A processing technology for extruded anchor

By using environmentally friendly saponification treatment liquids, including soap, aloe vera extract, sodium dodecyl benzene sulfonate, modified diatomaceous earth and sodium carboxymethyl cellulose, the problem of wastewater pollution in the extrusion anchor saponification treatment is solved and achieved It provides environmentally friendly, zero-emission and efficient anchorage treatment and improves the corrosion resistance and lubrication performance of the anchorage.

CN115852354BActive Publication Date: 2024-10-29BEIJING SANQIANG REBAR PRESTRESSING EQUIP CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202211501838.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-28
Publication Date
2024-10-29
Estimated Expiration
2042-11-28

AI Technical Summary

Technical Problem

The use of acid and alkali chemical reagents in the saponification treatment process of existing extrusion anchors results in the generation of wastewater and environmental pollution, and lacks an environmentally friendly treatment process.

Method used

Using an environmentally friendly saponification treatment solution including soap, aloe vera extract, sodium dodecylbenzene sulfonate, modified diatomaceous earth and sodium carboxymethylcellulose, zero emissions and environmental protection are achieved through impurity removal, phosphating and saponification steps Energy-saving treatment process.

Benefits of technology

This process improves the corrosion resistance and lubrication performance of the anchor, reduces environmental pollution, and achieves environmentally friendly and efficient anchor processing by generating a protective boundary lubricating film and a zinc phosphate layer.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present application discloses a processing process for an extruded anchor. The process comprises the following steps: impurity removal: the anchor is first placed in a de-impurity solution for rinsing, and then soaked in ethanol to remove impurities on the surface to obtain a rinsed anchor; phosphating: the rinsed anchor is placed in a zinc phosphating solution for soaking at a soaking temperature of 80-95°C, and then placed in clean water for cleaning, the zinc phosphating solution remaining on the surface of the anchor is cleaned, and the phosphated anchor is obtained; saponification: the phosphated anchor is placed in a saponification treatment solution for soaking at a soaking temperature of 60-75°C, and the soaking is repeated 3-5 times to obtain a saponified anchor; the saponification treatment solution comprises the following components: soap, aloe extract, sodium dodecylbenzene sulfonate, modified diatomaceous earth, sodium carboxymethyl cellulose and water. The components of the saponification treatment solution of the present application are all environmentally friendly and pollution-free substances. During the saponification treatment process, the effects of zero emission, no pollution to the surrounding environment, and environmental protection and energy saving are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of anchor production, and more specifically, it relates to a processing technology for extruded anchors. Background Art

[0002] The extrusion anchor is composed of an extrusion anchor ring and a matching extrusion spring inserted in the cavity of the extrusion anchor ring. Extrusion anchors are widely used in highway bridges, railway bridges, high-rise buildings, steel bar engineering, bridge and building reinforcement projects, etc. Extrusion anchors have a good stress concentration effect. In concrete structures, they can transfer tension to the inside and play an anchoring role.

[0003] The processing technology of squeezed anchor in the prior art usually includes the following steps: firstly, the anchor is degreased and degreased, then acid-washed and rust-removed, then washed again, then phosphated and saponified, and finally washed and dried to obtain a squeezed anchor with a clean surface. In the saponification process of the squeezed anchor, a large amount of acid and alkali chemical reagents are used, a large amount of wastewater is generated, and the reagents after processing and soaking can basically not be recycled, which leads to the problem of wastewater treatment for the production enterprise. If it is not properly treated, it may even cause great damage to the surrounding ecological environment.

[0004] Therefore, it is necessary to provide an environmentally friendly processing process for extruded anchors. Summary of the invention

[0005] In order to solve the problem that acid and alkali chemical reagents are used in the saponification process of the extruded anchor, which easily generates wastewater treatment and environmental pollution, the present application provides a treatment process for the extruded anchor.

[0006] The present application provides a processing technology for an extruded anchor, which adopts the following technical solution:

[0007] A processing process for an extruded anchor comprises the following steps:

[0008] S1. De-impurity: The anchor is first placed in a de-impurity liquid for rinsing, and then soaked in ethanol for 1-2 hours to remove impurities on the surface to obtain a rinsed anchor;

[0009] S2. Phosphating: Soak the rinsed anchor in a zinc phosphating solution for 10-15 minutes at a temperature of 80-95°C, and then wash it in clean water to clean the zinc phosphating solution remaining on the surface of the anchor to obtain a phosphated anchor;

[0010] S3. Saponification: Soak the phosphated anchor in saponification solution for 5-10 minutes at a temperature of 60-75°C. Repeat the soaking 3-5 times to obtain the saponified anchor, and then dry at room temperature.

[0011] The saponification treatment liquid comprises the following components in parts by weight: 20-40 parts of soap, 12-25 parts of aloe extract, 30-50 parts of sodium dodecylbenzene sulfonate, 3-8 parts of modified diatomaceous earth, 6-12 parts of sodium carboxymethyl cellulose and 120-280 parts of water.

