A method for preparing titanium anode plate by sol method
The preparation of titanium anode plates through the sol method solves the problems of uneven oxide distribution and metal loss in traditional processes, and achieves efficient preparation of titanium anode plates, extends its service life and improves catalytic activity.
Patent Information
- Application Number
- CN202211516082.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-29
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-11-29
AI Technical Summary
In the production process of traditional titanium anode plates, there are problems of uneven oxide distribution, large metal loss and cracks on the sintered surface, which affects its service life and catalytic activity.
The titanium anode plate was prepared by sol method, and the iridium trichloride was dissolved by water regia, the addition of tantalum pentachloride and dibutyltin dilaurate was formed to form a nano-scale MMO anode coating, combined with the gradient heating sintering process to ensure that Metal oxides are uniformly distributed and densely coated.
The metal oxide distribution is achieved evenly, the metal addition amount is basically not lost, and the coating is free of cracks, which significantly extends the service life and catalytic activity of the anode.
Smart Images

Figure CN115852349B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of anode plates, and in particular to a method for preparing a titanium anode plate by a sol method. Background Art
[0002] Metal oxide coating anodes are mainly used in the two major industries of hydrometallurgy and electrochemistry, and their application areas include sewage treatment, chemical industry, metallurgy, electroplating, organic synthesis, etc. The traditional manufacturing process of titanium anodes is to mix metal compounds with organic solvents such as n-butanol and isopropanol, and then sinter and thermally decompose them at 400-600℃. The traditional thermal separation method has problems such as uneven oxide distribution and considerable metal loss such as Sn and Pt, which can even reach 30% to 60%. In addition, the sintering process will cause cracks in the surface coating, which seriously affects the service life and catalytic activity of the anode.
[0003] Therefore, it is necessary to provide a new process to solve the above technical problems. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a method for preparing titanium anode plates by a sol method, in which the coating oxide is evenly distributed, the metal addition amount is basically not lost, the surface coating obtained by sintering has no cracks, the coating is dense, and the service life and catalytic activity of the anode can be greatly extended.
[0005] In order to solve the above problems, the technical solution of the present invention is as follows:
[0006] A method for preparing a titanium anode plate by a sol method comprises the following steps:
[0007] Step S1, pretreatment of titanium substrate;
[0008] Step S2, preparing aqua regia, adding iridium trichloride to an appropriate amount of aqua regia, heating and boiling until the iridium trichloride is completely dissolved; starting distillation, stopping distillation when no yellow gas is generated and no water is present, adding an organic alcohol solvent to obtain solution A, wherein the amount of iridium trichloride added is 8-12 g / m 2 count;
[0009] Among them, the amount of iridium trichloride added can be 8g iridium / m 2 , 10g iridium / m 2 or 12g iridium / m 2 , or other values within this range;
[0010] Step S3, adding tantalum pentachloride powder to an organic alcohol solvent, dissolving and filtering, the filtrate is solution B, wherein the amount of tantalum pentachloride added is 6-8 g / m 2 count;
[0011] Among them, the amount of tantalum pentachloride added can be 6g tantalum / m2 , 7g tantalum / m 2 or 8g tantalum / m 2 , or other values within this range.
[0012] Step S4, taking dibutyltin dilaurate, adding an organic alcohol solvent, and ultrasonically shaking to obtain a solution C, wherein the amount of dibutyltin dilaurate added is 16-20 g / m 2 count;
[0013] Among them, the amount of dibutyltin dilaurate can be 16g tin / m 2 , 18g tin / m 2 or 20g tin / m 2 , or other values within this range.
[0014] Step S5, adding citric acid to the ethylene glycol solution, and mixing them uniformly by ultrasonic vibration to obtain a nanosol solvent;
[0015] Step S6, heating the nanosol solvent to 50-65° C., adding the mixture of solution A, solution B and solution C to the nanosol solvent under continuous stirring, adding anhydrous ethanol after mutual dissolution, and adjusting the mass concentration of the solution to 5-8%, to obtain a nanosol coating solution;
[0016] The heating temperature can be 50°C, 55°C, 60°C or 65°C, or other temperature values within this range; the solution concentration is adjusted to 5%, 6%, 7% or 8%, or other values between 5-8%.
[0017] Step S7, the nano-sol coating is evenly coated on the surface of the titanium substrate in step S1, and after multiple drying and sintering processes, an MMO anode nano-coating is formed on the surface of the titanium substrate; the oxide components and their molar ratios in the MMO anode nano-coating are IrO 2 :Ta 2 O 5 :SnO 2 =1:0.75-0.85:2.8-3.2.
