An electrothermal soft bulletproof vest and a preparation method thereof

The electrically heated soft bulletproof vest with a sandwich structure, combining a conductive leather layer, a shear-thickening adhesive layer, and a non-woven fabric layer, solves the problems of traditional bulletproof vests being heavy, uncomfortable, and unable to provide heat in low-temperature environments. It achieves a combination of flexibility, protection, and electrothermal performance, and has real-time safety monitoring capabilities.

CN115854786BActive Publication Date: 2024-11-26UNIV OF SCI & TECH OF CHINA
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202211666189.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-23
Publication Date
2024-11-26
Estimated Expiration
2042-12-23

AI Technical Summary

Technical Problem

Existing bulletproof vest materials suffer from problems such as heavy weight, poor comfort, and inability to provide heat in low-temperature environments. Furthermore, flexible composite materials have not been sufficiently developed in terms of energy absorption and intelligent features.

Method used

The electrothermal soft bulletproof vest with a sandwich structure includes a conductive leather layer, a shear-thickened adhesive layer, and a non-woven fabric layer. It forms a conductive network by filtering MXene conductive material and combines it with a wireless sensing module to achieve electrothermal performance and protective function.

Benefits of technology

It combines flexibility, protection, and electrothermal performance, providing heat in cold environments and monitoring safety status in real time via wireless devices, thus enhancing wearing comfort and intelligence.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115854786B_ABST
    Figure CN115854786B_ABST
Patent Text Reader

Abstract

The present invention relates to an electric heating soft bulletproof vest and a preparation method thereof, wherein the vest is a sandwich structure, including a conductive leather layer, a shear thickening adhesive layer and a non-woven fabric layer, and the layers are tightly combined by the viscosity of the shear thickening adhesive. The present invention can be widely used in the field of soft bulletproof vests, not only can it resist impact, but also can help the wearer resist the cold and harsh environment with its electric heating performance, and can also transmit the impact signal to a mobile phone through a wireless device to monitor the safety status in real time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of multifunctional protection, and in particular to a soft bulletproof vest with electric heating performance and impact resistance and a preparation method thereof. Background Art

[0002] The bulletproof layer materials in traditional bulletproof vests are mostly high-strength materials: steel plates, ceramics, titanium alloys, etc. Although they have good impact resistance, they are hard and bulky, not comfortable, affect movement, and cannot provide the required heat for the human body in low temperature environments. In addition, when these hard materials are hit by bullets, they are also difficult to block the huge kinetic energy brought by the bullet impact. In recent years, a series of flexible materials have been developed for use as bulletproof materials. Bulletproof vests are gradually developing towards lightweight, intelligent, and multifunctional, and are gradually replacing traditional hard armor.

[0003] Leather is a traditional natural polymer material derived from animal skin, with good biocompatibility with the human body and excellent physical properties. As a popular material for ancient clothing, it is also widely used to prepare some multifunctional composite materials, such as leather sensors, flame-retardant leather, thermal camouflage leather, etc. The Chinese patent with publication number CN110957058B discloses a graphene-based conductive leather, which uses polyurethane as an elastic support, solves the bonding strength between graphene and leather fibers, and improves conductivity and elasticity. Although there are many interesting multifunctional leather composites, few people pay attention to energy absorption, which is very critical in bulletproof vests.

[0004] Shear thickening material is a strain rate-dependent flexible material. When the external force stimulus exceeds a critical value, its modulus or viscosity will increase sharply. This unique property demonstrates its great potential in soft body armor, and the flexible feature will not affect wearing comfort. The Chinese patent with publication number CN114322662B proposes an energy collection-storage wearable protective device and a preparation method thereof, using a shear-hardening rubber composite material as an energy collection module, and exhibiting excellent mechanical properties. The Chinese patent with publication number CN114395926A discloses a shear thickening rubber reinforced fabric composite material, which uses a hollow fabric to encapsulate the shear thickening rubber to obtain a wearable, flexible composite material with good protection under low-speed impact.