[0012] By adopting the above technical solution, the anchor is first immersed in a de-impurity liquid to remove impurities on the surface of the anchor, and then immersed in a zinc-based phosphating liquid to provide protection for the surface of the anchor to improve the corrosion resistance of the anchor, and then immersed in a saponification treatment liquid to increase the lubrication properties of the phosphating film to prepare for the next step of stretching, extrusion and other processes.

[0013] The saponification treatment liquid includes soap, aloe vera extract, sodium dodecylbenzene sulfonate, modified diatomaceous earth and sodium carboxymethyl cellulose. All components are environmentally friendly and pollution-free substances. During the saponification treatment process, zero emissions, no pollution to the surrounding environment, and environmental protection and energy saving are achieved. The main component of soap is sodium stearate. Sodium stearate forms a protective boundary lubrication film with the surface of the anchor. After the anchor is treated with zinc phosphating liquid, the surface is covered with a layer of zinc phosphate. When in contact with the saponification treatment liquid, zinc phosphate and sodium stearate undergo a double decomposition reaction. The zinc phosphate layer is converted into a zinc stearate layer with better lubrication properties, making the surface of the anchor smoother and facilitating the subsequent processing of the anchor. Aloe vera extract contains mucus, and aloe vera itself has a moisturizing effect, which increases the viscosity of soapy water and helps the further reaction of sodium stearate. In addition, aloe vera extract has a bactericidal effect, which ensures a good sanitary environment for the saponification treatment liquid and helps the recycling of the saponification treatment liquid. Sodium dodecylbenzene sulfonate has good surface activity. , wetting, penetration and emulsification properties. Sodium dodecylbenzene sulfonate and sodium stearate produce a synergistic effect to promote the lubrication effect of sodium stearate. Modified diatomaceous earth has a large specific surface area, high porosity and strong adsorption effect, which increases the adsorption capacity of the saponification reaction liquid on the surface of the anchor, can be firmly and directionally adsorbed on the surface of the anchor, increases the activation energy of the corrosion reaction, and enhances the rust resistance of the anchor. Sodium carboxymethyl cellulose can be used as an emulsifier, dispersant, and adhesive, which can make the modified diatomaceous earth evenly distributed in the solution, and can also increase the viscosity of the solution, so that the sodium stearate can further lubricate the anchor, increase the lubricity, aging resistance and corrosion resistance of the saponification treatment liquid, and then increase the smoothness of the anchor surface, which is convenient for the subsequent processing of the anchor.

[0014] Preferably, the method for preparing the saponification treatment solution comprises the following steps:

[0015] (1) dissolving soap in water, then adding sodium carboxymethyl cellulose, stirring at 1000-1800 rpm for 30-60 min to obtain a mixture 1;

[0016] (2) Adding aloe extract, sodium dodecylbenzene sulfonate and modified diatomaceous earth to the mixture obtained in step (1), stirring at a temperature of 60-85° C. for 1-3 hours to obtain a saponified solution.

[0017] By adopting the above technical scheme, sodium carboxymethyl cellulose is a surfactant, which is evenly dispersed in soapy water to increase the viscosity of the soapy water, and then aloe vera extract, sodium dodecylbenzene sulfonate and modified diatomaceous earth are added. Heating helps to evenly mix the raw materials. The combination of aloe vera extract and modified diatomaceous earth further improves the adsorption of the anchor surface, can adsorb reactants on the anchor surface, and further enhances the rust resistance, lubricity and corrosion resistance of the anchor.

[0018] Preferably, the preparation method of the aloe extract comprises the following steps:

[0019] (1) Slice fresh aloe vera, add ethanol, crush, squeeze for 20-40 minutes, and filter to obtain aloe vera juice;

[0020] (2) mixing the aloe vera juice obtained in step (1), sodium alginate, nanocellulose and polyethylene glycol, and stirring at a temperature of 60-80° C. for 10-20 minutes to obtain an aloe vera extract.

[0021] By adopting the above technical scheme, sodium alginate increases the viscosity of aloe juice, nanocellulose is used as a reinforcing agent to increase the viscosity and strength of the solution system, sodium alginate is cross-linked with the macromolecular active substances in the aloe juice, nanocellulose has a small volume and is filled into the structure of sodium alginate to enhance the strength and viscosity of the system, polyethylene glycol is further cross-linked with sodium alginate to improve the gel properties of the system, and further enhance the structural strength and bonding properties of the system; the preparation of aloe extract is applied to the subsequent saponification reaction liquid, which increases the viscosity of the saponification reaction liquid system, enables the saponification reaction liquid to better contact with the anchor, increases the lubrication performance of the anchor surface, and further reduces the probability of rust on the anchor surface.

