strength of the co-extruded film is higher than 5 N / 15 mm, there are film stretching and extension phenomena at the peeling interface of the co-extruded film. Therefore, the inner layer formula of Example 2 is better than the inner layer formula of Comparative Examples 1-2.
[0092] Comparative Example 4 uses barrier EVOH resin (ethylene molar content of 32) produced by Kuraray, which has a barrier performance similar to that of the vinyl alcohol-ethylene polymer resin (brand name DC3203FB produced by Japan Kosei Chemical) of the film of the present invention, so there is no significant difference in barrier performance. However, the heat seal layer of Comparative Example 4 uses polybutene PB8640 produced by Basel Company, which has an easy-to-open function, but the unsealing state is far less smooth than the co-extruded film of the present invention. The self-sealing unsealing of Comparative Example 4 is an interface (surface) pop-up phenomenon, while the unsealing of the present invention is an embedded unsealing. Therefore, the co-extruded film of the present invention has better sealing performance than Comparative Example 4.
[0093] Finally, it should be noted that although embodiments of the present invention have been shown and described above, it will be understood by those skilled in the art that various changes, modifications, substitutions and variations may be made to these embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A nine-layer co-extruded barrier film with self-sealing and easy-to-open properties, characterized in that: The film consists of an outer layer A (1), a sub-outer layer B (2), and a sub-outer layer C (3) , an adhesive layer D (4), a core layer E (5), an adhesive layer F (6), a sub-inner layer G (7), a sub-inner layer H (8) and an inner layer I (9), wherein the outer layer A (1) comprises 45-55 parts by weight of metallocene polyethylene and 45-55 parts by weight of linear low-density polyethylene; the sub-outer layer B (2) and the sub-inner layer H (8) each comprise 45-55 parts by weight of high-density polyethylene and 45-55 parts by weight of low-density polyethylene; the sub-outer layer C (3) and the sub-inner layer G (7) each comprise 70-80 parts by weight of high-density polyethylene and 20-30 parts by weight of polyolefin thermoplastic resin; the adhesive layer D (4) and the adhesive layer F (6) each comprise 100 parts by weight of polyolefin adhesive resin; the core layer E (5) comprises 100 parts of vinyl alcohol-ethylene polymer resin; the inner layer I (9) comprises 10-20 parts by weight of easy-to-release resin and 80-90 parts by weight of low-density polyethylene; The brand of the metallocene polyethylene is 2010MA produced by Exxon; the brand of the linear low-density polyethylene is 1002AY produced by Exxon; the brand of the high-density polyethylene is FB5600 produced by Borouge Chemical Company; the brand of the low-density polyethylene is 100AC produced by Exxon; the brand of the polyolefin thermoplastic resin is PL1880G produced by Dow Chemical Company; the brand of the polyolefin adhesive resin is PX3747 produced by Basel Company; the brand of the vinyl alcohol-ethylene polymer resin is DC3203FB produced by Japan Gode Chemical Company; the brand of the easy-release resin is Sealution 210 produced by Dow Chemical Company; The thickness ratio of the outer layer A (1), the sub-outer layer B (2), the sub-outer layer C (3), the adhesive layer D (4), the core layer E (5), the adhesive layer F (6), the sub-inner layer G (7), the sub-inner layer H (8) and the inner layer I (9) is 2:1:2:2:3:2:2:1:2; The thickness of the adhesive layer D (4) and the adhesive layer F (6) are both 4 um; the thickness of the core layer E (5) is 6 um.
2. The nine-layer co-extruded barrier film with self-sealing and easy-to-open properties according to claim 1, characterized in that: The outer layer A (1) comprises 55 parts by mass of metallocene polyethylene and 45 parts by mass of linear low-density polyethylene; the sub-outer layer B (2) and the sub-inner layer H (8) each comprise 55 parts by mass of high-density polyethylene and 45 parts by mass of low-density polyethylene; the sub-outer layer C (3) and the sub-inner layer G (7) each comprise 70 parts by mass of high-density polyethylene and 30 parts by mass of polyolefin thermoplastic resin; the inner layer I (9) comprises 15 parts by mass of easy-release resin and 85 parts by mass of low-density polyethylene.