[0018] In the present invention, the MMO anode nano-coating IrO 2 :Ta 2 O 5 :SnO 2The molar ratio can be 1:0.75:2.8, 1:0.75:3.0, 1:0.75:3.2, 1:0.81:2.8, 1:0.81:3.0, 1:0.81:3.2, 1:0.85:2.8, 1:0.85:3.02 or 1:0.85:3.2, and can be other values within this range. The amount of metal elements Ir, Ta, and Sn is calculated based on the area of the titanium anode substrate. For example, the amount of metal element Ir can be 8-12 g / m 2 Calculation, correspondingly, the amount of metal elements Ta and Sn added is calculated based on the ratio of each component in the metal oxide.
[0019] Furthermore, in step S1, the titanium substrate pretreatment includes the following steps:
[0020] Step S11, sandblasting the titanium substrate to roughen its surface;
[0021] Specifically, 24# brown corundum is used for sandblasting;
[0022] Step S12, placing in a mixed solution of oxalic acid and hydrochloric acid for acid etching, wherein the oxalic acid concentration in the mixed solution is 8-10wt%, and the hydrochloric acid concentration is 3-8wt%;
[0023] The oxalic acid concentration may be 8wt%, 9wt% or 10wt%, or other values; the hydrochloric acid concentration may be 3%, 5%, 6% or 8%, or other values; the acid etching temperature may be 80-90°C, such as 80°C, 85°C or 90°C, or other temperature values within the range; the acid etching time may be 6-8h, such as 6h, 7h or 8h, or other values within the range;
[0024] Step S13, rinsing with clean water and drying after acid etching;
[0025] Step S14, sintering at 650-700°C for 3-4 hours to form an oxygen-deficient titanium oxide film (Ti 4 O 7 ), and cooled with the furnace for standby use; wherein, the sintering temperature can be 650°C, 680°C or 700°C, or other temperature values within this range; the sintering time can be 3h, 3.5h or 4h, or other time values within this range.
[0026] Furthermore, in step S7, the drying and sintering process includes the following steps:
[0027] Step S71, evenly apply the prepared solution on the surface of the titanium substrate, set the drying furnace to 100-130°C, dry for 5-10 minutes, then set the oxidation furnace to 340-360°C for 15-30 minutes, and repeat this operation twice;
[0028] Among them, the drying temperature can be 100°C, 110°C, 120°C or 130°C, or other values within this range; the drying time can be 5min, 8min or 10min, or other values within this range; the sintering temperature can be 340°C, 350°C or 360°C, or other values within this range; the sintering time can be 15min, 20min, 25min or 30min, or other values within this range.
[0029] Step S72, continue coating, set the drying furnace temperature to 100-130°C, dry for 5-10 minutes, set the oxidation furnace to 380-420°C for 15-30 minutes, and repeat this operation twice;
[0030] The drying temperature can be 100°C, 110°C, 120°C or 130°C, or other values within this range; the drying time can be 5 min, 8 min or 10 min, or other values within this range; the sintering temperature can be 380°C, 400°C or 420°C, or other values within this range; the sintering time can be 15 min, 20 min, 25 min or 30 min, or other values within this range.
[0031] Step S73, continue coating, set the drying furnace temperature to 100-130°C, dry for 5-10 minutes, set the oxidation furnace to 440-460°C for 15-30 minutes, until the coating liquid is completely applied, and sinter for the last oxidation for 55-70 minutes, and then cool down and take out of the furnace;
[0032] Among them, the drying temperature can be 100°C, 110°C, 120°C or 130°C, or other values within the range; the drying time can be 5min, 8min or 10min, or other values within the range; the sintering temperature can be 440°C, 450°C or 460°C, or other values within the range; the sintering time can be 15min, 20min, 25min or 30min, or other values within the range; and the last sintering time can be 55min, 60min, 65min or 70min, or other values within the range.
[0033] In the present invention, the organic alcohol is one of n-butanol and isopropanol.
[0034] Compared with the prior art, the method for preparing titanium anode plates by the sol method provided by the present invention has the following beneficial effects:
[0035] 1. The method for preparing titanium anode plates by a sol method provided by the present invention adopts a sol method to prepare a coating, citric acid forms a complex with metal ions, and then reacts with an organic alcohol to form a polymer, so that the metal ions are highly evenly dispersed in the polymer, and then a coating is formed by sintering. The metal oxides in the coating are evenly distributed and nanometer-scale, and the amount of metal added is basically not lost. The coating has few cracks and strong bonding force, which can improve the service life and catalytic activity of the anode.