[0022] Preferably, the mass ratio of the aloe juice, sodium alginate and nanocellulose is 1:3-10:2-6.

[0023] By adopting the above technical scheme, the mass ratio of aloe juice, sodium alginate and nanocellulose is controlled to obtain an aloe extract with higher system strength and greater viscosity. The compound of aloe juice, sodium alginate and nanocellulose has a synergistic effect. Aloe juice and sodium alginate are cross-linked to form a cross-linked network structure, and nanocellulose is filled in the pores of the network structure, which further increases the viscosity and strength of the system and helps the subsequent saponification treatment of the anchor.

[0024] Preferably, the nanocellulose has a diameter of 3-20 nm, a length of 120-300 nm, and an aspect ratio of 10-50.

[0025] By adopting the above technical solution, the size of nanocellulose is limited, so that nanocellulose has good bioadaptability, which is conducive to the mixing of nanocellulose and sodium alginate, and the reaction will be more complete, which helps to enhance the mechanical properties of sodium alginate.

[0026] Preferably, the pretreatment method of modified diatomite comprises the following steps: mixing raw diatomite with HCl solution, heating at 80-100°C for 1-3h, filtering, washing and drying; then adding chitosan, cellulose acetate and surfactant, stirring for 1-3h, filtering, drying and grinding to obtain modified diatomite.

[0027] By adopting the above technical scheme, hydrochloric acid not only improves the purity of the original diatomite and removes impurities, but also reduces the density of diatomite, increases the specific surface area of ​​the original diatomite, and improves the pore structure of diatomite, so that the diatomite treated with hydrochloric acid has stronger adsorption and chemical activity, chitosan has good biocompatibility, the pore structure on the surface of the original diatomite promotes the adhesion of chitosan, and chitosan has bonding properties, which increases the stability of the pore structure of diatomite, acetate fiber forms a network structure with chitosan and is mixed with diatomite at the same time, which enhances the structural strength, adsorption and chemical activity of diatomite, and in the subsequent saponification process of the anchor, the adsorption effect of the modified diatomite on the surface of the anchor is increased, which helps to accelerate the lubrication reaction of the anchor, and has better lubrication effect and aging resistance and anti-corrosion performance.

[0028] Preferably, the mass ratio of the diatomaceous earth, chitosan and cellulose acetate is 1:6-15:2.5-6.5.

[0029] By adopting the above technical scheme, the mass ratio of diatomite, chitosan and acetate fiber is controlled to obtain modified diatomite with stronger viscosity, better adsorption and better chemical activity. The diatomite, chitosan and acetate fiber are compounded to form a network cross-linked structure, which improves the strength and adsorption of the diatomite and helps the subsequent saponification treatment of the anchor.

[0030] Preferably, the surfactant is one or more of polyethylene oxide, polystyrene sulfonate and sodium dodecylbenzene sulfonate.

[0031] Preferably, the impurity removal liquid is a mixture of sodium gluconate, fatty alcohol polyoxyethylene ether and lotus leaf extract in a mass ratio of 1:2-5:3-6.

[0032] By adopting the above technical scheme, sodium gluconate contains a considerable number of hydroxyl and carboxyl groups, which can be complexed with metal ions as a ligand to become a chelating agent to remove metal impurities on the surface of the anchor. Fatty alcohol polyoxyethylene ether has good emulsification, cleaning, wetting and degreasing effects, and can remove residual oil stains on the surface of the anchor. The combination of sodium gluconate and fatty alcohol polyoxyethylene ether enhances the cleaning effect and anti-rust ability of the anchor. The lotus leaf extract is alkaline, and the combination of sodium gluconate and fatty alcohol polyoxyethylene ether enhances the chelating ability of sodium gluconate, thereby accelerating the ability to remove impurities on the surface of the anchor.

[0033] Preferably, the zinc-based phosphating solution comprises the following components in parts by weight: 50-80 parts of phosphoric acid, 25-40 parts of zinc oxide, 10-20 parts of zinc dihydrogen phosphate, 1-5 parts of potassium chlorate and 10-20 parts of malic acid.

[0034] By adopting the above technical solution, when the anchor is immersed in the zinc phosphating solution, the Fe anodic oxidation process occurs on the surface, and the phosphate precipitates and crystallizes into a phosphating film. Zinc dihydrogen phosphate and potassium chlorate cooperate to accelerate the Zn 2+ The film-forming rate of phosphating is increased, the phosphating time is shortened, and the corrosion resistance of the phosphating film is significantly improved. Malic acid can accelerate the film-forming rate of phosphating. The use of potassium chlorate and zinc dihydrogen phosphate can well promote the growth of crystal nuclei and improve the stability of the phosphating film. It further makes the phosphating film uniform and dense, and the film layer has better corrosion resistance.