[0005] Judging from the currently disclosed patents, shear thickening gel composites have excellent protective effects when dealing with impacts, and have certain development potential as bulletproof vest materials, but their intelligence and multifunctionality are difficult to guarantee, and most composite materials are difficult to be specifically applied to wearable bulletproof vests due to poor biocompatibility. Flexible leather-based materials are highly functional and suitable for wear, but there is little research in the field of energy absorption. Obviously, combining the two to design soft bulletproof vests with flexibility, versatility and impact resistance has important application prospects in related fields. Summary of the invention

[0006] The technology of the present invention solves the problem: Overcoming the shortcomings of the prior art, providing an electrothermal soft bulletproof vest and a preparation method thereof, the bulletproof vest integrates flexibility, protection, in-situ sensing and electrothermal performance, and can be widely used in the field of soft bulletproof vests. While protecting the user from impact, its electrothermal performance can also help the wearer resist the harsh cold environment and monitor the safety status in real time through wireless devices.

[0007] The present invention is achieved through the following technical solutions:

[0008] In the first aspect, an electrothermal soft bulletproof vest of the present invention integrates protection, in-situ sensing and electrothermal performance. The vest is a sandwich structure, including a conductive leather layer, a shear thickening adhesive layer and a non-woven fabric layer, and the layers are tightly combined by the viscosity of the shear thickening adhesive; the conductive leather layer is a sensing layer and an electric heating layer, and the shear thickening adhesive layer is the main protective layer.

[0009] Furthermore, the conductive leather layer is cowhide, which is cut into a vest style and treated with ethanol to remove the waterproof layer on the surface of the vest; then the treated vest is filtered, and the filtration method is as follows: the MXene conductive material is filtered through the treated vest with the conductive leather layer to form an array, and the filtered MXene conductive material sheets are completely dispersed in the multi-level structure network of the vest to form a conductive network.

[0010] Furthermore, the volume of the suction filtration is 1 to 20 mL.

[0011] Furthermore, the shear thickening adhesive layer is formed by cross-linking silicone oil and boric acid, and is completely adhered to the inner side of the conductive leather layer; the mass ratio of the silicone oil and boric acid is 20:1 to 30:1; and the shear thickening adhesive is formed at a temperature of 160°C to 200°C.

[0012] Furthermore, the changes in electrical signals generated by the impact of the vest are wirelessly transmitted through wireless devices to monitor the safety of the human body in situ.

[0013] Furthermore, the conductive leather layer is connected via a Bluetooth sensor module.

[0014] In a second aspect, the present invention provides a method for preparing the electrothermal soft bulletproof vest, comprising the following steps:

[0015] a. The silicone oil and boric acid are mixed evenly in a ratio of 20:1 to 30:1, and then placed in an oven for heat treatment at 160°C to 200°C, and n-octanoic acid is added in the middle to obtain a shear thickening glue after cross-linking;

[0016] b. Preparation of MXene aqueous solution by HF etching;

[0017] c. Cut the leather into the shape of a vest and then further treat it with ethanol to remove the waterproof layer on the surface of the vest;

[0018] d. The array area is pre-divided on the front and back of the vest, and the MXene aqueous solution is filtered; 1-20mL of MXene aqueous solution is filtered from each subunit in the array and dried at room temperature;

[0019] e. Use silver paste and copper foil to build electrodes on the surface of each subunit to complete the conductive path;

[0020] f. Apply the shear thickening glue evenly on the inside of the vest at a mass ratio of 1:1 to 1:5, then cut the non-woven fabric into a specified shape and attach it to the shear thickening glue to form a sandwich structure to obtain an electric heating soft bulletproof vest.

[0021] The advantages of the present invention compared with the prior art are:

[0022] (1) The present invention uses leather as a matrix and adopts a preparation method of suction filtration to obtain conductive leather, and designs a flexible multifunctional soft bulletproof vest. The bulletproof vest integrates protection, in-situ sensing and electrothermal performance, and can be widely used in the field of soft bulletproof vests. It can not only resist impact, but also help the wearer resist the cold and harsh environment with its electrothermal performance. In addition, the impact signal can be transmitted to the mobile phone through a wireless device to monitor the safety status in real time.