3. A process for preparing a nine-layer co-extruded barrier film having self-sealing and easy-to-open properties as claimed in any one of claims 1 to 2, characterized in that: The steps include: S1. According to the formula composition of each layer in the film, weigh the components of each mass and put them into nine extruders respectively. The resin is melted at high temperature in the extruder to form a fluid melt; S2, the melt is filtered through a filter screen, and then passes through a die distributor and an annular die in sequence to form a bubble tube film, and is cooled and shaped under an internal air cooling device and an external air cooling device; S3. The shaped film is stretched forward by a rotating device and a traction device, and then passes through a thickness measuring system, a deflection system, a corona treatment system, and a trimming device in sequence, and finally is rolled into a roll film by a winding device, thereby obtaining a nine-layer co-extruded barrier film that is self-sealing and easy to peel off.
4. The process for preparing a nine-layer co-extruded barrier film having self-sealing and easy-to-open properties according to claim 3, characterized in that: The processing temperatures of the nine extruders in step S1 are as follows: The extrusion temperatures of the extruder of the outer layer A (1) are 50°C, 185°C, 190°C, 195°C, 200°C, 200, and 200°C respectively; The extrusion temperatures of the extruder of the secondary outer layer B (2) are 60°C, 190°C, 195°C, 200°C, 205°C, 205°C, and 205°C respectively; The extrusion temperatures of the extruder of the secondary outer layer C (3) are 60°C, 190°C, 195°C, 200°C, 205°C, 205°C, and 205°C respectively; The extrusion temperatures of the adhesive layer D (4) extruder are 80°C, 210°C, 215°C, 220°C, 220°C, 220°C, and 220°C respectively; The extrusion temperatures of the extruder of the core layer E (5) are 100°C, 215°C, 220°C, 220°C, 220°C, 220°C, and 220°C respectively; The extrusion temperatures of the adhesive layer F (6) extruder are: 80°C, 210°C, 215°C, 220°C, 220°C, 220°C, 220°C; The extrusion temperatures of the extruder of the secondary inner layer G (7) are 60°C, 190°C, 195°C, 200°C, 205°C, 205°C, and 205°C respectively; The extrusion temperatures of the extruder of the secondary inner layer H (8) are 60°C, 190°C, 195°C, 200°C, 205°C, 205°C, and 205°C respectively; The extrusion temperatures of the inner layer I (9) extruder are 50°C, 185°C, 190°C, 195°C, 200°C, 200°C, and 200°C respectively; The temperatures in the die zone are: 220℃, 220℃, 220℃, 220℃, 220℃, 220℃, 220℃, 220℃, 220℃, 220℃, 220℃, 220℃ respectively.
5. The process for preparing a nine-layer co-extruded barrier film having self-sealing and easy-to-open properties according to claim 4, characterized in that: The screw diameters of the nine extruders are 70mm, 60mm, 60mm, 50mm, 50mm, 50mm, 60mm, 60mm and 70mm respectively; the die head diameter of the extruder is 500mm; and the extrusion capacity of the extruder is 580±20kg / h.
6. The process for preparing a nine-layer co-extruded barrier film having self-sealing and easy-to-open properties according to claim 3, characterized in that: The filter screen is 70 mesh / 90 mesh / 100 mesh / 90 mesh.
7. The process for preparing a nine-layer co-extruded barrier film having self-sealing and easy-to-open properties according to claim 3, characterized in that: The traction speed of the traction device is 55±5m / min; the traction tension is 90±10N; the contact roller tension of the winding device is 30±10N; and the winding tension is 40±10N.
Citation Information
Patent Citations
Easy-tearing packaging film and production process thereof
CN105667035A
Easy-cutting nylon EVOH high-barrier film and production method thereof
CN107745561A
Easy-to-tear stretchable multi-layer co-extrusion casting film and production method thereof
CN108016013A
High-temperature-steaming-resistant high-barrier base film, easy-to-tear film comprising same and preparation method of high-temperature-steaming-resistant high-barrier base film
CN108068423A
High-transparent high-barrier and easy-taking opening sealing cover membrane and production technology thereof
CN109263211A