[0035] In summary, this application has the following beneficial effects:

[0036] 1. The saponification treatment liquid of the present application includes soap, aloe extract, sodium dodecylbenzene sulfonate, modified diatomaceous earth and sodium carboxymethyl cellulose. Each component is an environmentally friendly and pollution-free substance. During the saponification treatment process, zero emissions, no pollution to the surrounding environment, and environmental protection and energy saving effects are achieved. The main component of soap is sodium stearate, which forms a protective boundary lubrication film with the surface of the anchor. After the anchor is treated with zinc phosphating liquid, the surface is covered with a layer of zinc phosphate. When in contact with the saponification treatment liquid, the zinc phosphate and sodium stearate undergo a double decomposition reaction, and the zinc phosphate layer is converted into a zinc stearate layer with better lubrication performance, making the surface of the anchor smoother and convenient for subsequent processing of the anchor; aloe vera extract has a moisturizing effect, increases the viscosity of soapy water, and helps the further reaction of sodium stearate. Sodium dodecylbenzene sulfonate and sodium stearate produce a synergistic effect to promote the lubrication of sodium stearate; modified diatomaceous earth has a large specific surface area, high porosity and strong adsorption, which increases the adsorption capacity of the saponification reaction liquid on the anchor surface, can be firmly and directional adsorbed on the anchor surface, increases the activation energy of the corrosion reaction, and enhances the rust resistance of the anchor;.

[0037] 2. The sodium carboxymethyl cellulose of the present application can be used as an emulsifier, dispersant, and adhesive, which can make the modified diatomaceous earth evenly distributed in the solution, and can also increase the viscosity of the solution, so that the sodium stearate can further lubricate the anchor, increase the lubricity, aging resistance and corrosion resistance of the saponification treatment liquid, and then increase the smoothness of the anchor surface, which is convenient for the subsequent processing of the anchor.

[0038] 3. The anchor of the present application is first immersed in a de-impurity liquid to remove impurities on the surface of the anchor, and then immersed in a zinc-based phosphating liquid to provide protection for the surface of the anchor to improve the corrosion resistance of the anchor, and then immersed in a saponification treatment liquid to increase the lubrication properties of the phosphating film to prepare for the next step of stretching, extrusion and other processes. DETAILED DESCRIPTION

[0039] The following examples further illustrate the present application in detail.

[0040] Preparation Example of Aloe Extract

[0041] Preparation Example 1-1

[0042] The preparation method of aloe extract comprises the following steps:

[0043] (1) Slice 10 kg of fresh aloe vera, add 100 L of ethanol, crush, squeeze for 30 min, and filter to obtain aloe vera juice;

[0044] (2) mixing the aloe juice, sodium alginate, nanocellulose and 50 L of polyethylene glycol obtained in step (1), and stirring at 70° C. for 20 minutes to obtain an aloe extract, wherein the mass ratio of the aloe juice, sodium alginate and nanocellulose is 1:6:4; the diameter of the nanocellulose is 3-20 nm, the length is 120-300 nm, and the aspect ratio is between 10-50.

[0045] Preparation Example 1-2

[0046] The difference from Preparation Example 1-1 is that the mass ratio of aloe juice, sodium alginate and nanocellulose is 1:3:2.

[0047] Preparation Example 1-3

[0048] The difference from Preparation Example 1-1 is that the mass ratio of aloe juice, sodium alginate and nanocellulose is 1:10:6.

[0049] Preparation Example 1-4

[0050] The difference from Preparation Example 1-1 is that the mass ratio of aloe juice, sodium alginate and nanocellulose is 1:20:10.

[0051] Preparation Example 1-5

[0052] The difference from Preparation Example 1-1 is that an equal amount of aloe vera juice is used instead of sodium alginate.

[0053] Preparation Example 1-6

[0054] The difference from Preparation Example 1-1 is that an equal amount of aloe vera juice is used instead of nanocellulose.

[0055] Preparation example of modified diatomite

[0056] Preparation Example 2-1

[0057] The pretreatment method of modified diatomite comprises the following steps: taking 40 kg of diatomite raw soil and mixing it with 400 L of HCl solution with a mass fraction of 5%, heating it at a temperature of 90°C for 1 hour, filtering, washing and drying it; then adding chitosan, cellulose acetate and 3 kg of polyethylene oxide, stirring it for 2 hours, filtering, drying and grinding it to obtain modified diatomite, wherein the mass ratio of the diatomite raw soil, chitosan and cellulose acetate is 1:10:4.

[0058] Preparation Example 2-2

[0059] The difference from Preparation Example 2-1 is that the mass ratio of diatomaceous earth, chitosan and acetate fiber is 1:6:2.5.

[0060] Preparation Example 2-3

[0061] The difference from Preparation Example 2-1 is that the mass ratio of diatomaceous earth, chitosan and cellulose acetate is 1:15:6.5.