[0023] (2) The present invention can be widely used in the field of intelligent and multifunctional soft bulletproof vests. While effectively buffering impact damage and protecting human safety, it can also provide heat through electrothermal properties to help the wearer stay warm in cold environments.

[0024] (3) All layers of the present invention are made of flexible materials, and leather as the base material further increases wearing comfort. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 The voltammetric curves of conductive leather with different MXene volumes filtered;

[0026] Figure 2is the resistance of conductive leather with different MXene contents;

[0027] Figure 3 The temperature change of conductive leather with different MXene contents at 3.0V voltage;

[0028] Figure 4 The temperature change of the conductive leather under different voltages for filtering 10mL MXene;

[0029] Figure 5 The temperature change of the conductive leather / shear thickening glue / non-woven fabric subunit under different voltages;

[0030] Figure 6 It is the power-on and power-off cycle curve of the conductive leather / shear thickening adhesive / non-woven fabric subunit at a voltage of 3.0V;

[0031] Figure 7 The temperature change curve of the conductive leather / shear thickening glue / non-woven fabric subunit under step voltage;

[0032] Figure 8 The rheological properties of the shear thickening glue;

[0033] Fig. 9 The stress-strain curves of conductive leather with different MXene contents;

[0034] Fig.10 Force signals of conductive leather with different MXene contents under drop hammer impact;

[0035] Fig.11 Force signals of samples containing different shear thickening glues (SSG) under falling weight impact (sample X means that the mass of shear thickening glue is X times that of leather;

[0036] Fig.12 The comparison of the resistance signal changes of the samples under the impact of falling hammers at different heights (the mass of the shear thickening glue used in the samples is 1 times the mass of the leather);

[0037] Fig.13 This is the process of the mobile phone receiving the resistance signal when the hammer hits the vest;

[0038] Fig.14 is the initial velocity-residual velocity curve of leather and sample at bullet impact;

[0039] Fig.15 A display picture of the designed vest;

[0040] Fig.16 This is a diagram showing the location of the MXene array on the inside of the vest;

[0041] Fig.17This is the infrared image of the vest when it is powered on (the human body's comfortable temperature is around 35°C);

[0042] Fig.18 This is the infrared image of the vest when it is powered on (the highest temperature is around 65℃);

[0043] Fig.19 It is a structural diagram of the electric heating bulletproof vest of the present invention;

[0044] Fig. 20 It is a flow chart for realizing the preparation method of the present invention. DETAILED DESCRIPTION

[0045] The present invention is described in detail below with reference to the accompanying drawings and embodiments.

[0046] The performance parameters of the samples prepared in the examples were tested according to the following test methods:

[0047] A. The specific method for measuring the electrical properties of conductive leather is as follows:

[0048] The conductive leather was connected to copper foil with silver paste as electrodes, and the electrical properties were measured using an impedance meter test system (Solartron Analytical, AMETEK Advanced Measurement Technology, Inc.).

[0049] B. The specific method for measuring the rheological properties of shear thickening glue is as follows:

[0050] The shear thickening gel was pressed into a film with a thickness of 1 mm and a diameter of 20 mm using a mold, and its shear thickening properties were then characterized using a commercial rheometer (Physica MCR 302, Anton Paar Co., Austria).

[0051] C. The specific method for measuring the electrothermal performance of the sample is as follows:

[0052] The sample was placed on the printed sample holder, and the temperature signal was collected using an automatic range DC power supply (IT8500, Itech Electronics Co., Ltd.) and a thermocouple (DT-3891G, Shenzhen Hengjia Machinery Industry Co., Ltd.).

[0053] D. The specific method of measuring the electrothermal performance of the vest is as follows:

[0054] The vest was put on the human-shaped mold and powered by a DC power supply (IT8500, Itech Electronics Co., Ltd.), and the electrical and thermal properties of the vest were collected using an infrared camera (ImageIR 8325).