[0036] Second, the method for preparing a titanium anode plate by a sol method provided by the present invention, the surface of the titanium substrate is roughened and the surface impurity elements are removed, and the treated titanium substrate is then sintered at a high temperature to form an oxygen-deficient titanium oxide film (Ti 4 O 7 ), the main active ingredient contains Ti 4 O 7 It has the characteristics of good conductivity and corrosion resistance; and it can prevent active oxygen from penetrating into the titanium substrate through the coating cracks during the electrolysis process, resulting in the formation of non-conductive titanium dioxide film, which affects the life of the anode.
[0037] 3. The method for preparing titanium anode plate by sol method provided by the present invention, iridium element uses iridium trichloride as raw material and is dissolved in aqua regia, the purpose is to ensure that the solution system Ir 4+ The stability of the valence state; the tin element uses dibutyltin dilaurate as the raw material, which is an organic solvent and can reduce the loss rate of the tin element in the subsequent high-temperature sintering process. The tin dioxide formed after sintering has good electrocatalytic activity and coating density, thereby improving the electrochemical performance and life of the anode.
[0038] 4. The method for preparing titanium anode plates by the sol-gel method provided by the present invention adopts a gradient temperature rise sintering process, the purpose of which is to reduce the internal stress of the coating, further reduce cracks on the coating surface, improve the density of the anode coating and extend the life of the anode. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0040] Figure 1 This is the XRD diagram of the titanium substrate after sintering of the present invention;
[0041] Figure 2 This is the SEM morphology of the coating prepared in Comparative Example 1;
[0042] Figure 3 This is a SEM morphology image of the coating prepared in Example 1 of the present invention;
[0043] Figure 4 This is a comparison chart of the LSV of the anode plates prepared in Example 1 and Comparative Example 1.
[0044] Figure 5 This is a CV comparison chart of the anode plates prepared in Example 1 and Comparative Example 1. DETAILED DESCRIPTION
[0045] In order to enable those skilled in the art to better understand the technical solutions in the embodiments of the present invention and to make the above-mentioned objects, features and advantages of the present invention more obvious and understandable, the specific implementation modes of the present invention are further described below in conjunction with the accompanying drawings.
[0046] It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention. In addition, the technical features involved in each embodiment of the present invention described below can be combined with each other as long as there is no conflict between them.
[0047] Comparative Example 1
[0048] A method for preparing a titanium anode plate (coating is IrO2-Ta 2 O 5 -SnO 2 ), comprising the following steps:
[0049] Step S1, pretreatment of titanium substrate;
[0050] The specific process is: use 24# brown corundum for sandblasting, then use 8%-10% oxalic acid + 5% hydrochloric acid for acid etching, acid etching temperature: 85℃, process for 6 hours, and dry for use.
[0051] Step S2, preparing aqua regia, adding iridium trichloride to an appropriate amount of aqua regia, heating and boiling until the iridium trichloride is completely dissolved; starting distillation, and stopping distillation when no yellow gas is generated and no water is present, and adding an organic alcohol solvent to obtain solution A;
[0052] Among them, aqua regia is made by mixing AR grade concentrated hydrochloric acid and AR grade concentrated nitric acid in a ratio of 3:1. The specific process is: first pour the hydrochloric acid into a glass cup, then pour the nitric acid into the hydrochloric acid, and stir continuously with a glass rod. The best effect is to use it within half an hour after preparation, and the oxidation ability is the strongest;
[0053] Solution A preparation process is: take out 50ml of the prepared aqua regia and pour it into a glass bottle, then add 18.5g / m 2 (Iridium 10g / m 2) Pour iridium trichloride slowly in batches while stirring continuously, then heat and boil until completely dissolved; then start distillation until it becomes viscous and stop distillation when yellow gas begins to appear; then add n-butanol to 60 ml to prepare solution A.
[0054] Step S3, adding tantalum pentachloride powder to an organic alcohol solvent, dissolving and filtering, and the filtrate is solution B;
[0055] Specifically, take 15g / m 2 (Tantalum 7.57g / m 2 ) Put tantalum pentachloride powder into a glass bottle, add 75 ml of n-butanol, stir and filter (you can use a suction filter bottle). If the solution is less than 75 ml after filtering, add n-butanol to make up to 75 ml.