[0062] Preparation Example 2-4

[0063] The difference from Preparation Example 2-1 is that the mass ratio of diatomaceous earth, chitosan and cellulose acetate is 1:20:1.5.

[0064] Preparation Example 2-5

[0065] The difference from Preparation Example 2-1 is that an equal amount of diatomaceous earth is used instead of chitosan.

[0066] Preparation Example 2-6

[0067] The difference from Preparation Example 2-1 is that an equal amount of diatomaceous earth is used instead of acetate fiber.

[0068] Example

[0069] Example 1

[0070] A processing process for an extruded anchor comprises the following steps:

[0071] S1. De-impurity: The anchor is first placed in a de-impurity liquid for rinsing, and then soaked in ethanol for 2 hours to remove impurities on the surface, thereby obtaining a rinsed anchor;

[0072] S2, phosphating: the rinsed anchor is placed in a zinc phosphating solution for 10 minutes at a soaking temperature of 80°C, and then placed in clean water for cleaning to clean the zinc phosphating solution remaining on the surface of the anchor to obtain a phosphated anchor;

[0073] S3, saponification: put the phosphated anchor into the saponification treatment solution for 8 minutes, the soaking temperature is 75°C, repeat the soaking 3 times to obtain the saponified anchor, and then dry it at room temperature;

[0074] The saponification treatment liquid includes the following components in parts by weight: 30 kg of soap, 20 kg of aloe extract, 40 kg of sodium dodecylbenzene sulfonate, 5 kg of modified diatomaceous earth, 8 kg of sodium carboxymethyl cellulose and 200 kg of water. The aloe extract is prepared by Preparation Example 1-1; the modified diatomaceous earth is prepared by Preparation Example 2-1.

[0075] The method for preparing the saponification treatment liquid comprises the following steps:

[0076] (1) Dissolve soap in water, then add sodium carboxymethyl cellulose, and stir at 1800 rpm for 45 min to obtain a mixture 1;

[0077] (2) Add aloe extract, sodium dodecylbenzene sulfonate and modified diatomaceous earth to the mixture obtained in step (1), stir at 80° C. for 2 h, and obtain a saponified solution.

[0078] The impurity removal liquid is a mixture of sodium gluconate, fatty alcohol polyoxyethylene ether and lotus leaf extract in a mass ratio of 1:4:4.

[0079] The zinc-based phosphating solution includes the following components in parts by weight: 60 kg of phosphoric acid, 30 kg of zinc oxide, 15 kg of zinc dihydrogen phosphate, 3 kg of potassium chlorate, and 15 kg of malic acid. The zinc-based phosphating solution is prepared by mixing phosphoric acid, zinc oxide, zinc dihydrogen phosphate, potassium chlorate, and malic acid.

[0080] Example 2

[0081] The difference from Example 1 is that, in a treatment process for an extruded anchor, the saponification treatment liquid includes the following components in parts by weight: 40 kg of soap, 12 kg of aloe extract, 30 kg of sodium dodecylbenzene sulfonate, 3 kg of modified diatomaceous earth, 6 kg of sodium carboxymethyl cellulose and 120 kg of water.

[0082] Example 3

[0083] The difference from Example 1 is that, in a treatment process for an extruded anchor, the saponification treatment liquid comprises the following components in parts by weight: 20 kg of soap, 25 kg of aloe extract, 50 kg of sodium dodecylbenzene sulfonate, 8 kg of modified diatomaceous earth, 12 kg of sodium carboxymethyl cellulose and 280 kg of water.

[0084] Example 4

[0085] The difference from Example 1 is that the impurity removal liquid is a mixture of sodium gluconate, fatty alcohol polyoxyethylene ether and lotus leaf extract in a mass ratio of 1:2:3.

[0086] Example 5

[0087] The difference from Example 1 is that the zinc-based phosphating solution includes the following components in parts by weight: 80 kg of phosphoric acid, 25 kg of zinc oxide, 10 kg of zinc dihydrogen phosphate, 5 kg of potassium chlorate, and 10 kg of malic acid.

[0088] Example 6

[0089] The difference from Example 1 is that the aloe extract is prepared using Preparation Example 1-2.

[0090] Example 7

[0091] The difference from Example 1 is that the aloe extract is prepared using Preparation Example 1-3.

[0092] Example 8

[0093] The difference from Example 1 is that the aloe extract is prepared using Preparation Examples 1-4.

[0094] Example 9

[0095] The difference from Example 1 is that the aloe extract is prepared using Preparation Examples 1-5.

[0096] Example 10

[0097] The difference from Example 1 is that the aloe extract is prepared using Preparation Examples 1-6.

[0098] Embodiment 11

[0099] The difference from Example 1 is that the modified diatomaceous earth is prepared using Preparation Example 2-2.

[0100] Example 12

[0101] The difference from Example 1 is that the modified diatomaceous earth is prepared using Preparation Example 2-3.