[0055] E. The specific method of the protective performance of the sample under low-speed impact is as follows:

[0056] The sample was placed on a force sensor (KD3005C, Yangzhou Kedong), and a 0.55 kg hammer was released from different heights using a drop hammer impact device (ZCJ1302-A, Meters Industries). After the sample was impacted, the force sensor amplified the signal through a charge amplifier (YE5853, Donghua Testing), and finally the data was collected through a digital oscilloscope (Tektronix DPO2014B).

[0057] F. The specific method for measuring the protective performance of the sample under ballistic impact is as follows:

[0058] In the high-speed ballistic impact test, the whole system consists of an air gun (manufacturer and model not available), a laser velocimeter (manufacturer and model not available), a high-speed camera (PHANTOM 2701090-1650) and a digital oscilloscope (Tektronix DPO 2014B). The sample is fixed on the fixture and clamped by screws. The distance between the muzzle and the fixture is 15 cm. The speed of the bullet is controlled by adjusting the air pressure. The initial velocity of the bullet is measured by the laser velocimeter, and the residual velocity is collected by high-speed photography.

[0059] The preparation method of MXene aqueous solution is as follows:

[0060] 1 g LiF and 20 mL HCL were added to a polytetrafluoroethylene beaker and stirred for half an hour. Then 1 g MAX was added intermittently at 60 °C. After stirring evenly, the mixture was reacted on a magnetic stirrer for 24 h. The product was then centrifuged and the upper layer solution was taken to obtain an aqueous solution of MXene.

[0061] Among them: LiF and MAX were purchased from Aladdin Chemical Co., Ltd., China.

[0062] The method for preparing the conductive leather subunit sample is as follows:

[0063] The leather surface was soaked with ethanol, and the waterproof layer on the surface was removed by gently polishing with sandpaper. 1 mL of the solution was taken with a pipette for filtration. The leather was cut into 5*5 cm in size and sandwiched in the middle of the filtration bottle. After filtration, it was dried at room temperature to obtain conductive leather. Then, copper foil was attached to the surface with silver paste as an electrode. Then, the same mass of shear thickening glue was applied on the fiber side, and a non-woven fabric layer was attached to obtain a subunit sample of a sandwich structure.

[0064] Wherein: the leather is ordinary commercial natural cowhide; the model of the filtration device is SHZ-111B circulating water multi-purpose vacuum pump.

[0065] The method for preparing the conductive leather subunit sample is as follows:

[0066] The leather surface was soaked with ethanol, and the waterproof layer on the surface was removed by gently polishing with sandpaper. 5 mL of the solution was taken with a pipette for filtration. The leather was cut into 5*5 cm in size and sandwiched in the middle of the filtration bottle. After filtration, it was dried at room temperature to obtain conductive leather. Then, copper foil was attached to the surface with silver paste as an electrode. Then, the same mass of shear thickening glue was applied on the fiber side, and a non-woven fabric layer was attached to obtain a subunit sample of a sandwich structure.

[0067] Wherein: the leather is ordinary commercial natural cowhide; the model of the filtration device is SHZ-111B circulating water multi-purpose vacuum pump.

[0068] The method for preparing the conductive leather subunit sample is as follows:

[0069] The leather surface was soaked with ethanol, and the waterproof layer on the surface was removed by gently polishing with sandpaper. 10 mL of the solution was taken with a pipette for filtration. The leather was cut into 5*5 cm in size and sandwiched in the middle of the filtration bottle. After filtration, it was dried at room temperature to obtain conductive leather. Then, copper foil was attached to the surface with silver paste as an electrode. Then, the same mass of shear thickening glue was applied on the fiber side, and a non-woven fabric layer was attached to obtain a subunit sample of a sandwich structure.

[0070] Wherein: the leather is ordinary commercial natural cowhide; the model of the filtration device is SHZ-111B circulating water multi-purpose vacuum pump.