[0056] Step S4, taking dibutyltin dilaurate, adding an organic alcohol solvent, and ultrasonically shaking to obtain a solution C;
[0057] Specifically, take 98 ml / m of dibutyltin dilaurate 2 (Sn 18.7g / m 2 ), add 120ml / m of anhydrous ethanol 2 , ultrasonic vibration for 15 minutes.
[0058] Step S5, solution A, solution B and solution C are mixed, and then 180 ml / m of n-butanol is added. 2 , isopropyl alcohol 150ml / m 2 , shake well for later use;
[0059] Step S6, uniformly coating the prepared coating liquid on the surface of the titanium substrate in step S1, and forming a conventional MMO anode coating on the surface of the titanium substrate through multiple drying and sintering processes;
[0060] Specifically, the prepared solution is evenly coated on the surface of the titanium substrate, the drying furnace is set to 120°C, and the drying is performed for 5-10 minutes, and then the oxidation furnace is set to 350°C and kept warm for 20 minutes, and this operation is repeated twice;
[0061] Continue coating, set the drying oven temperature to 120℃, dry for 5-10 minutes, set the oxidation oven to 400℃ and keep warm for 20 minutes, repeat this operation twice;
[0062] Continue coating, set the drying furnace temperature to 120℃, dry for 5-10 minutes, set the oxidation furnace to 450℃ and keep warm for 20 minutes, until all the coating liquid is applied, and sinter for the last oxidation for 60 minutes, then cool down and take out of the furnace.
[0063] Example 1
[0064] A method for preparing a titanium anode plate (coating is IrO2-Ta2 O 5 -SnO 2 ), comprising the following steps:
[0065] Step S1, pretreatment of titanium substrate;
[0066] The specific process is: use 24# brown corundum for sandblasting, then use 8%-10% oxalic acid + 5% hydrochloric acid for acid etching, acid etching temperature: 85℃, process for 6 hours, and dry for use.
[0067] The treated substrate was sintered at 680℃ for 4h to form an oxygen-deficient titanium oxide film (Ti 4 O 7 ), and then cool in the furnace for later use.
[0068] See also Figure 1 , is the XRD diagram of the titanium substrate after sintering of the present invention. Figure 1 It can be seen that after high temperature sintering, the phases of the sample are mainly TiO 2-x 、Ti 4 O 7 and Ta 2 O 5 , the main active ingredient Ti 4 O 7 It has the characteristics of good conductivity and corrosion resistance; and can prevent active oxygen from penetrating into the titanium substrate through the coating cracks during the electrolysis process, resulting in the formation of non-conductive titanium dioxide film, which affects the life of the anode.
[0069] Step S2, preparing aqua regia, adding iridium trichloride to an appropriate amount of aqua regia, heating and boiling until the iridium trichloride is completely dissolved; starting distillation, and stopping distillation when no yellow gas is generated and no water is present, and adding an organic alcohol solvent to obtain solution A;
[0070] Among them, aqua regia is made by mixing AR grade concentrated hydrochloric acid and AR grade concentrated nitric acid in a ratio of 3:1. The specific process is: first pour the hydrochloric acid into a glass cup, then pour the nitric acid into the hydrochloric acid, and stir continuously with a glass rod. The best effect is to use it within half an hour after preparation, and the oxidation ability is the strongest;
[0071] Solution A preparation process is: take out 50ml of the prepared aqua regia and pour it into a glass bottle, then add 18.5g / m 2 (Iridium 10g / m 2 ) Pour iridium trichloride slowly in batches while stirring continuously, then heat and boil until completely dissolved; then start distillation until it becomes viscous and stop distillation when yellow gas begins to appear; then add n-butanol to 60 ml to prepare solution A.
[0072] Step S3, adding tantalum pentachloride powder to an organic alcohol solvent, dissolving and filtering, and the filtrate is solution B;
[0073] Specifically, take 15g / m 2 (Tantalum 7.57g / m 2 ) Put tantalum pentachloride powder into a glass bottle, add 75 ml of n-butanol, stir and filter (you can use a suction filter bottle). If the solution is less than 75 ml after filtering, add n-butanol to make up to 75 ml.
[0074] Step S4, taking dibutyltin dilaurate, adding an organic alcohol solvent, and ultrasonically shaking to obtain a solution C;
[0075] Specifically, take 98 ml / m of dibutyltin dilaurate 2 (Sn 18.7g / m 2 ), add 120ml / m of anhydrous ethanol 2 , ultrasonic vibration for 15 minutes.