[0102] Embodiment 13

[0103] The difference from Example 1 is that the modified diatomaceous earth is prepared using Preparation Example 2-4.

[0104] Embodiment 14

[0105] The difference from Example 1 is that the modified diatomaceous earth is prepared using Preparation Example 2-5.

[0106] Embodiment 15

[0107] The difference from Example 1 is that the modified diatomaceous earth is prepared using Preparation Example 2-6.

[0108] Comparative Example

[0109] Comparative Example 1

[0110] A treatment process for an extruded anchor comprises the following components, wherein a saponification treatment liquid comprises the following components in parts by weight: 10 kg of soap, 30 kg of aloe extract, 20 kg of sodium dodecylbenzene sulfonate, 12 kg of modified diatomaceous earth, 3 kg of sodium carboxymethyl cellulose and 100 kg of water.

[0111] Comparative Example 2

[0112] The difference from Example 1 is that the saponification treatment liquid includes the following components in parts by weight: 50 kg of soap, 10 kg of aloe extract, 70 kg of sodium dodecylbenzene sulfonate, 2 kg of modified diatomaceous earth, 15 kg of sodium carboxymethyl cellulose and 300 kg of water.

[0113] Comparative Example 3

[0114] The difference from Example 1 is that an equal amount of soap is used to replace the aloe extract.

[0115] Comparative Example 4

[0116] The difference from Example 1 is that an equal amount of soap is used to replace the modified diatomaceous earth.

[0117] Comparative Example 5

[0118] The difference from Example 1 is that an equal amount of diatomaceous earth is used instead of modified diatomaceous earth.

[0119] Performance testing

[0120] Detection method / test method

[0121] 1. Treat the anchor samples according to the treatment process of Examples 1-15 and Comparative Examples 1-5, and test the board appearance, salt spray resistance test, and film removability test.

[0122] (1) Board surface appearance: Observe the board surface with the naked eye to see whether it is flat and uniform.

[0123] (2) Salt spray resistance test: The test is carried out in accordance with the national standard "GB / T 10125-2012 Artificial atmosphere corrosion test salt spray test", with a test temperature of 30±2℃ and a NaCl concentration of 50±5g / L. The time when the white rust area of ​​the anchor sample is greater than 5% is recorded; the anchor sample is subjected to an artificial aging test using a UV accelerated aging test machine to observe the condition of the lubricating film.

[0124] (3) Demolding test: The anchor sample was immersed in a 3% NaOH aqueous solution at 30°C for 30 seconds, and the weight of the lubricating film before and after demolding was measured using a film measuring instrument to calculate the lubricating film residual rate. Lubricating film residual rate (%) = (lubricating film weight after demolding treatment / lubricating film weight before demolding treatment) * 100. The test results are shown in Table 1.

[0125] Table 1

[0126] Board appearance Salt spray time (h) Resistance to artificial accelerated aging (h) Lubricating film residual rate (%) Example 1 Smooth and even 200 80h slight powdering 2.0% Example 2 Smooth and even 200 79h Slightly powdery 2.1% Example 3 Smooth and even 199 80h slight powdering 2.0% Example 4 Smooth and even 198 78h slight powdering 2.0% Example 5 Smooth and even 199 79h Slightly powdery 2.1% Example 6 Smooth and even 199 79h Slightly powdery 2.0% Example 7 Smooth and even 200 78h slight powdering 2.1% Example 8 Smooth and even 183 68h slight powdering 5% Example 9 Smooth and even 151 42h slight powdering 3% Example 10 Smooth and even 165 57h Slightly powdery 6% Embodiment 11 Smooth and even 199 79h Slightly powdery 2.0% Example 12 Smooth and even 198 78h slight powdering 2.1% Embodiment 13 Smooth and even 178 64h slight powdering 6% Embodiment 14 Smooth and even 151 58h slight powdering 4% Embodiment 15 Smooth and even 160 49h slight powdering 5% Comparative Example 1 Smooth and even 180 65h slight powdering 8% Comparative Example 2 Smooth and even 178 63h Slightly powdery 9% Comparative Example 3 Smooth and even 120 32h slight powdering 12% Comparative Example 4 Smooth and even 100 21h slight powdering 15% Comparative Example 5 Smooth and even 159 62h slight powdering 13%

[0127] As can be seen from Table 1, the anchors treated by the present application have excellent aging and corrosion resistance, salt spray resistance and no film release after treatment in Examples 1-7 and 11-12. The salt spray resistance reaches 200 hours, and the saponification film has slight powdering after 80 hours, and the residual rate of the lubricating film is 2%. This shows that the saponification treatment liquid prepared by the present application has good lubricity, aging resistance and corrosion resistance, thereby increasing the smoothness of the anchor surface and facilitating the subsequent processing of the anchor.