[0071] The method for preparing the conductive leather subunit sample is as follows:

[0072] The leather surface was soaked with ethanol, and the waterproof layer on the surface was removed by gently polishing with sandpaper. 15 mL of the solution was taken with a pipette for filtration. The leather was cut into 5*5 cm in size and sandwiched in the middle of the filtration bottle. After filtration, it was dried at room temperature to obtain conductive leather. Then, copper foil was attached to the surface with silver paste as an electrode. Then, the same mass of shear thickening glue was applied on the fiber side, and a non-woven fabric layer was attached to obtain a sub-unit sample of a sandwich structure.

[0073] Wherein: the leather is ordinary commercial natural cowhide; the model of the filtration device is SHZ-111B circulating water multi-purpose vacuum pump.

[0074] The method for preparing the conductive leather subunit sample is as follows:

[0075] The leather surface was soaked with ethanol, and the waterproof layer on the surface was removed by gently polishing with sandpaper. 20 mL of the solution was taken with a pipette for filtration. The leather was cut into 5*5 cm in size and sandwiched in the middle of the filtration bottle. After filtration, it was dried at room temperature to obtain conductive leather. Then, copper foil was attached to the surface with silver paste as an electrode. Then, the same mass of shear thickening glue was applied on the fiber side, and a non-woven fabric layer was attached to obtain a subunit sample of a sandwich structure.

[0076] Wherein: the leather is ordinary commercial natural cowhide; the model of the filtration device is SHZ-111B circulating water multi-purpose vacuum pump.

[0077] The resistance of the conductive leathers prepared in 2-6 was tested respectively, and the test methods were in accordance with the specific method of measuring the electrical properties of the conductive leather in A of the aforementioned test method. The test results are as follows:

[0078] Volume of MXene solution filtered (mL) 1 5 10 15 20 Resistance(Ω) 953 27.7 11.5 7.60 3.05

[0079] like Fig.19 , 20 As shown, the method for preparing the electric heating bulletproof vest is as follows:

[0080] a. Silicone oil and boric acid were mixed evenly in a ratio of 20:1, and then placed in an oven for heating at 180°C, 0.25wt% of n-octanoic acid was added in the middle, and shear thickening glue was obtained after cross-linking for 2h.

[0081] b. The MXene raw material is etched by HF to obtain a multilayer MXene sheet, and then ultrasonic water washing is continued to peel the multilayer sheet into a single-layer MXene sheet to obtain a MXene aqueous solution, and the concentration is adjusted to 4.84 mg / mL.

[0082] c. Cut the leather into the shape of a vest as the substrate 1, and then further treat it with ethanol to remove the waterproof layer on the surface of the vest.

[0083] d. The array area is pre-divided on the front and back of the vest, and 10 mL of MXene solution is taken with a pipette for filtration. After completion, it is dried at room temperature to obtain a single MXene array subunit 2.

[0084] e. Use silver paste to attach copper foil as electrode 3 on each sub-unit in the array to form a conductive path.

[0085] f. The shear thickening glue is evenly applied to the inside of the vest at a mass ratio of 1:1, and then the non-woven fabric is cut into a specified shape and attached to the shear thickening glue to form a sandwich structure to obtain the electrically heated soft bulletproof vest.

[0086] Figure 1 The volt-ampere curves of conductive leather with different MXene volumes filtered out; after filtering the MXene conductive material, the volt-ampere characteristic curve of the leather illustrates that the filtration method of the present invention brings excellent conductivity to the leather.

[0087] Figure 2 The resistance of conductive leather with different MXene contents is shown in Figure 2, which shows that the resistance of conductive leather gradually decreases with the increase of MXene content.

[0088] Figure 3 The temperature change of conductive leather with different MXene contents at a voltage of 3.0 V; with the increase of MXene content, the temperature coverage range of the conductive leather at a voltage of 3.0 V is about 30°C to 140°C, which illustrates that the conductive leather in the present invention has excellent electrothermal performance.