[0076] Step S5, adding citric acid to the ethylene glycol solution, and mixing them uniformly by ultrasonic vibration to obtain a nanosol solvent;
[0077] Specifically, 63.5g / m 2 Add 143ml / m of citric acid 2 Ethylene glycol, to obtain the nanosol solvent;
[0078] Step S6, heating the nanosol solvent to 60° C., adding a mixture of solution A, solution B and solution C to the nanosol solvent under continuous stirring, and adding anhydrous ethanol after mutual dissolution to obtain a nanosol coating solution;
[0079] Specifically, continue stirring for 2-3 hours until all the mixture is dissolved, then add 343 ml / m of anhydrous ethanol. 2 .
[0080] Step S7, uniformly coating the prepared coating liquid on the surface of the titanium substrate in step S1, and forming a MMO anode nano coating on the surface of the titanium substrate through multiple drying and sintering processes;
[0081] Specifically, the prepared solution is evenly coated on the surface of the titanium substrate, the drying furnace is set to 120°C, and the drying is performed for 5-10 minutes, and then the oxidation furnace is set to 350°C and kept warm for 20 minutes, and this operation is repeated twice;
[0082] Continue coating, set the drying oven temperature to 120℃, dry for 5-10 minutes, set the oxidation oven to 400℃ and keep warm for 20 minutes, repeat this operation twice;
[0083] Continue coating, set the drying furnace temperature to 120℃, dry for 5-10 minutes, set the oxidation furnace to 450℃ and keep warm for 20 minutes, until all the coating liquid is applied, and sinter for the last oxidation for 60 minutes, then cool down and take out of the furnace.
[0084] In this embodiment, the molar ratio of the metal oxides in the coating is IrO2:Ta 2 O 5 :SnO 2 =1:0.81:3.02.
[0085] The spectral detection values of each element of the oxidation coating formed in Comparative Example 1 and Example 1 are as follows:
[0086]
[0087]
[0088] It can be seen from the above results that the preparation method of the present invention significantly reduces the metal loss rate, especially the metal tin loss rate.
[0089] Please refer to Figure 2 and Figure 3 ,in Figure 2 This is the SEM morphology of the coating prepared in Comparative Example 1; Figure 3 This is a SEM morphology of the coating prepared in Example 1 of the present invention. Figure 2 and Figure 3 It can be seen that the titanium anode plate prepared in Example 1 has a nano-scale MMO coating with few cracks and strong bonding strength.
[0090] The anode plates of Comparative Example 1 and Example 1 were subjected to life test analysis, and the test methods and data are as follows:
[0091] 1. Experimental instruments and materials:
[0092] High-frequency voltage and current device, multimeter, wires and connectors, tap water, sulfuric acid, beaker, glass rod, and titanium anode plate.
[0093] 2. Experimental steps
[0094] 2.1 Prepare 1 mol / L sulfuric acid solution, stir thoroughly and set aside at 40-50℃;
[0095] 2.2 Pour the sulfuric acid solution into 1L beakers, with a volume of 1L;
[0096] 2.3 Cut the test piece polished on sandpaper into samples no larger than 1cm*1cm and fix them on the positive electrode of the titanium anode material.
[0097] 2.4 Use wires to connect the current voltage device and the titanium anode material (in series) with sulfuric acid solution as the electrolyte;
[0098] 2.5 Start the power supply and set the corresponding current density: 40000A / m2
[0099] 2.6 Record the initial voltage (usually 4 hours after the start of electrolysis), and then measure the voltage of each titanium anode at regular intervals every day and record it.
[0100] 2.7 When the voltage reaches 1.5 times of the initial stable voltage, it is the failure time of the standard test piece and the enhanced life test is completed.
[0101] 3. Data results:
[0102]
[0103] It can be seen from the above data that when the two groups of samples were tested in the same environment, the titanium anode plate prepared by the sol method of the present invention had the longest life, which was nearly twice that of the anode plate of the control example, reflecting excellent electrochemical performance.
[0104] See also Figure 4 , which is a LSV comparison diagram of the anode plates prepared in Example 1 and Comparative Example 1, wherein Ir-Ta-Sn-1 represents the conventional coating of Comparative Example 1, and Ir-Ta-Sn-2 represents the nanoscale coating of Example 1. Figure 4 It can be seen that with the same coating formula, the electrode potential of the sol nano coating is significantly lower than that of the conventional coating, and it saves energy during use and has high electrocatalytic activity.