[0128] Example 8 changes the mass ratio of aloe juice, sodium alginate and nanocellulose. It can be seen from Table 1 that the salt spray resistance is 183h, the saponification film has slight powdering after 68h, and the residual rate of the lubricating film is 5%. Compared with Examples 1, 6-7, the mass ratio of aloe juice, sodium alginate and nanocellulose is 1:3-10:2-6, and the treated anchor has excellent aging resistance and corrosion resistance, salt spray resistance and no demolding property, indicating that the compound of aloe juice, sodium alginate and nanocellulose has good physical and chemical properties, which is helpful for the subsequent processing of the anchor.

[0129] In Example 9, no sodium alginate is added. As can be seen from Table 1, the salt spray resistance of the anchor is 151h, the saponification film has slight powdering after 42h, and the residual rate of the lubricating film is 3%. In Example 10, no nanocellulose is added. The salt spray resistance of the anchor is 165h, the saponification film has slight powdering after 57h, and the residual rate of the lubricating film is 6%. Compared with Examples 1 and 6-8, which do not add sodium alginate and nanocellulose respectively, the aging resistance and corrosion resistance and salt spray resistance of the treated anchor are relatively poor, indicating that sodium alginate increases the viscosity of aloe juice, sodium alginate is cross-linked with the macromolecular active substances in the aloe juice, and nanocellulose is filled in the pores of the network structure, which further increases the viscosity and strength of the system and increases the subsequent lubrication performance of the anchor surface.

[0130] Example 13 changes the mass ratio of diatomaceous earth, chitosan and acetate fiber. It can be seen from Table 1 that the salt spray resistance is 178h, the saponification film is slightly powdered after 64h, and the residual rate of the lubricating film is 6%. Compared with Examples 1 and 11-12, the mass ratio of diatomaceous earth, chitosan and acetate fiber is 1:6-15:2.5-6.5. The treated anchor has excellent aging resistance and corrosion resistance, salt spray resistance and no demolding property, indicating that the compound between diatomaceous earth, chitosan and acetate fiber has good physical and chemical properties, which is helpful for the subsequent processing of the anchor.

[0131] In Example 14, no chitosan is added. As can be seen from Table 1, the salt spray resistance of the anchor is 151h, the saponification film has slight powdering after 58h, and the residual rate of the lubricating film is 4%. In Example 10, no acetate fiber is added, and the salt spray resistance of the anchor is 160h. The saponification film has slight powdering after 49h, and the residual rate of the lubricating film is 5%. Compared with Examples 1, 11-12, no chitosan and acetate fiber are added respectively. The aging resistance and corrosion resistance of the treated anchor are relatively poor, and the salt spray resistance is relatively high, and the residual rate of the lubricating film is high, indicating that chitosan has bonding properties and increases the stability of the pore structure of diatomaceous earth. Acetate fiber forms a network structure with chitosan and is mixed with diatomaceous earth, which enhances the structural strength, adsorption and chemical activity of the diatomaceous earth, further increases the viscosity and strength of the system, and increases the subsequent lubrication and aging resistance of the anchor surface.

[0132] Comparative Example 1-2 changes the content of each component of the saponification treatment liquid. It can be seen from Table 1 that the salt spray resistance of the anchor reaches 180h, the saponification film is slightly powdered after 65h, and the residual rate of the lubricating film is 9%. It can be seen that the components of the present application cooperate with each other and work together to make the prepared anchor have better lubricity, aging resistance and corrosion resistance, thereby increasing the smoothness of the anchor surface.

[0133] In Comparative Example 3, aloe vera extract is not added. As can be seen from Table 1, the salt spray resistance of the anchor is 120h, the saponification film is slightly powdered after 32h, and the residual rate of the lubricating film is 12%. Compared with Example 1, the aging and corrosion resistance and salt spray resistance of the treated anchor are relatively poor, and the residual rate of the lubricating film is relatively high, indicating that the aloe vera extract increases the viscosity of soapy water and promotes the further reaction of sodium stearate. Subsequently, it cooperates with other components to increase the lubricity, aging resistance and corrosion resistance of the saponification treatment liquid, which is convenient for the subsequent processing of the anchor.

[0134] Comparative Example 4 does not add modified diatomaceous earth. As can be seen from Table 1, the salt spray resistance of the anchor is 100h, the saponification film is slightly powdered after 21h, and the residual rate of the lubricating film is 15%. Compared with Example 1, the aging resistance and corrosion resistance and salt spray resistance of the treated anchor are relatively poor, and the residual rate of the lubricating film is relatively high, indicating that the modified diatomaceous earth increases the adsorption capacity of the saponification reaction liquid on the surface of the anchor, increases the activation energy of the corrosion reaction, and enhances the rust resistance of the anchor. When combined with other components, the combined effect is better.