[0089] Figure 4 The temperature change of the conductive leather for filtering 10mL MXene at different voltages; the temperature of the conductive leather increases from 37°C to about 100°C when the power is applied from 1.0V to 3.0V, indicating that the conductive leather prepared in the present invention has a wide temperature coverage range.

[0090] Figure 5 It is the temperature change of the conductive leather / shear thickening glue / non-woven fabric subunit under different voltages; the temperature of the sample subunit increases from 36°C to about 87°C when the power is turned on from 1.0V to 3.0V, which shows that the addition of shear thickening glue in the present invention improves the impact resistance of the sample and has little effect on the electrothermal performance.

[0091] Figure 6 It is the power-on and power-off cycle curve of the conductive leather / shear thickening glue / non-woven fabric subunit at a voltage of 3.0V; when the sample subunit is cyclically powered on at a voltage of 3.0V, it stably reaches about 95°C, indicating that the vest in the present invention has a certain stability in use.

[0092] Figure 7 This is the temperature change curve of the conductive leather / shear thickening glue / non-woven fabric subunit under step voltage; the temperature of the sample subunit also steadily increases from 37°C to about 100°C under the loading of 1.0V to 3.0V step voltage, indicating that the vest in the present invention has a wider adjustable temperature range.

[0093] Figure 8 is the rheological property of the shear thickening glue; the relationship between the storage modulus and the loss modulus of the shear thickening glue under the shear excitation loading of 0.1-100Hz indicates that the shear thickening glue used in the present invention is successfully prepared and has an obvious rate-dependent effect.

[0094] Fig. 9 The stress-strain curves of conductive leathers with different MXene contents illustrate that the conductive leather used in the present invention has a certain mechanical strength and is suitable for use as a substrate for soft bulletproof vests.

[0095] Fig.10 This is the force signal of conductive leather with different MXene contents under drop hammer impact. Conductive leather with different MXene contents has similar force buffering effect under drop hammer impact, which indicates that the introduction of MXene in the present invention has no effect on the mechanical properties of leather.

[0096] Fig.11 Figure 3 is the force signal of samples containing different shear thickening glue (SSG) under the impact of falling hammer (sample X means that the mass of shear thickening glue is X times that of leather; under the impact of falling hammer, different contents of shear thickening glue increase the force buffering effect of the sample, indicating that the introduction of shear thickening glue in the present invention has a great improvement on the impact resistance.

[0097] Fig.12 The figure is a comparison of the changes in resistance signals of the samples under drop hammer impact at different heights (the mass of the shear thickening glue used in the samples is 1 times the mass of the leather); as the height of the drop hammer impact increases, the resistance change generated by the sample when impacted also increases, indicating that the vest in the present invention has the ability to in-situ sense and monitor impact.

[0098] Fig.13 The process is that when the vest is hit by a small hammer, the mobile phone receives the resistance signal; when the vest is hit by a small hammer, an electrical signal is transmitted through the Bluetooth device, and a corresponding resistance change signal is obtained on the mobile phone, which shows that the vest in the present invention has the ability to transmit signals wirelessly.

[0099] Fig.14 The initial velocity-residual velocity curve of the leather and the sample when impacted by a bullet; the limiting breakdown velocity of the pure leather after fitting is about 81 m / s, and the limiting breakdown velocity of the sample is about 92 m / s, which indicates that the vest of the present invention has certain anti-ballistic performance, and is improved by the shear thickening adhesive layer.

[0100] Fig.16 This is a diagram showing the position of the MXene array on the inside of the vest; it illustrates that the vest in the present invention increases the temperature coverage range of electric heating by designing the array.

[0101] Fig.17 This is an infrared image of the vest when it is powered on (the comfortable temperature for the human body is around 35°C); under a lower voltage, the temperature of the vest is stably maintained at around 35°C, a temperature suitable for warmth for the human body, which shows that the vest in the present invention has stable electrothermal performance and can maintain the temperature requirements of the human body.