[0105] See also Figure 5 , which is a CV comparison diagram of the anode plates prepared in Example 1 and Comparative Example 1. Wherein (a) represents the CV curve of the anode plate of Comparative Example 1, and (b) represents the CV curve of the anode plate of Example 1. The principle of the cyclic voltammetry CV polarization curve is that the larger the area enclosed by the curve area, the more active sites there are. By comparison, it can be seen that the anode plate coating of Example 1 of the present invention has more active sites, indicating that the anode plate of Example 1 has higher electrocatalytic activity.
[0106] The voltammetric area enclosed by the cyclic voltammetric curve is proportional to the surface charge capacity of the titanium anode coating. The larger the area enclosed by the cyclic voltammetric curve, the greater the voltammetric charge on the surface of the oxide anode, the more active points on the surface, the larger the electrochemical effective surface area, and the more stable the electrocatalytic activity of the electrode.
[0107] The embodiments of the present invention are described in detail above with reference to the accompanying drawings, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations made to these embodiments without departing from the principles and spirit of the present invention are still within the scope of protection of the present invention.
Claims
1. A method for preparing a titanium anode plate by a sol method, It is characterized in that The steps include: Step S1, titanium substrate pretreatment: The titanium substrate is subjected to sandblasting to roughen its surface; Put it into a mixed solution of oxalic acid and hydrochloric acid for acid etching, wherein the concentration of oxalic acid in the mixed solution is 8-10wt%, and the concentration of hydrochloric acid is 3-8wt%; After acid etching, rinse with clean water and dry; Sinter at 650-700℃ for 3-4h, and cool in the furnace for later use; Step S2, preparing aqua regia, adding iridium trichloride to an appropriate amount of aqua regia, heating and boiling until the iridium trichloride is completely dissolved; starting distillation, stopping distillation when no yellow gas is generated and no water is present, adding an organic alcohol solvent to obtain solution A, wherein the amount of iridium trichloride added is 8-12 g / m 2 count; Step S3, adding tantalum pentachloride powder to an organic alcohol solvent, dissolving and filtering, the filtrate is solution B, wherein the amount of tantalum pentachloride added is 6-8 g / m 2 count; Step S4, taking dibutyltin dilaurate, adding an organic alcohol solvent, and ultrasonically shaking to obtain a solution C, wherein the amount of dibutyltin dilaurate added is 16-20 g / m 2 count; Step S5, adding citric acid to the ethylene glycol solution, and mixing them uniformly by ultrasonic vibration to obtain a nanosol solvent; Step S6, heating the nanosol solvent to 50-65° C., adding the mixture of solution A, solution B and solution C to the nanosol solvent under continuous stirring, adding anhydrous ethanol after mutual dissolution, and adjusting the mass concentration of the solution to 5-8%, thereby obtaining a nanosol coating solution; Step S7, uniformly coating the nano-sol coating on the surface of the titanium substrate in step S1, and forming a MMO anode nano-coating on the surface of the titanium substrate through multiple drying and sintering processes; the drying and sintering process includes the following steps: The prepared solution is evenly coated on the surface of the titanium substrate, the drying furnace is set to 100-130°C, and the drying is performed for 5-10 minutes. Then the oxidation furnace is set to 340-360°C and kept warm for 15-30 minutes. This operation is repeated twice. Continue coating, set the drying furnace temperature to 100-130℃, dry for 5-10 minutes, set the oxidation furnace to 380-420℃ and keep warm for 15-30 minutes, repeat this operation twice; Continue coating, set the drying furnace temperature to 100-130℃, dry for 5-10 minutes, set the oxidation furnace to 440-460℃ and keep warm for 15-30 minutes, until all the coating liquid is applied, the last oxidation sintering for 55-70 minutes, and then cool down and take out of the furnace; The oxide components and their molar ratios in the MMO anode nanocoating are IrO 2 :Ta 2 O 5 :SnO 2 =1:0.75-0.85:2.8-3.
2.
2. The method for preparing a titanium anode plate by a sol method according to claim 1, It is characterized in that The acid etching temperature is 80-90°C, and the acid etching time is 6-8h.
Citation Information
Patent Citations
Ti / SnO2 electrode as well as preparation method and application
CN104528890A
Preparation method of coating anode plate
CN109706513A
Titanium-based titanium oxide bipolar plate and preparation method thereof
CN110071302A
Coating electrode containing titanium black intermediate layer, preparation method and applications thereof, and electrochemical water treatment equipment
CN111003759A
Preparation method of titanium anode with titanium-based coating
CN112795908A