[0135] In Comparative Example 5, an equal amount of diatomaceous earth is used instead of modified diatomaceous earth. As can be seen from Table 1, the salt spray resistance of the anchor is 159h, the saponification film is slightly powdered after 62h, and the residual rate of the lubricating film is 13%. Compared with Example 1, the aging and corrosion resistance and salt spray resistance of the treated anchor are relatively poor, and the residual rate of the lubricating film is relatively high, indicating that the modified diatomaceous earth prepared in the present application has a large specific surface area, a high porosity and a strong adsorption effect, which is helpful for subsequent coordination with other components. The obtained saponification treatment liquid has good lubricity, aging resistance and corrosion resistance, thereby increasing the smoothness of the anchor surface and facilitating the subsequent processing of the anchor.

[0136] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed. However, as long as it is within the scope of the claims of the present application, it shall be protected by the patent law.

Claims

1. A processing process for an extruded anchor, characterized in that: The following steps are involved: S1. De-impurity: The anchor is first placed in a de-impurity liquid for rinsing, and then soaked in ethanol for 1-2 hours to remove impurities on the surface, thereby obtaining a rinsed anchor; S2. Phosphating: Soak the rinsed anchor in a zinc phosphating solution for 10-15 minutes at a temperature of 80-95°C, and then wash it in clean water to clean the zinc phosphating solution remaining on the surface of the anchor to obtain a phosphated anchor; S3. Saponification: Soak the phosphated anchor in saponification solution for 5-10 minutes at a temperature of 60-75°C. Repeat the soaking 3-5 times to obtain the saponified anchor, and then dry at room temperature. The saponification treatment liquid comprises the following components in parts by weight: 20-40 parts of soap, 12-25 parts of aloe extract, 30-50 parts of sodium dodecylbenzene sulfonate, 3-8 parts of modified diatomaceous earth, 6-12 parts of sodium carboxymethyl cellulose and 120-280 parts of water; The preparation method of the aloe extract comprises the following steps: (1) Slice fresh aloe vera, add ethanol, crush, squeeze for 20-40 minutes, and filter to obtain aloe vera juice; (2) mixing the aloe vera juice obtained in step (1), sodium alginate, nanocellulose and polyethylene glycol, and stirring at a temperature of 60-80° C. for 10-20 minutes to obtain an aloe vera extract; The modified diatomite pretreatment method comprises the following steps: mixing raw diatomite with HCl solution, heating at 80-100°C for 1-3h, filtering, washing and drying; then adding chitosan, cellulose acetate and surfactant, stirring for 1-3h, filtering, drying and grinding to obtain the modified diatomite.

2. A processing process for a squeeze anchor according to claim 1, characterized in that: The method for preparing the saponification treatment liquid comprises the following steps: (1) Dissolve soap in water, then add sodium carboxymethyl cellulose, and stir at 1000-1800 rpm for 30-60 min to obtain a mixture 1; (2) Add aloe extract, sodium dodecylbenzene sulfonate and modified diatomaceous earth to the mixture obtained in step (1), stir at a temperature of 60-85° C. for 1-3 hours to obtain a saponified solution.

3. A processing process for a squeeze anchor according to claim 1, characterized in that: The mass ratio of the aloe juice, sodium alginate and nanocellulose is 1:3-10:2-6.

4. A processing process for a squeeze anchor according to claim 1, characterized in that: The nanocellulose has a diameter of 3-20 nm, a length of 120-300 nm, and an aspect ratio of 10-50.

5. A processing process for a squeeze anchor according to claim 1, characterized in that: The mass ratio of the diatomaceous earth, chitosan and acetate fiber is 1:6-15:2.5-6.

5.

6. A processing method for a squeeze anchor according to claim 1, characterized in that: The surfactant is one or more of polyethylene oxide, polystyrene sulfonate and sodium dodecylbenzene sulfonate.

7. A processing method for a squeeze anchor according to claim 1, characterized in that: The impurity removal liquid is prepared by mixing sodium gluconate, fatty alcohol polyoxyethylene ether and lotus leaf extract in a mass ratio of 1:2-5:3-6.

8. The processing method of a squeeze anchor according to claim 1, characterized in that: The zinc phosphating solution comprises the following components in parts by weight: 50-80 parts of phosphoric acid, 25-40 parts of zinc oxide, 10-20 parts of zinc dihydrogen phosphate, 1-5 parts of potassium chlorate and 10-20 parts of malic acid.

Citation Information

Patent Citations

  • Preparation method for phosphating ferrous lithium high-temperature-resistant phosphating film material for metal

    CN105063589A

  • Steel rim vehicle wheel surface phosphating treatment method

    CN108914110A

  • Phosphating process for steel pipe

    CN110359036A

  • Stainless steel range hood surface treatment liquid and preparation method thereof

    CN110484378A

  • Phosphating treatment method for surface of stamping die

    CN112853334A