[0102] Fig.18 This is an infrared image of the vest when it is powered on (high temperature is around 65°C); under a relatively high voltage, the temperature of the vest is stably maintained at a high temperature of around 65°C, which indicates that if the vest of the present invention is in a harsh environment and high temperature is required, it can also be stably achieved.

[0103] like Fig.15 , 19As shown, two 2*2 array areas are designed on the front chest of the vest, and a 4*4 array area is designed on the back, with a total of 24 sub-units, which can be connected in series or in parallel. After power is turned on, the heating area can cover most of the upper body of the human body, achieving the effect of electric heating to provide temperature, which shows that the vest in the present invention has achieved the effect of wearable heating clothing.

[0104] like Fig. 20 As shown, the MXene raw material is first etched, centrifuged and washed to obtain an aqueous solution of the MXene conductive sheet layer, and then filtered on a vest by suction filtration. Fig.15 The conductive array is connected to the circuit and then coated with a shear thickening adhesive layer and a non-woven fabric layer to obtain the final electric heating soft bulletproof vest. It is explained that the vest of the present invention achieves a multifunctional effect through the synergy between the layers.

[0105] Finally, it should be noted that: Obviously, the above embodiments are only examples for clearly explaining the present invention, and are not intended to limit the implementation methods. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from this are still within the scope of protection of the present invention.

Claims

1. An electric heating soft bulletproof vest, characterized by: The vest integrates protection, in-situ sensing and electric heating performance. The vest is a sandwich structure, including a conductive leather layer, a shear thickening adhesive layer and a non-woven fabric layer. The layers are tightly combined by the viscosity of the shear thickening adhesive. The conductive leather layer is the sensing layer and the electric heating layer, and the shear thickening adhesive layer is the main protective layer. The conductive leather layer is cowhide, which is cut into a vest style and treated with ethanol to remove the waterproof layer on the surface of the vest; then the treated vest is filtered, and the filtration method is as follows: the MXene conductive material is filtered through the treated vest with the conductive leather layer to form an array, and the filtered MXene conductive material sheets are completely dispersed in the multi-level structure network of the vest to form a conductive network.

2. The electrically heated soft bulletproof vest according to claim 1, characterized in that: The volume of the suction filtration is 1 to 20 mL.

3. The electrically heated soft bulletproof vest according to claim 1, characterized in that: The shear thickening adhesive layer is formed by cross-linking silicone oil and boric acid, and is completely attached to the inner side of the conductive leather layer; the mass ratio of the silicone oil to boric acid is 20:1 to 30:1; the shear thickening adhesive is formed at a temperature of 160°C to 200°C.

4. The electrically heated soft bulletproof vest according to claim 1, characterized in that: The changes in electrical signals generated by the impact of the vest are wirelessly transmitted through wireless devices to monitor the safety of the human body in situ.

5. The electrically heated soft bulletproof vest according to claim 4, characterized in that: Connected to the conductive leather layer via a Bluetooth sensor module.

6. A method for preparing the electrically heated soft bulletproof vest according to any one of claims 1 to 4, comprising the following steps: a. The silicone oil and boric acid are mixed evenly in a ratio of 20:1 to 30:1, and then placed in an oven for heat treatment at 160°C to 200°C, and n-octanoic acid is added in the middle to obtain a shear thickening glue after cross-linking; b. Preparation of MXene aqueous solution by HF etching; c. Cut the leather into the shape of a vest and then further treat it with ethanol to remove the waterproof layer on the surface of the vest; d. The array area is pre-divided on the front and back of the vest to filter the MXene aqueous solution; 1-20 mL of MXene aqueous solution is filtered from each subunit in the array and dried at room temperature; e. Use silver paste and copper foil to build electrodes on the surface of each subunit to complete the conductive path; f. Apply the shear thickening glue evenly on the inside of the vest at a mass ratio of 1:1 to 1:5, then cut the non-woven fabric into a specified shape and attach it to the shear thickening glue to form a sandwich structure to obtain an electric heating soft bulletproof vest.

Citation Information

Cited By

  • Sensible stab-resistant bulletproof fabric and preparation method thereof

    CN117885401A